Composite membrane as well as preparation method and application thereof
By using sulfonated polyimide and polybenzimidazole and Yb-doped perovskite nanoparticles in the composite membrane, the problem of insufficient proton conduction performance of perfluorosulfonic acid membrane at high temperatures is solved, and a high-temperature fuel cell is realized efficient operation and reduce material costs.
Patent Information
- Application Number
- CN202410956742.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-19
AI Technical Summary
The existing perfluorosulfonic acid films cannot show excellent proton conduction performance under high temperature environments, which limits the high-temperature application of proton exchange membrane fuel cells, and the high price of materials is not conducive to the promotion of fuel cells.
Using sulfonated polyimide and polybenzimidazole as material components of the composite film, and embedded Yb-doped perovskite nanoparticles in the membrane matrix, the preparation method of sulfonated polyimide and polybenzimidazole The composite membrane is prepared by dissolution process to improve the proton conduction performance at high temperatures.
The high proton conduction performance of the composite membrane in a high temperature environment is achieved, the doping ability of acid and the conductivity of protons are enhanced, and it is suitable for high-temperature fuel cells, and the cost is relatively low.
Smart Images

Figure CN118983480A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of fuel cell technology, and in particular to a composite membrane and a preparation method and application thereof. Background Art
[0002] The proton exchange membrane fuel cell (PEMFC) is a widely used fuel cell with promising prospects. Perfluorosulfonic acid (PFSA) is commonly used as the electrolyte membrane material in PEMFCs. Nafion, with its high proton conductivity and excellent mechanical and thermal properties, is currently one of the most widely used electrolyte membrane materials. Current PEMFCs are typically used in relatively low-temperature environments (60-80°C). Above 80°C, the proton conductivity of PFSA materials, such as Nafion, decreases significantly. In particular, above 100°C, liquid water evaporates into a gaseous state. Without liquid water wetting, the proton conductivity of the PFSA membrane drops rapidly, making it unable to perform the electrolyte function. Therefore, PEMFCs cannot be used in high-temperature environments. Furthermore, the high cost of PFSA materials hinders the widespread application of fuel cells.
[0003] High-temperature fuel cells have a number of advantages over low-temperature fuel cells, such as: (1) Higher electrical performance: The increase in temperature also increases the degree and speed of the electrochemical reaction, thereby increasing the output voltage of the electrochemical reaction; (2) Easier water management: Water flooding is one of the main reasons for the performance degradation of fuel cells at high currents. Temperatures above 100°C mean that all water is in gaseous form, and the flooding problem that plagues low-temperature fuel cells will no longer exist. (3) Fuel cell catalysts are extremely susceptible to poisoning by CO gas, causing irreversible degradation, while high-temperature fuel cells have a higher tolerance to CO poisoning.
[0004] However, existing perfluorosulfonic acid membranes cannot perform well under high-temperature operating conditions. Summary of the Invention
[0005] The present application provides a composite membrane and its preparation method and application, which can have good proton conduction performance in a high-temperature environment.
[0006] In a first aspect, the present application provides a composite membrane, comprising a membrane matrix, wherein the components of the membrane matrix include sulfonated polyimide and polybenzimidazole, wherein the mass ratio of the sulfonated polyimide to the polybenzimidazole is (5-40):100.
[0007] As an optional embodiment, the composite film further includes Yb-doped perovskite nanoparticles, and the Yb-doped perovskite nanoparticles are embedded in the film matrix.
[0008] As an optional embodiment, the mass proportion of the Yb-doped perovskite nanoparticles in the composite film does not exceed 15%.
[0009] As an optional implementation manner, the particle size of the Yb-doped perovskite nanoparticles is 40 nm to 60 nm.
[0010] As an optional embodiment, the sulfonated polyimide comprises:
[0011] Wherein, n is selected from any positive integer.
[0012] In a second aspect, the present application provides a method for preparing a composite membrane, wherein the composite membrane is the composite membrane provided in the first aspect; the method comprises:
[0013] Sulfonated polyimide and polybenzimidazole are obtained;
[0014] mixing the sulfonated polyimide and polybenzimidazole in a solvent to obtain a slurry;
[0015] The slurry is subjected to thin film preparation to obtain a composite membrane.
[0016] As an optional embodiment, the preparation method of the sulfonated polyimide includes:
[0017] iodine, thiourea and acetophenone are heated and mixed to obtain a mixture;
[0018] dissolving the mixture in a solvent, and then neutralizing and precipitating to obtain a precipitate;
[0019] Recrystallizing the precipitate to obtain a monoamine;
[0020] The monoamine and 2-formylbenzenesulfonic acid are mixed and reacted to obtain a sulfonated aromatic diamine;
[0021] reacting the sulfonated aromatic diamine and pyromellitic dianhydride to obtain polyamic acid;
[0022] The polyamic acid, pyridine and acetic anhydride are mixed and reacted to obtain sulfonated polyimide.
