Negative electrode interface protection layer of solid-state lithium metal battery, preparation method of negative electrode interface protection layer and solid-state lithium metal battery

By using the interface protective layer prepared by lithium conduction material and polytetrafluoroethylene in lithium metal batteries, the interface problem between the lithium metal negative electrode and the sulfide solid electrolyte is solved, and the excellent cycle of lithium metal batteries under high current density is achieved. Performance and stability significantly improve the cycle stability and electrochemical performance of the battery.

CN118983443AActive Publication Date: 2024-11-19SHANDONG UNIV

Patent Information

Application Number
CN202411041786.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The interface side reaction between the lithium metal negative electrode and the sulfide solid electrolyte, the high interface impedance and the growth of lithium dendrites seriously affect the cycle life and electrochemical performance of sulfide-based solid lithium metal batteries, especially under high current density. good.

Method used

A mixed interface protective layer of lithium conductive materials (such as red phosphorus or black phosphorus) and polytetrafluoroethylene is prepared by ball milling and roll pressing to form an interface protective layer with ionic/electronic hybrid conductivity characteristics to isolate lithium metal from solid state of sulfide Side reaction of electrolytes promotes uniform deposition of lithium metal.

Benefits of technology

It significantly improves the circulation performance of solid-state lithium metal batteries, with a discharge capacity retention rate of more than 80% in 1000 weeks, which is much higher than that of batteries without interface protection (less than 30%), and remains stable under high current density, extending the use of batteries life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983443A_ABST
    Figure CN118983443A_ABST
Patent Text Reader

Abstract

The invention discloses a solid-state lithium metal battery negative electrode interface protection layer, a preparation method thereof and a solid-state lithium metal battery, and belongs to the technical field of solid-state lithium metal batteries. The negative electrode interface protection layer of the solid-state lithium metal battery is obtained by mixing and rolling a lithium conducting material and polytetrafluoroethylene; the lithium conducting material is red phosphorus or black phosphorus, and the mass ratio of the lithium conducting material to the polytetrafluoroethylene is (80-98): (2-20). The solid-state lithium metal battery obtained by assembling the solid-state lithium metal battery negative electrode interface protection layer provided by the invention has excellent cycle stability, the discharge capacity retention rate of 1000 weeks can still be higher than 80% and is far higher than that of a solid-state lithium metal battery without an interface protection layer, and the preparation method is simple and easy to implement, high in operability, low in cost and suitable for industrial production. And the method can be integrated on the existing solid-state lithium metal battery manufacturing process to realize large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid-state lithium metal batteries, and in particular to a solid-state lithium metal battery negative electrode interface protection layer and a preparation method thereof, and a solid-state lithium metal battery. Background Art

[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] With the rapid development of electric vehicles and large-scale energy storage technology, lithium-ion batteries based on graphite anodes and liquid organic electrolytes are difficult to meet the requirements of high energy density and safety at the same time. Lithium metal batteries based on sulfide solid electrolytes use inorganic solid electrolytes with high mechanical strength and thermal stability to replace flammable and volatile organic electrolytes, and use lithium metal with high specific capacity as the anode material, thereby greatly improving the safety and energy density of the battery. However, the interfacial side reactions between the lithium metal anode and the sulfide solid electrolyte, high interfacial impedance and the growth of lithium dendrites seriously affect the cycle life and electrochemical performance of sulfide-based solid-state lithium metal batteries.

[0004] At present, there are two main methods to improve the interface problem between lithium metal anode and sulfide solid electrolyte: one is to dope or coat the solid electrolyte, and the other is to modify the surface of lithium metal anode and construct an interface buffer layer to improve the interface compatibility between lithium metal anode and solid electrolyte. Although the above strategies can alleviate the interface problem to a certain extent and promote the uniform deposition of lithium metal at the interface, under high current density, due to the insufficient transfer rate of lithium atoms in lithium metal, interfacial voids are formed during the discharge process, destroying the trend of uniform deposition of lithium metal without dendrites, causing lithium metal to begin to grow in a dendritic manner, and eventually pierce the solid electrolyte, resulting in a short circuit in the battery and little improvement in cycle performance.