[0023] As an optional embodiment, the slurry further includes Yb-doped perovskite nanoparticles.
[0024] As an optional embodiment, the method for preparing the Yb-doped perovskite nanoparticles includes:
[0025] Strontium acetate, cerium n-butoxide and ytterbium acetate are mixed in a stearic acid solution to obtain a gel;
[0026] The gel is heat-treated and then sintered to obtain Yb-doped perovskite nanoparticles.
[0027] In a third aspect, the present application provides a fuel cell, comprising the composite membrane provided in the first aspect.
[0028] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0029] The composite membrane provided in the embodiments of the present application uses sulfonated polyimide and polybenzimidazole as material components. Among them, sulfonated polyimide is a sulfonated aromatic polymer. Due to its cyclic structures such as pyridine, pyrazole, triazole and imidazole, it can exhibit high conductivity at high temperatures in the absence of liquid water; and these heterocyclic polymers have basic nitrogen sites, which facilitate proton transfer at higher temperatures. In addition, the N atoms and NH groups in the membrane structure enhance the doping ability of acids and the conductivity of protons. This enables the composite membrane to have good proton conductivity in high temperature environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0032] Figure 1 A flowchart of the method provided in the embodiment of the present application. DETAILED DESCRIPTION
[0033] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0034] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0035] Under high-temperature operating conditions, existing perfluorosulfonic acid membranes cannot demonstrate excellent performance, and other materials need to be selected to prepare high-temperature fuel cell electrolyte membranes.
[0036] The present application intends to provide a novel sulfonated polyimide (SPI) synthesized using a novel thiazole heterocycle-containing diamine as a raw material, and using the sulfonated polyimide (SPI) and polybenzimidazole (PBI) as composite membrane raw materials to form a composite membrane that has good proton conductivity performance under high-temperature operating conditions.
[0037] An embodiment of the present application provides a composite membrane, which includes a membrane matrix. The components of the membrane matrix include sulfonated polyimide and polybenzimidazole, wherein the mass ratio of the sulfonated polyimide to the polybenzimidazole is (5-40):100.
[0038] Sulfonated polyimide (SPI) has excellent thermal stability, chemical stability and mechanical stability, and due to its hydrophilic structure, it can effectively transport protons and shows suitable proton conductivity, and has the potential to be an alternative material for high-temperature proton membranes.
[0039] The composite membrane utilizes sulfonated polyimide and polybenzimidazole as its material components. Sulfonated polyimide is a sulfonated aromatic polymer. Its cyclic structures, including pyridine, pyrazole, triazole, and imidazole, allow it to exhibit high conductivity at high temperatures in the absence of liquid water. Furthermore, these heterocyclic polymers possess basic nitrogen sites, which facilitate proton transfer at higher temperatures. Furthermore, the nitrogen atoms and NH groups in the membrane structure enhance acid doping and proton conductivity, enabling the composite membrane to exhibit excellent proton conductivity even in high-temperature environments.
[0040] In some embodiments, the composite film further includes Yb-doped perovskite nanoparticles, and the Yb-doped perovskite nanoparticles are embedded in the film matrix.
[0041] Yb-doped perovskite nanoparticles exhibit good proton conductivity and excellent chemical stability. Yb-doped perovskite nanoparticles reduce the ionic repulsion between positively charged and hydrogen ions, increasing proton transfer capacity. Furthermore, perovskite materials exhibit good proton conductivity over a temperature range of 200°C to 1200°C. Yb-doped perovskite nanoparticles are stable at high temperatures and can be used in high-temperature fuel cells.
[0042] By adding Yb-doped perovskite nanoparticles into the composite membrane, the proton conduction performance of the composite membrane in a high-temperature environment can be further improved.
[0043] In some embodiments, the Yb-doped perovskite nanoparticles account for no more than 15% by weight of the composite film.
[0044] Exemplarily, the mass proportion of the Yb-doped perovskite nanoparticles in the composite film can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%, etc., and it can also be any value not exceeding 15%.
[0045] In some embodiments, the Yb-doped perovskite nanoparticles have a particle size of 40 nm to 60 nm.
[0046] Illustratively, the particle size of the Yb-doped perovskite nanoparticles can be 40 nm, 42 nm, 44 nm, 46 nm, 48 nm, 50 nm, 52 nm, 54 nm, 56 nm, 58 nm or 60 nm, etc., and can also be any value within the range of 40 nm to 60 nm.
[0047] In some embodiments, the sulfonated polyimide comprises:
[0048] Wherein, n is selected from any positive integer.
[0049] Exemplarily, the preparation process of sulfonated polyimide can be:
[0050] 1) Synthesis of diamines:
[0051] ① Synthesis of Monoamine: Heat and stir iodine, thiourea, and acetophenone in a molar ratio of 1:2:1. Stir for 8-12 hours at 100-120°C. Dissolve the mixture in sufficient deionized water and, once fully dissolved, neutralize with 1 mol / L sodium hydroxide solution to produce a precipitate. Collect and dry the precipitate. Recrystallize the precipitate from 50 wt.% ethanol to produce the monoamine, 4-(2-aminothiazole)-benzene.
[0052] ② Synthesis of diamine: Mix 4-(2-aminothiazole)-benzene and 2-formylbenzenesulfonic acid in a molar mass ratio of 2:1 in a sufficient amount of hydrochloric acid solution, reflux and condense at 100°C for 8 to 12 hours, cool to room temperature, and filter to collect the product diamine, i.e., sulfonated aromatic diamine.
[0053] The reaction process is as follows:
[0054]
[0055] 2) Synthesis of sulfonated polyimide (SPI):
[0056] The obtained diamine and pyromellitic dianhydride (molar mass ratio of 1:1) are mixed with N-methylpyrrolidone, and the solution is stirred for 24 hours to prepare polyamic acid. Subsequently, pyridine and acetic anhydride (the volume ratio of pyridine to acetic anhydride is 2-2.5:1) are added and mixed, and the stirring time is 8-12 hours at 100°C. The mixture is then transferred to sufficient methanol and stirred at room temperature for 8-12 hours. Finally, the precipitate is filtered, washed with methanol and hot deionized water, and dried at 100°C to obtain sulfonated polyimide (SPI).
[0057] The reaction process is as follows:
[0058]
[0059]
[0060] Figure 1 A flow chart of the method provided in the embodiment of the present application is shown in FIG. Figure 1 As shown, an embodiment of the present application provides a method for preparing a composite membrane.
[0061] This method is used to prepare the above-mentioned composite membrane. The specific content of the composite membrane can be referred to the above-mentioned embodiment. Since this method adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here.
[0062] In an embodiment of the present application, the method includes:
[0063] S1. Obtaining sulfonated polyimide and polybenzimidazole;
[0064] In some embodiments, the method for preparing the sulfonated polyimide comprises:
[0065] S1.1. Heat and mix iodine, thiourea, and acetophenone to obtain a mixture;
[0066] Specifically, in this embodiment, iodine, thiourea, and acetophenone are heated and stirred in a molar ratio of 1:2:1 for 8 to 12 hours at a temperature of 100 to 120°C.
[0067] S1.2. dissolving the mixture in a solvent, and then neutralizing and precipitating to obtain a precipitate;
[0068] Specifically, in this embodiment, the mixture was dissolved in a sufficient amount of deionized water, and after being fully dissolved, it was neutralized with a sufficient amount of 1 mol / L sodium hydroxide solution to generate a precipitate, which was then collected and dried.
[0069] S1.3. Recrystallizing the precipitate to obtain a monoamine;
[0070] Specifically, in this example, the precipitate was recrystallized from an ethanol solution (50 wt.%) to produce a monoamine, 4-(2-aminothiazole)-benzene.
[0071] S1.4. The monoamine and 2-formylbenzenesulfonic acid are mixed and reacted to obtain a sulfonated aromatic diamine;
[0072] Specifically, in this embodiment, 4-(2-aminothiazole)-benzene and 2-formylbenzenesulfonic acid are mixed in a sufficient amount of hydrochloric acid solution at a molar mass ratio of 2:1, and refluxed at 100° C. for 8 to 12 hours, then cooled to room temperature, and the product sulfonated aromatic diamine, i.e., aromatic diamine, is collected by filtration.
[0073] S1.5. The sulfonated aromatic diamine and pyromellitic dianhydride are reacted to obtain a polyamic acid;
[0074] Specifically, in this embodiment, the obtained diamine and pyromellitic dianhydride (molar mass ratio of 1:1) were mixed with N-methylpyrrolidone, and the solution was stirred for 24 hours to prepare polyamic acid.
[0075] S1.6. The polyamic acid, pyridine and acetic anhydride are mixed and reacted to obtain a sulfonated polyimide.
[0076] Specifically, in this embodiment, pyridine and acetic anhydride (the volume ratio of pyridine to acetic anhydride is 2 to 2.5:1) are then mixed into the polyamic acid and stirred for 8 to 12 hours at 100°C. The mixture is then transferred to a sufficient amount of methanol and stirred at room temperature for 8 to 12 hours. Finally, the precipitate is filtered, washed with methanol and hot deionized water, and dried at 100°C to obtain SPI.
[0077] S2. The sulfonated polyimide and polybenzimidazole are mixed in a solvent to obtain a slurry;
[0078] In some embodiments, the slurry further includes Yb-doped perovskite nanoparticles. Furthermore, a method for preparing the Yb-doped perovskite nanoparticles includes: mixing strontium acetate, cerium n-butoxide, and ytterbium acetate in a stearic acid solution to obtain a gel; and heat-treating the gel, followed by sintering, to obtain the Yb-doped perovskite nanoparticles.