[0005] Therefore, how to construct an interface protection layer so that the assembled solid-state lithium metal battery still has good cycle performance at high current density is an urgent problem to be solved. Summary of the invention

[0006] In view of this, the present invention provides a solid-state lithium metal battery negative electrode interface protection layer and a preparation method thereof, and a solid-state lithium metal battery. The interface protection layer provided by the present invention has the characteristics of ion / electron mixed conductivity, inducing lithium metal to be uniformly deposited inside the interface layer, isolating the side reactions between lithium metal and sulfide solid electrolyte, thereby significantly improving the cycle performance of the all-solid-state battery.

[0007] In a first aspect, the present invention provides a solid-state lithium metal battery negative electrode interface protection layer, which is obtained by mixing and rolling a lithium conductive material and polytetrafluoroethylene; the lithium conductive material is red phosphorus or black phosphorus, and the mass ratio of the lithium conductive material to polytetrafluoroethylene is (80-98):(2-20).

[0008] Preferably, the mass ratio of the lithium conductive material to polytetrafluoroethylene is (85-95):(5-15).

[0009] Preferably, the molecular weight of the polytetrafluoroethylene is greater than 1,000,000 g / mol.

[0010] In a second aspect, the present invention provides a method for preparing the above-mentioned solid-state lithium metal battery negative electrode interface protection layer, comprising the following steps:

[0011] The lithium conductive material is ball-milled in an inert atmosphere, and the ball-milled lithium conductive material is ground and mixed with polytetrafluoroethylene, pressed into a film, and then rolled to a specified thickness to obtain the film.

[0012] Preferably, the grinding, mixing and pressing film-forming steps are performed under an inert atmosphere.

[0013] Furthermore, the inert atmosphere in the ball milling step and the grinding, mixing and pressing film forming step is selected from one or both of argon and nitrogen.

[0014] Preferably, the ball milling speed in the ball milling step is 200-400 rpm, the ball milling time is 8-15 hours, and the ball-to-material ratio is (20-40):1.

[0015] Preferably, the thickness is rolled to 30-100 μm.

[0016] In a third aspect, the present invention provides a solid-state lithium metal battery, comprising a positive electrode, a sulfide solid electrolyte layer, an interface protection layer and a metal lithium negative electrode;

[0017] The sulfide solid electrolyte layer is arranged between the positive electrode and the metal lithium negative electrode, the interface protection layer is arranged between the sulfide solid electrolyte layer and the metal lithium negative electrode, and the interface protection layer is the above-mentioned solid-state lithium metal battery negative electrode interface protection layer.

[0018] In a fourth aspect, the present invention provides a method for preparing the above-mentioned solid-state lithium metal battery, comprising the following steps:

[0019] S1. Pressing a sulfide solid electrolyte material to obtain a sulfide solid electrolyte layer;

[0020] S2. Placing an interface protection layer and a positive electrode material on both sides of the sulfide solid electrolyte layer, respectively, and pressing to obtain a three-layer structure of an interface protection layer-sulfide solid electrolyte layer-positive electrode;

[0021] S3. Place a lithium sheet on one side of the interface protective layer and press it.

[0022] Preferably, the pressing pressure of step S1 is 50-150 MPa, the pressing pressure of step S2 is 300-400 MPa, and the pressing pressure of step S3 is 150-250 MPa.

[0023] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0024] (1) The lithium-conducting material in the negative electrode interface protection layer of the solid-state lithium metal battery provided by the present invention can form Li3P that conducts lithium ions quickly after lithiation, thereby accelerating the lithium ion transmission rate and uniformizing the lithium ion concentration. On the one hand, polytetrafluoroethylene acts as a binder to form a film of the lithium-conducting material, and on the other hand, it is reduced to form carbon and LiF when in contact with lithium metal. The carbon increases the electronic conductivity of the interface protection layer and uniformizes the electric field distribution. LiF has high interface energy and can inhibit the growth of lithium dendrites. As a result, the solid-state lithium metal battery assembled by the assembly has excellent cycle stability, and the discharge capacity retention rate after 1000 cycles can still be higher than 80%, which is much higher than that of a solid-state lithium metal battery without an interface protection layer (less than 30%).