[0079] Specifically, in this embodiment, the preparation method of Yb-doped perovskite nanoparticles can be as follows: ammonium cerium nitrate is mixed into n-butanol to react to prepare cerium n-butoxide, and then strontium acetate, cerium n-butoxide, and ytterbium acetate (molar mass ratio of 10:9:1) are dissolved in sufficient deionized water to prepare three solutions, and these three solutions are added to the stearic acid solution and stirred until a uniform gel is obtained. Then, the gel is cooled to room temperature and heat-treated at 120°C for 3 hours. The obtained dried gel is treated at 1000°C for 24 hours to obtain Yb-doped perovskite nanoparticles with a particle size of .
[0080] S3. Prepare a thin film from the slurry to obtain a composite film.
[0081] Specifically, in this embodiment, the process for preparing a composite film without Yb-doped perovskite nanoparticles can be as follows: First, polybenzimidazole (PBI) powder is dissolved in N,N-dimethylacetamide under an inert atmosphere at 150°C. The prepared sulfonated polyimide (SPI) powder is mixed with the polybenzimidazole (PBI) solution (SPI:PBI mass ratio is 5% to 40%), stirred at 30°C for 8 hours, and the mixture is cast onto a glass plate using a spatula. The wet film thickness can be controlled by controlling the gap between the spatula and the coating. The composite film is then heated in a vacuum at 80°C to obtain the composite film.
[0082] Specifically, in this embodiment, the process of preparing a composite membrane containing Yb-doped perovskite nanoparticles can be as follows: first, sulfonated polyimide (SPI) is mixed with polybenzimidazole (PBI) in N,N-dimethylacetamide (SPI: PBI mass ratio is 5% to 40%), and then stirred at 30°C for 8 to 12 hours. Next, the Yb-doped perovskite nanoparticles are added to another portion of N,N-dimethylacetamide and fully dispersed. While dispersing, they are mixed with the PBI / SPI solution to obtain a uniform solution. Finally, a scraper is used to cast the mixture onto a glass plate. The wet film thickness can be controlled by controlling the gap of the scraper. It is then heated in vacuum at 80°C to obtain a doped electrolyte membrane.
[0083] The present application will be further described below in conjunction with specific examples. It should be understood that these examples are intended to illustrate the present application only and are not intended to limit the scope of the present application. The experimental methods in the following examples where specific conditions are not specified are usually measured in accordance with national standards. If there are no corresponding national standards, then the methods are carried out in accordance with general international standards, conventional conditions, or according to the conditions recommended by the manufacturer.
[0084] Example 1
[0085] A composite film, the preparation method of which is as follows:
[0086] 1. Synthesis of diamines
[0087] First, synthesize a monoamine. Iodine, thiourea, and acetophenone are heated and stirred in a molar ratio of 1:2:1. Stir for 8 to 12 hours at 100 to 120°C. The mixture is then dissolved in sufficient deionized water. Once fully dissolved, it is neutralized with a sufficient amount of 1 mol / L sodium hydroxide solution to produce a precipitate, which is collected and dried. The precipitate is recrystallized from a 50 wt.% ethanol solution to produce 4-(2-aminothiazole)-benzene.
[0088] Subsequently, a diamine was synthesized by mixing 4-(2-aminothiazole)-benzene and 2-formylbenzenesulfonic acid in a molar ratio of 2:1 in a sufficient amount of hydrochloric acid solution. After reflux condensation at 100° C. for 8 to 12 hours, the mixture was cooled to room temperature and the product diamine was collected by filtration.
[0089] 2. Synthesis of sulfonated polyimide (SPI)
[0090] The diamine obtained in step 1 and pyromellitic dianhydride (molar mass ratio of 1:1) were mixed with N-methylpyrrolidone, and the solution was stirred for 24 hours to prepare polyamic acid. Pyridine and acetic anhydride (the volume ratio of pyridine to acetic anhydride was 2.2:1) were then added and mixed, and the stirring time was 8 to 12 hours at a stirring temperature of 100°C. The mixture was then transferred to sufficient methanol and stirred at room temperature for 8 to 12 hours. Finally, the precipitate was filtered out, washed with methanol and hot deionized water, and dried at 100°C to obtain sulfonated polyimide (SPI).
[0091] 3. Preparation of composite membrane
[0092] First, polybenzimidazole (PBI) powder was dissolved in N,N-dimethylacetamide at 150°C under an inert atmosphere. The sulfonated polyimide (SPI) powder prepared in step 2 was mixed with the polybenzimidazole (PBI) solution (SPI:PBI mass ratio of 3%) and stirred at 30°C for 8 hours. The mixture was then cast onto a glass plate using a doctor blade. The wet film thickness was controlled by adjusting the doctor blade gap. The composite membrane was then heated in a vacuum at 80°C to obtain the desired film.