[0025] (2) The preparation method of the negative electrode interface protection layer of the solid-state lithium metal battery of the present invention is simple and easy, has strong operability and low cost, and can be integrated into the existing solid-state lithium metal battery manufacturing process to achieve large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0027] Figure 1 The XRD patterns of the initial red phosphorus, the ball-milled red phosphorus, and the lithiated red phosphorus in Example 1 of the present invention are shown;

[0028] Figure 2 The critical current density curve of the solid-state lithium metal battery with an interface protection layer prepared in Example 1 of the present invention;

[0029] Figure 3 The critical current density curve of the solid-state lithium metal battery without an interface protective layer prepared in Comparative Example 1 of the present invention;

[0030] Figure 4 This is a rate diagram of a solid-state lithium metal battery with an interface protection layer prepared in Example 1 of the present invention;

[0031] Figure 5 This is a cycle diagram of a solid-state lithium metal battery with an interface protection layer prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0033] The invention provides a solid-state lithium metal battery negative electrode interface protection layer, which is obtained by mixing and rolling a lithium conductive material and polytetrafluoroethylene; the lithium conductive material is red phosphorus or black phosphorus, and the mass ratio of the lithium conductive material to polytetrafluoroethylene is (80-98):(2-20).

[0034] In the negative electrode interface protection layer of the solid-state lithium metal battery of the present invention, the lithium-conducting material can form Li3P which conducts lithium ions quickly after being lithiated, thereby accelerating the lithium ion transmission rate and homogenizing the lithium ion concentration; polytetrafluoroethylene, on the one hand, acts as a binder to form a film of the lithium-conducting material, and on the other hand, is reduced to form carbon and LiF when in contact with lithium metal, wherein carbon increases the electronic conductivity of the interface protection layer and homogenizes the electric field distribution, and LiF has high interface energy and can inhibit the growth of lithium dendrites; polyvinylidene fluoride (PVDF), which is a common binder in batteries, is difficult to form a film using the method of the present invention; although the non-fluorine binder polyacrylonitrile (PAN) can react with lithium metal to form Li3N and accelerate the lithium ion conduction at the interface, lithium dendrites will still be formed under high current density due to the limitation of the lithium atom transmission rate in lithium metal, and its cycle performance is poor.

[0035] The solid-state lithium metal battery negative electrode interface protection layer of the present invention has the characteristics of ion / electron mixed conductivity, inducing lithium metal to deposit uniformly inside the interface layer, isolating the side reaction between lithium metal and sulfide solid electrolyte, and improving the cycle performance of the all-solid-state battery.

[0036] The mass ratio of lithium conductive material and polytetrafluoroethylene will affect the final cycle performance of solid-state lithium metal battery. If the polytetrafluoroethylene content in the interface protection layer is too low, it is difficult to form a stable conductive network, which will have an adverse effect on the cycle performance of the battery; if the polytetrafluoroethylene content in the interface protection layer is too high, lithium metal will be deposited at the interface between the interface protection layer and the solid electrolyte, and the interface protection layer will not be able to inhibit lithium dendrites.

[0037] In the present invention, the mass ratio of the lithium conductive material to polytetrafluoroethylene is preferably (85-95):(5-15). Under the above mass ratio, the solid-state lithium metal battery exhibits a higher critical current density and discharge capacity retention rate.

[0038] In the present invention, the molecular weight of the polytetrafluoroethylene is 1000000 g mol -1 If the molecular weight of polytetrafluoroethylene is too low, its film-forming property will be reduced, and it will be difficult to roll to a lower thickness.

[0039] The present invention also provides a method for preparing the above-mentioned solid-state lithium metal battery negative electrode interface protection layer, comprising the following steps:

[0040] The lithium conductive material is ball-milled in an inert atmosphere, and the ball-milled lithium conductive material is ground and mixed with polytetrafluoroethylene, pressed into a film, and then rolled to a specified thickness to obtain the film.

[0041] In the present invention, the grinding, mixing and pressing film-forming steps are performed under an inert atmosphere. The inert atmosphere in the ball milling step and the grinding, mixing and pressing film-forming step is selected from one or both of argon and nitrogen, preferably argon. The inert atmosphere can prevent the lithium conductive material and oxygen from reacting to generate impurities during the ball milling process and the grinding, mixing and pressing film-forming process.

[0042] In the present invention, the ball milling speed of the ball milling step is 200-400 rpm, the ball milling time is 8-15 hours, and the ball milling material ratio is (20-40): 1. The present invention does not impose any special restrictions on the ball milling material used in the ball milling process, and the ball milling material commonly used in the art can be used.

[0043] In the present invention, the thickness is rolled to 30-100 μm. Within the above range, the interface lithium ion transmission can be ensured to be favorable, and the interface protection layer can also have a certain mechanical strength.