[0093] Example 2
[0094] A composite film, the preparation method of which is as follows:
[0095] 1. Synthesis of diamines
[0096] First, synthesize a monoamine. Iodine, thiourea, and acetophenone are heated and stirred in a molar ratio of 1:2:1. Stir for 8 to 12 hours at 100 to 120°C. The mixture is then dissolved in sufficient deionized water. Once fully dissolved, it is neutralized with a sufficient amount of 1 mol / L sodium hydroxide solution to produce a precipitate, which is collected and dried. The precipitate is recrystallized from a 50 wt.% ethanol solution to produce 4-(2-aminothiazole)-benzene.
[0097] Subsequently, a diamine was synthesized by mixing 4-(2-aminothiazole)-benzene and 2-formylbenzenesulfonic acid in a molar ratio of 2:1 in a sufficient amount of hydrochloric acid solution. After reflux condensation at 100° C. for 8 to 12 hours, the mixture was cooled to room temperature and the product diamine was collected by filtration.
[0098] 2. Synthesis of sulfonated polyimide (SPI)
[0099] The diamine obtained in step 1 and pyromellitic dianhydride (molar mass ratio of 1:1) were mixed with N-methylpyrrolidone, and the solution was stirred for 24 hours to prepare polyamic acid. Pyridine and acetic anhydride (the volume ratio of pyridine to acetic anhydride was 2.2:1) were then added and mixed, and the stirring time was 8 to 12 hours at a stirring temperature of 100°C. The mixture was then transferred to sufficient methanol and stirred at room temperature for 8 to 12 hours. Finally, the precipitate was filtered out, washed with methanol and hot deionized water, and dried at 100°C to obtain sulfonated polyimide (SPI).
[0100] 3. Preparation of composite membrane
[0101] First, polybenzimidazole (PBI) powder was dissolved in N,N-dimethylacetamide at 150°C under an inert atmosphere. The sulfonated polyimide (SPI) powder prepared in step 2 was mixed with the polybenzimidazole (PBI) solution (5% SPI:PBI by mass ratio) and stirred at 30°C for 8 hours. The mixture was then cast onto a glass plate using a doctor blade. The wet film thickness was controlled by adjusting the doctor blade gap. The composite membrane was then heated in a vacuum at 80°C to obtain the desired film.
[0102] Example 3
[0103] A composite film, the preparation method of which is as follows:
[0104] 1. Synthesis of diamines
[0105] First, synthesize a monoamine. Iodine, thiourea, and acetophenone are heated and stirred in a molar ratio of 1:2:1. Stir for 8 to 12 hours at 100 to 120°C. The mixture is then dissolved in sufficient deionized water. Once fully dissolved, it is neutralized with a sufficient amount of 1 mol / L sodium hydroxide solution to produce a precipitate, which is collected and dried. The precipitate is recrystallized from a 50 wt.% ethanol solution to produce 4-(2-aminothiazole)-benzene.
[0106] Subsequently, a diamine was synthesized by mixing 4-(2-aminothiazole)-benzene and 2-formylbenzenesulfonic acid in a molar ratio of 2:1 in a sufficient amount of hydrochloric acid solution. After reflux condensation at 100° C. for 8 to 12 hours, the mixture was cooled to room temperature and the product diamine was collected by filtration.
[0107] 2. Synthesis of sulfonated polyimide (SPI)
[0108] The diamine obtained in step 1 and pyromellitic dianhydride (molar mass ratio of 1:1) were mixed with N-methylpyrrolidone, and the solution was stirred for 24 hours to prepare polyamic acid. Pyridine and acetic anhydride (the volume ratio of pyridine to acetic anhydride was 2.2:1) were then added and mixed, and the stirring time was 8 to 12 hours at a stirring temperature of 100°C. The mixture was then transferred to sufficient methanol and stirred at room temperature for 8 to 12 hours. Finally, the precipitate was filtered out, washed with methanol and hot deionized water, and dried at 100°C to obtain sulfonated polyimide (SPI).
[0109] 3. Preparation of composite membrane
[0110] First, polybenzimidazole (PBI) powder was dissolved in N,N-dimethylacetamide at 150°C under an inert atmosphere. The sulfonated polyimide (SPI) powder prepared in step 2 was mixed with the polybenzimidazole (PBI) solution (SPI:PBI mass ratio of 25%) and stirred at 30°C for 8 hours. The mixture was then cast onto a glass plate using a doctor blade. The wet film thickness was controlled by adjusting the doctor blade gap. The composite membrane was then heated in a vacuum at 80°C to obtain the desired film.