[0044] The present invention provides a solid-state lithium metal battery, comprising a positive electrode, a sulfide solid electrolyte layer, an interface protection layer and a metal lithium negative electrode;

[0045] The sulfide solid electrolyte layer is arranged between the positive electrode and the metal lithium negative electrode, the interface protection layer is arranged between the sulfide solid electrolyte layer and the metal lithium negative electrode, and the interface protection layer is the above-mentioned solid-state lithium metal battery negative electrode interface protection layer.

[0046] The solid-state lithium metal battery negative electrode interface protection layer of the present invention has the characteristics of ion / electron mixed conductivity, which induces the uniform deposition of metallic lithium inside the interface protection layer, isolates the side reaction between metallic lithium and the sulfide solid electrolyte, thereby improving the cycle performance of the solid-state lithium metal battery. The discharge capacity retention rate after 1000 cycles can still be higher than 80%, which is much higher than that of the solid-state lithium metal battery without an interface protection layer (less than 30%).

[0047] The present invention does not impose any special restrictions on the positive electrode, and the positive electrode of the solid-state lithium metal battery commonly used in the art can be used. The active material in the positive electrode can be selected from one or more of lithium cobalt oxide, lithium manganese oxide, ternary nickel cobalt manganese oxide, lithium iron phosphate and lithium nickel manganese oxide. The present invention does not impose any special restrictions on the material of the sulfide solid electrolyte layer, and the sulfide solid electrolyte material commonly used in the art can be used, such as lithium sulfur phosphorus chloride fast ion conductor (Li6PS5Cl), lithium germanium phosphorus sulfur fast ion conductor (Li 10 GeP2S 12 ), lithium sulfur phosphorus fast ion conductor (Li7P3S 11 )wait.

[0048] The present invention also provides a method for preparing the above-mentioned solid-state lithium metal battery, comprising the following steps:

[0049] S1. Pressing a sulfide solid electrolyte material to obtain a sulfide solid electrolyte layer;

[0050] S2. Placing an interface protection layer and a positive electrode material on both sides of the sulfide solid electrolyte layer, respectively, and pressing to obtain a three-layer structure of an interface protection layer-sulfide solid electrolyte layer-positive electrode;

[0051] S3. Place a lithium sheet on one side of the interface protective layer and press it.

[0052] In the present invention, the pressing pressure of step S1 is 50-150 MPa, the pressing pressure of step S2 is 300-400 MPa, and the pressing pressure of step S3 is 150-250 MPa.

[0053] The method for preparing the negative electrode interface protection layer of the solid-state lithium metal battery and the method for assembling the solid-state lithium metal battery using the same are both simple and easy to implement, low in cost, and easy to mass produce.

[0054] The technical solution of the present invention is further described below in conjunction with specific embodiments. In the following embodiments, PTFE represents polytetrafluoroethylene.

[0055] Example 1

[0056] This embodiment provides a method for preparing a negative electrode interface protection layer of a solid-state lithium metal battery and a method for assembling a solid-state lithium metal battery using the same.

[0057] Step 1: Under an argon atmosphere, 2.0 g of red phosphorus material was ball-milled using a zirconia ball with a diameter of 10 mm. The ball-milling speed was set to 300 rpm, the ball-milling time was 10 hours, and the ball-to-material ratio was 30:1.

[0058] Step 2: Under an argon atmosphere, 950 mg of red phosphorus and 50 mg of PTFE (the mass ratio of red phosphorus to PTFE is 95:5) are continuously ground, mixed and pressed in a mortar to completely bond the two materials into a film, and then rolled to a thickness of 30 μm in a roller press to obtain a solid-state lithium metal battery negative electrode interface protection layer; finally, it is cut into discs with a diameter of 10 mm, recorded as Li-95% RP.

[0059] Step 3: Weigh the positive electrode active material LiCoO2 and the sulfide solid electrolyte Li6PS5Cl in a mass ratio of 70:30, and then grind them thoroughly in a mortar to obtain a composite positive electrode material (adding a solid electrolyte to conduct lithium ions); add 100 mg of Li6PS5Cl sulfide solid electrolyte material to an insulating outer cylinder with a diameter of 10 mm, and press it under a pressure of 100 MPa to obtain a sulfide solid electrolyte layer; then add 10 mg of the composite positive electrode material to one side, and add the Li-95% RP interface protection layer obtained in step 2 to the other side, and then pressurize it at a pressure of 360 MPa to form a three-layer structure of interface protection layer-sulfide solid electrolyte layer-positive electrode; finally, place a lithium sheet with a diameter and thickness of 10 mm and 100 μm respectively on the other side of the interface protection layer, and pressurize it at a pressure of 200 MPa to obtain a solid-state lithium metal battery.

[0060] Example 2

[0061] This embodiment provides a method for preparing a negative electrode interface protection layer of a solid-state lithium metal battery and a method for assembling a solid-state lithium metal battery using the same.

[0062] Step 1: Under an argon atmosphere, 2.0 g of red phosphorus material was ball-milled using a zirconia ball with a diameter of 10 mm. The ball-milling speed was set to 300 rpm, the ball-milling time was 10 hours, and the ball-to-material ratio was 30:1.

[0063] Step 2: Under an argon atmosphere, 900 mg of red phosphorus and 100 mg of PTFE (the mass ratio of red phosphorus to PTFE is 90:10) are continuously ground, mixed and pressed in a mortar to completely bond the two materials into a film, and then rolled to a thickness of 30 μm in a roller press to obtain a solid-state lithium metal battery negative electrode interface protection layer; finally, it is cut into discs with a diameter of 10 mm, recorded as Li-90% RP.

[0064] Step 3: Weigh the positive electrode active material LiCoO2 and the sulfide solid electrolyte Li6PS5Cl in a mass ratio of 70:30, and then grind them thoroughly in a mortar to obtain a composite positive electrode material; add 100 mg of Li6PS5Cl sulfide solid electrolyte material to an insulating outer cylinder with a diameter of 10 mm, and press it under a pressure of 100 MPa to obtain a sulfide solid electrolyte layer; then add 10 mg of the composite positive electrode material to one side, and add the Li-90% RP interface protection layer obtained in step 2 to the other side, and then pressurize it at a pressure of 360 MPa to form a three-layer structure of interface protection layer-sulfide solid electrolyte layer-positive electrode; finally, place a lithium sheet with a diameter and thickness of 10 mm and 100 μm respectively on the other side of the interface protection layer, and pressurize it at a pressure of 200 MPa to obtain a solid-state lithium metal battery.

[0065] Example 3

[0066] This embodiment provides a method for preparing a negative electrode interface protection layer of a solid-state lithium metal battery and a method for assembling a solid-state lithium metal battery using the same.

[0067] Step 1: Under an argon atmosphere, 2.0 g of red phosphorus material was ball-milled using a zirconia ball with a diameter of 10 mm. The ball-milling speed was set to 300 rpm, the ball-milling time was 10 hours, and the ball-to-material ratio was 30:1.

[0068] Step 2: Under an argon atmosphere, 850 mg of red phosphorus and 150 mg of PTFE (the mass ratio of red phosphorus to PTFE is 95:5) are continuously ground, mixed and pressed in a mortar to completely bond the two materials into a film, and then rolled to a thickness of 30 μm in a roller press to obtain a solid-state lithium metal battery negative electrode interface protection layer; finally, it is cut into discs with a diameter of 10 mm, recorded as Li-85% RP.

[0069] Step 3: Weigh the positive electrode active material LiCoO2 and the sulfide solid electrolyte Li6PS5Cl in a mass ratio of 70:30, and then grind them thoroughly in a mortar to obtain a composite positive electrode material; add 100 mg Li6PS5Cl sulfide solid electrolyte material to an insulating outer cylinder with a diameter of 10 mm, and press it under a pressure of 100 MPa to obtain a sulfide solid electrolyte layer; then add 10 mg of the composite positive electrode material to one side, and add the Li-85% RP interface protection layer obtained in step 2 to the other side, and then pressurize it at a pressure of 360 MPa to form a three-layer structure of interface protection layer-sulfide solid electrolyte layer-positive electrode; finally, place a lithium sheet with a diameter and thickness of 10 mm and 100 μm respectively on the other side of the interface protection layer, and pressurize it at a pressure of 200 MPa to obtain a solid-state lithium metal battery.

[0070] Example 4

[0071] This embodiment provides a method for preparing a negative electrode interface protection layer of a solid-state lithium metal battery and a method for assembling a solid-state lithium metal battery using the same.

[0072] Step 1: Under an argon atmosphere, 2.0 g of black phosphorus material was ball-milled using a zirconia ball with a diameter of 10 mm. The ball-milling speed was set to 300 rpm, the ball-milling time was 10 hours, and the ball-to-material ratio was 30:1.