[0111] Example 4
[0112] A composite film, the preparation method of which is as follows:
[0113] 1. Synthesis of diamines
[0114] First, synthesize a monoamine. Iodine, thiourea, and acetophenone are heated and stirred in a molar ratio of 1:2:1. Stir for 8 to 12 hours at 100 to 120°C. The mixture is then dissolved in sufficient deionized water. Once fully dissolved, it is neutralized with a sufficient amount of 1 mol / L sodium hydroxide solution to produce a precipitate, which is collected and dried. The precipitate is recrystallized from a 50 wt.% ethanol solution to produce 4-(2-aminothiazole)-benzene.
[0115] Subsequently, a diamine was synthesized by mixing 4-(2-aminothiazole)-benzene and 2-formylbenzenesulfonic acid in a molar ratio of 2:1 in a sufficient amount of hydrochloric acid solution. After reflux condensation at 100° C. for 8 to 12 hours, the mixture was cooled to room temperature and the product diamine was collected by filtration.
[0116] 2. Synthesis of sulfonated polyimide (SPI)
[0117] The diamine obtained in step 1 and pyromellitic dianhydride (molar mass ratio of 1:1) were mixed with N-methylpyrrolidone, and the solution was stirred for 24 hours to prepare polyamic acid. Pyridine and acetic anhydride (the volume ratio of pyridine to acetic anhydride was 2.2:1) were then added and mixed, and the stirring time was 8 to 12 hours at a stirring temperature of 100°C. The mixture was then transferred to sufficient methanol and stirred at room temperature for 8 to 12 hours. Finally, the precipitate was filtered out, washed with methanol and hot deionized water, and dried at 100°C to obtain sulfonated polyimide (SPI).
[0118] 3. Preparation of composite membrane
[0119] First, polybenzimidazole (PBI) powder was dissolved in N,N-dimethylacetamide at 150°C under an inert atmosphere. The sulfonated polyimide (SPI) powder prepared in step 2 was mixed with the polybenzimidazole (PBI) solution (SPI:PBI mass ratio: 40%) and stirred at 30°C for 8 hours. The mixture was then cast onto a glass plate using a doctor blade. The wet film thickness was controlled by adjusting the doctor blade gap. The composite membrane was then heated in a vacuum at 80°C to obtain the desired film.
[0120] Example 5
[0121] A composite film, the preparation method of which is as follows:
[0122] 1. Synthesis of diamines
[0123] First, synthesize a monoamine. Iodine, thiourea, and acetophenone are heated and stirred in a molar ratio of 1:2:1. Stir for 8 to 12 hours at 100 to 120°C. The mixture is then dissolved in sufficient deionized water. Once fully dissolved, it is neutralized with a sufficient amount of 1 mol / L sodium hydroxide solution to produce a precipitate, which is collected and dried. The precipitate is recrystallized from a 50 wt.% ethanol solution to produce 4-(2-aminothiazole)-benzene.
[0124] Subsequently, a diamine was synthesized by mixing 4-(2-aminothiazole)-benzene and 2-formylbenzenesulfonic acid in a molar ratio of 2:1 in a sufficient amount of hydrochloric acid solution. After reflux condensation at 100° C. for 8 to 12 hours, the mixture was cooled to room temperature and the product diamine was collected by filtration.
[0125] 2. Synthesis of sulfonated polyimide (SPI)
[0126] The diamine obtained in step 1 and pyromellitic dianhydride (molar mass ratio of 1:1) were mixed with N-methylpyrrolidone, and the solution was stirred for 24 hours to prepare polyamic acid. Pyridine and acetic anhydride (the volume ratio of pyridine to acetic anhydride was 2.2:1) were then added and mixed, and the stirring time was 8 to 12 hours at a stirring temperature of 100°C. The mixture was then transferred to sufficient methanol and stirred at room temperature for 8 to 12 hours. Finally, the precipitate was filtered out, washed with methanol and hot deionized water, and dried at 100°C to obtain sulfonated polyimide (SPI).
[0127] 3. Preparation of composite membrane
[0128] First, polybenzimidazole (PBI) powder was dissolved in N,N-dimethylacetamide at 150°C under an inert atmosphere. The sulfonated polyimide (SPI) powder prepared in step 2 was mixed with the polybenzimidazole (PBI) solution (SPI:PBI mass ratio: 45%) and stirred at 30°C for 8 hours. The mixture was then cast onto a glass plate using a doctor blade. The wet film thickness was controlled by adjusting the doctor blade gap. The composite film was then heated in a vacuum at 80°C to obtain the desired film.
[0129] Example 6
[0130] A composite film, the preparation method of which is as follows:
[0131] 1. Synthesis of diamines
[0132] First, synthesize a monoamine. Iodine, thiourea, and acetophenone are heated and stirred in a molar ratio of 1:2:1. Stir for 8 to 12 hours at 100 to 120°C. The mixture is then dissolved in sufficient deionized water. Once fully dissolved, it is neutralized with a sufficient amount of 1 mol / L sodium hydroxide solution to produce a precipitate, which is collected and dried. The precipitate is recrystallized from a 50 wt.% ethanol solution to produce 4-(2-aminothiazole)-benzene.