[0073] Step 2: Under an argon atmosphere, 950 mg of black phosphorus and 50 mg of PTFE (the mass ratio of black phosphorus to PTFE is 95:5) are continuously ground, mixed and pressed in a mortar to completely bond the two materials into a film, and then rolled to a thickness of 30 μm in a roller press to obtain a solid-state lithium metal battery negative electrode interface protection layer; finally, it is cut into discs with a diameter of 10 mm, recorded as Li-95% BP.

[0074] Step 3: Weigh the positive electrode active material LiCoO2 and the sulfide solid electrolyte Li6PS5Cl in a mass ratio of 70:30, and then grind them thoroughly in a mortar to obtain a composite positive electrode material; add 100 mg of Li6PS5Cl sulfide solid electrolyte material to an insulating outer cylinder with a diameter of 10 mm, and press it under a pressure of 100 MPa to obtain a sulfide solid electrolyte layer; then add 10 mg of the composite positive electrode material to one side, and add the Li-95% BP interface protection layer obtained in step 2 to the other side, and then pressurize it at a pressure of 360 MPa to form a three-layer structure of interface protection layer-sulfide solid electrolyte layer-positive electrode; finally, place a lithium sheet with a diameter and thickness of 10 mm and 100 μm respectively on the other side of the interface protection layer, and pressurize it at a pressure of 200 MPa to obtain a solid-state lithium metal battery.

[0075] Example 5

[0076] This embodiment provides a method for preparing a negative electrode interface protection layer of a solid-state lithium metal battery and a method for assembling a solid-state lithium metal battery using the same.

[0077] Step 1: Under an argon atmosphere, 2.0 g of black phosphorus material was ball-milled using a zirconia ball with a diameter of 10 mm. The ball-milling speed was set to 300 rpm, the ball-milling time was 10 hours, and the ball-to-material ratio was 30:1.

[0078] Step 2: Under an argon atmosphere, 900 mg of black phosphorus and 100 mg of PTFE (the mass ratio of black phosphorus to PTFE is 90:10) are continuously ground, mixed and pressed in a mortar to completely bond the two materials into a film, and then rolled to a thickness of 30 μm in a roller press to obtain a solid-state lithium metal battery negative electrode interface protection layer; finally, it is cut into discs with a diameter of 10 mm, recorded as Li-90% BP.

[0079] Step 3: Weigh the positive electrode active material LiCoO2 and the sulfide solid electrolyte Li6PS5Cl in a mass ratio of 70:30, and then grind them thoroughly in a mortar to obtain a composite positive electrode material; add 100 mg of Li6PS5Cl sulfide solid electrolyte material to an insulating outer cylinder with a diameter of 10 mm, and press it under a pressure of 100 MPa to obtain a sulfide solid electrolyte layer; then add 10 mg of the composite positive electrode material to one side, and add the Li-90% BP interface protection layer obtained in step 2 to the other side, and then pressurize at a pressure of 360 MPa to form a three-layer structure of interface protection layer-sulfide solid electrolyte layer-positive electrode; finally, place a lithium sheet with a diameter and thickness of 10 mm and 100 μm respectively on the other side of the interface protection layer, and pressurize it at a pressure of 200 MPa to obtain a solid-state lithium metal battery.

[0080] Example 6

[0081] This embodiment provides a method for preparing a negative electrode interface protection layer of a solid-state lithium metal battery and a method for assembling a solid-state lithium metal battery using the same.

[0082] Step 1: Under an argon atmosphere, 2.0 g of black phosphorus material was ball-milled using a zirconia ball with a diameter of 10 mm. The ball-milling speed was set to 300 rpm, the ball-milling time was 10 hours, and the ball-to-material ratio was 30:1.

[0083] Step 2: Under an argon atmosphere, 850 mg of black phosphorus and 150 mg of PTFE (the mass ratio of black phosphorus to PTFE is 95:5) are continuously ground, mixed and pressed in a mortar to completely bond the two materials into a film, and then rolled to a thickness of 30 μm in a roller press to obtain a solid-state lithium metal battery negative electrode interface protection layer; finally, it is cut into discs with a diameter of 10 mm, recorded as Li-85% BP.

[0084] Step 3: Weigh the positive electrode active material LiCoO2 and the sulfide solid electrolyte Li6PS5Cl in a mass ratio of 70:30, and then grind them thoroughly in a mortar to obtain a composite positive electrode material; add 100 mg of Li6PS5Cl sulfide solid electrolyte material to an insulating outer cylinder with a diameter of 10 mm, and press it under a pressure of 100 MPa to obtain a sulfide solid electrolyte layer; then add 10 mg of the composite positive electrode material to one side, and add the Li-85% BP interface protection layer obtained in step 2 to the other side, and then pressurize it at a pressure of 360 MPa to form a three-layer structure of interface protection layer-sulfide solid electrolyte layer-positive electrode; finally, place a lithium sheet with a diameter and thickness of 10 mm and 100 μm respectively on the other side of the interface protection layer, and pressurize it at a pressure of 200 MPa to obtain a solid-state lithium metal battery.

[0085] Comparative Example 1

[0086] Compared with Example 1, this comparative example does not include the preparation of the interface protection layer.

[0087] The positive electrode active material LiCoO2 and the sulfide solid electrolyte Li6PS5Cl were weighed in a mass ratio of 70:30, and then fully ground using a mortar to obtain a composite positive electrode material; 100 mg of Li6PS5Cl sulfide solid electrolyte material was added to an insulating outer cylinder with a diameter of 10 mm, and pressed at a pressure of 100 MPa to obtain a sulfide solid electrolyte layer; then 10 mg of the composite positive electrode material was added to one side, and then pressurized at a pressure of 360 MPa to form a two-layer structure of sulfide solid electrolyte layer-positive electrode; then a lithium sheet with a diameter and thickness of 10 mm and 100 μm, respectively, was placed on the other side of the sulfide solid electrolyte layer, and pressurized at a pressure of 200 MPa to obtain a solid-state lithium metal battery.

[0088] Comparative Example 2

[0089] Compared with Example 1, the difference is that this comparative example does not add polytetrafluoroethylene, and only uses red phosphorus as the interface protective layer. The specific steps are as follows:

[0090] Step 1: Under an argon atmosphere, 2.0 g of red phosphorus material was ball-milled using a zirconia ball with a diameter of 10 mm. The ball-milling speed was set to 300 rpm, the ball-milling time was 10 hours, and the ball-to-material ratio was 30:1.

[0091] Step 2: Weigh the positive electrode active materials LiCoO2 and Li6PS5Cl in a mass ratio of 70:30, and then grind them thoroughly in a mortar to obtain a composite positive electrode material; add 100 mg of sulfide solid electrolyte material to an insulating outer cylinder with a diameter of 10 mm, and press it under a pressure of 100 MPa to obtain a sulfide solid electrolyte layer; then add 10 mg of the composite positive electrode material to one side, and add 2 mg of the ball-milled red phosphorus obtained in step 1 to the other side, and then pressurize at a pressure of 360 MPa to form a three-layer structure of red phosphorus layer-sulfide solid electrolyte layer-positive electrode; finally, place a lithium sheet with a diameter and thickness of 10 mm and 100 μm respectively on the other side of the red phosphorus layer, and pressurize it at a pressure of 200 MPa to obtain a solid-state lithium metal battery.

[0092] Comparative Example 3

[0093] The difference between this comparative example and Example 1 is that polytetrafluoroethylene is replaced by polyacrylonitrile (PAN) in this comparative example.

[0094] Test example

[0095] The electrochemical performance tests were conducted on the solid-state lithium metal batteries of Examples 1 to 6 and Comparative Examples 1 to 3. The test results are shown in Table 1.

[0096] Table 1 Electrochemical properties of solid-state lithium metal batteries of Examples 1 to 6 and Comparative Examples 1 to 3

[0097]

[0098]

[0099] Note: The first week discharge capacity in Table 1 was tested at 1C rate, and the 1000-week discharge capacity retention rate was measured at 20C rate, 1C = 140 mAh / g.

[0100] The experimental results show that the solid-state lithium metal battery using the interface protection layer prepared by Examples 1 to 6 of the present invention has a higher critical current density and cycle stability. Compared with Comparative Example 2, the interface protection layer prepared by the present invention has the characteristics of mixed ion-electron conductivity after contacting lithium metal, can induce lithium metal to deposit in the protection layer, and has better electrochemical performance. Compared with Comparative Example 3, although PAN can react with lithium metal to form Li3N and accelerate interfacial lithium ion conduction, at high current density, lithium dendrites will still be formed due to the limitation of lithium atom transfer rate in lithium metal.

[0101] Figure 1The XRD patterns of the red phosphorus in the initial state, the red phosphorus after ball milling, and the red phosphorus after lithiation in Example 1. The red phosphorus after lithiation refers to the interface protection layer taken out after the battery is assembled and left to stand for 12 hours, without charge and discharge test. It can be seen from the figure that the red phosphorus film can be lithiated to form Li3P with fast lithium conduction properties after contacting lithium metal, without additional processing steps, and the operation is simple.