[0133] Subsequently, a diamine was synthesized by mixing 4-(2-aminothiazole)-benzene and 2-formylbenzenesulfonic acid in a molar ratio of 2:1 in a sufficient amount of hydrochloric acid solution. After reflux condensation at 100° C. for 8 to 12 hours, the mixture was cooled to room temperature and the product diamine was collected by filtration.
[0134] 2. Synthesis of sulfonated polyimide (SPI)
[0135] The diamine obtained in step 1 and pyromellitic dianhydride (molar mass ratio of 1:1) were mixed with N-methylpyrrolidone, and the solution was stirred for 24 hours to prepare polyamic acid. Pyridine and acetic anhydride (the volume ratio of pyridine to acetic anhydride was 2.2:1) were then added and mixed, and the stirring time was 8 to 12 hours at a stirring temperature of 100°C. The mixture was then transferred to sufficient methanol and stirred at room temperature for 8 to 12 hours. Finally, the precipitate was filtered out, washed with methanol and hot deionized water, and dried at 100°C to obtain sulfonated polyimide (SPI).
[0136] 3. Synthesis of Yb-doped perovskite nanoparticles
[0137] Cerium ammonium nitrate was mixed with n-butanol to react and prepare cerium n-butoxide. Subsequently, strontium acetate, cerium n-butoxide, and ytterbium acetate (molar mass ratio of 10:9:1) were dissolved in sufficient deionized water to prepare three solutions. These three solutions were added to the stearic acid solution and stirred until a uniform gel was obtained. The gel was then cooled to room temperature and heat-treated at 120°C for 3 hours. The resulting dried gel was treated at 1000°C for 24 hours to obtain Yb-doped perovskite nanoparticles with a particle size of 1.5447 nm.
[0138] 4. Preparation of composite membrane
[0139] First, a specific amount of sulfonated polyimide (SPI) is mixed with polybenzimidazole (PBI) in N,N-dimethylacetamide (SPI: PBI mass ratio is 25%), and then stirred at 30°C for 8 to 12 hours. Next, the Yb-doped perovskite nanoparticles prepared in step 3 are added to another portion of polybenzimidazole (PBI) in N,N-dimethylacetamide and fully dispersed (the mass proportion of Yb-doped perovskite nanoparticles in the composite film is 8%). While dispersing, it is mixed with the PBI / SPI solution to obtain a uniform solution. Finally, a scraper is used to cast the mixture onto a glass plate. The gap between the scraper and the coating can be controlled to control the thickness of the wet film. It is then heated in vacuum at 80°C to obtain a composite film.
[0140] Example 7
[0141] A composite film, the preparation method of which is as follows:
[0142] 1. Synthesis of diamines
[0143] First, synthesize a monoamine. Iodine, thiourea, and acetophenone are heated and stirred in a molar ratio of 1:2:1. Stir for 8 to 12 hours at 100 to 120°C. The mixture is then dissolved in sufficient deionized water. Once fully dissolved, it is neutralized with a sufficient amount of 1 mol / L sodium hydroxide solution to produce a precipitate, which is collected and dried. The precipitate is recrystallized from a 50 wt.% ethanol solution to produce 4-(2-aminothiazole)-benzene.
[0144] Subsequently, a diamine was synthesized by mixing 4-(2-aminothiazole)-benzene and 2-formylbenzenesulfonic acid in a molar ratio of 2:1 in a sufficient amount of hydrochloric acid solution. After reflux condensation at 100° C. for 8 to 12 hours, the mixture was cooled to room temperature and the product diamine was collected by filtration.
[0145] 2. Synthesis of sulfonated polyimide (SPI)
[0146] The diamine obtained in step 1 and pyromellitic dianhydride (molar mass ratio of 1:1) were mixed with N-methylpyrrolidone, and the solution was stirred for 24 hours to prepare polyamic acid. Pyridine and acetic anhydride (the volume ratio of pyridine to acetic anhydride was 2.2:1) were then added and mixed, and the stirring time was 8 to 12 hours at a stirring temperature of 100°C. The mixture was then transferred to sufficient methanol and stirred at room temperature for 8 to 12 hours. Finally, the precipitate was filtered out, washed with methanol and hot deionized water, and dried at 100°C to obtain sulfonated polyimide (SPI).
[0147] 3. Synthesis of Yb-doped perovskite nanoparticles
[0148] Cerium ammonium nitrate was mixed with n-butanol to react and prepare cerium n-butoxide. Subsequently, strontium acetate, cerium n-butoxide, and ytterbium acetate (molar mass ratio of 10:9:1) were dissolved in sufficient deionized water to prepare three solutions. These three solutions were added to the stearic acid solution and stirred until a uniform gel was obtained. The gel was then cooled to room temperature and heat-treated at 120°C for 3 hours. The resulting dried gel was treated at 1000°C for 24 hours to obtain Yb-doped perovskite nanoparticles with a particle size of 1.5447 nm.