[0102] Figure 2 This is the critical current density curve of the solid-state lithium metal battery with an interface protection layer prepared in Example 1 of the present invention, Figure 3 The critical current density curve of the solid-state lithium metal battery without an interface protective layer prepared in Comparative Example 1 of the present invention shows that the use of the interface protective layer of Example 1 can better inhibit the formation of lithium dendrites and improve the interface stability between lithium metal and the solid electrolyte.

[0103] Figure 4 This is a rate diagram of a solid-state lithium metal battery with an interface protection layer prepared in Example 1 of the present invention. Since the interface protection layer after lithiation has good ion and electron conductivity, the solid-state lithium metal battery using the interface protection layer exhibits excellent rate performance and can still provide 10.2 mAh g even at a rate of 50C. -1 Specific capacity. Figure 5 This is a cycle diagram of the solid-state lithium metal battery with an interface protection layer prepared in Example 1 of the present invention. It can be stably cycled for 1000 times at a rate of 20C without the occurrence of short circuit.

[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A solid-state lithium metal battery negative electrode interface protection layer, characterized in that: The lithium conductive material is obtained by mixing and rolling a lithium conductive material and polytetrafluoroethylene; the lithium conductive material is red phosphorus or black phosphorus, and the mass ratio of the lithium conductive material to polytetrafluoroethylene is (80-98):(2-20).

2. The solid-state lithium metal battery negative electrode interface protection layer according to claim 1, characterized in that: The mass ratio of the lithium conductive material to polytetrafluoroethylene is (85-95):(5-15).

3. The solid-state lithium metal battery negative electrode interface protection layer according to claim 1, characterized in that: The molecular weight of the polytetrafluoroethylene is greater than 1,000,000.

4. The method for preparing the negative electrode interface protection layer of a solid-state lithium metal battery according to any one of claims 1 to 3, characterized in that: The steps include: The lithium conductive material is ball-milled in an inert atmosphere, and the ball-milled lithium conductive material is ground and mixed with polytetrafluoroethylene, pressed into a film, and then rolled to a specified thickness to obtain the film.

5. The preparation method according to claim 4, characterized in that: The grinding, mixing and pressing film-forming steps are performed under an inert atmosphere.

6. The preparation method according to claim 5, characterized in that: The inert atmosphere in the ball milling step and the grinding, mixing and pressing film forming step is selected from one or both of argon and nitrogen.

7. The preparation method according to claim 4, characterized in that: The ball milling speed of the ball milling step is 200-400 rpm, the ball milling time is 8-15 hours, and the ball-to-material ratio is (20-40):

1.

8. The preparation method according to claim 4, characterized in that: Roll to a thickness of 30 to 100 μm.

9. A solid-state lithium metal battery, characterized in that: It includes a positive electrode, a sulfide solid electrolyte layer, an interface protection layer and a metal lithium negative electrode; The sulfide solid electrolyte layer is arranged between the positive electrode and the metal lithium negative electrode, the interface protection layer is arranged between the sulfide solid electrolyte layer and the metal lithium negative electrode, and the interface protection layer is the solid-state lithium metal battery negative electrode interface protection layer according to any one of claims 1 to 3.

10. The method for preparing a solid-state lithium metal battery according to claim 9, characterized in that: The steps include: S1. Pressing a sulfide solid electrolyte material to obtain a sulfide solid electrolyte layer; S2. Placing an interface protection layer and a positive electrode material on both sides of the sulfide solid electrolyte layer, respectively, and pressing to obtain a three-layer structure of an interface protection layer-sulfide solid electrolyte layer-positive electrode; S3. Place a lithium sheet on one side of the interface protective layer and press it.

Citation Information

Patent Citations

  • Protection method and product for lithium metal / sodium metal negative electrodes

    CN110224177A

  • Flexible battery negative electrode, preparation method thereof and flexible battery

    CN111276700A

  • Lithium-based electrode and secondary lithium battery

    CN113690407A

  • Bifunctional interface modification layer for solid-state lithium battery and lithium battery

    CN115064779A

  • All-solid-state battery with low interface resistance and high lithium metal stability and preparation method of all-solid-state battery

    CN115360320A

Cited By

  • Solid electrolyte layer, and solid-state battery and electronic device comprising same

    CN121123379A