[0149] 4. Preparation of composite membrane
[0150] First, a specific amount of sulfonated polyimide (SPI) is mixed with polybenzimidazole (PBI) in N,N-dimethylacetamide (SPI: PBI mass ratio is 25%), and then stirred at 30°C for 8 to 12 hours. Next, the Yb-doped perovskite nanoparticles prepared in step 3 are added to another portion of polybenzimidazole (PBI) in N,N-dimethylacetamide and fully dispersed (the mass proportion of Yb-doped perovskite nanoparticles in the composite film is 15%). While dispersing, it is mixed with the PBI / SPI solution to obtain a uniform solution. Finally, a scraper is used to cast the mixture onto a glass plate. The gap of the scraper can be controlled to control the thickness of the wet film. It is then heated in vacuum at 80°C to obtain a composite film.
[0151] Example 8
[0152] A composite film, the preparation method of which is as follows:
[0153] 1. Synthesis of diamines
[0154] First, synthesize a monoamine. Iodine, thiourea, and acetophenone are heated and stirred in a molar ratio of 1:2:1. Stir for 8 to 12 hours at 100 to 120°C. The mixture is then dissolved in sufficient deionized water. Once fully dissolved, it is neutralized with a sufficient amount of 1 mol / L sodium hydroxide solution to produce a precipitate, which is collected and dried. The precipitate is recrystallized from a 50 wt.% ethanol solution to produce 4-(2-aminothiazole)-benzene.
[0155] Subsequently, a diamine was synthesized by mixing 4-(2-aminothiazole)-benzene and 2-formylbenzenesulfonic acid in a molar ratio of 2:1 in a sufficient amount of hydrochloric acid solution. After reflux condensation at 100° C. for 8 to 12 hours, the mixture was cooled to room temperature and the product diamine was collected by filtration.
[0156] 2. Synthesis of sulfonated polyimide (SPI)
[0157] The diamine obtained in step 1 and pyromellitic dianhydride (molar mass ratio of 1:1) were mixed with N-methylpyrrolidone, and the solution was stirred for 24 hours to prepare polyamic acid. Pyridine and acetic anhydride (the volume ratio of pyridine to acetic anhydride was 2.2:1) were then added and mixed, and the stirring time was 8 to 12 hours at a stirring temperature of 100°C. The mixture was then transferred to sufficient methanol and stirred at room temperature for 8 to 12 hours. Finally, the precipitate was filtered out, washed with methanol and hot deionized water, and dried at 100°C to obtain sulfonated polyimide (SPI).
[0158] 3. Synthesis of Yb-doped perovskite nanoparticles
[0159] Cerium ammonium nitrate was mixed with n-butanol to react and prepare cerium n-butoxide. Subsequently, strontium acetate, cerium n-butoxide, and ytterbium acetate (molar mass ratio of 10:9:1) were dissolved in sufficient deionized water to prepare three solutions. These three solutions were added to the stearic acid solution and stirred until a uniform gel was obtained. The gel was then cooled to room temperature and heat-treated at 120°C for 3 hours. The resulting dried gel was treated at 1000°C for 24 hours to obtain Yb-doped perovskite nanoparticles with a particle size of 1.5447 nm.
[0160] 4. Preparation of composite membrane
[0161] First, a specific amount of sulfonated polyimide (SPI) is mixed with polybenzimidazole (PBI) in N,N-dimethylacetamide (SPI: PBI mass ratio is 25%), and then stirred at 30°C for 8 to 12 hours. Next, the Yb-doped perovskite nanoparticles prepared in step 3 are added to another portion of polybenzimidazole (PBI) in N,N-dimethylacetamide and fully dispersed (the mass proportion of Yb-doped perovskite nanoparticles in the composite film is 20%). While dispersing, it is mixed with the PBI / SPI solution to obtain a uniform solution. Finally, a scraper is used to cast the mixture onto a glass plate. The gap between the scraper and the coating can be controlled to control the thickness of the wet film. It is then heated in vacuum at 80°C to obtain a composite film.
[0162] Comparative Example 1
[0163] Commercially available phosphoric acid high-temperature membrane.
[0164] Performance tests were conducted on the films provided in the various examples and comparative examples (it should be noted that the thickness of the films provided in the various examples and comparative examples was 55 μm), and the results are shown in the following table.
[0165]
[0166] As can be seen from the above table, the composite membrane provided by the present application can have a high proton conductivity at high temperature and a good elastic modulus.
[0167] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a hard limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numbers within the range. For example, the description of a range from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0168] In this application, unless otherwise specified, the directional words used, such as "upper" and "lower", refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of the present application specification, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships can exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" refers to one or more, and "plurality" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b and c can be single or multiple.
[0169] The foregoing is merely a list of specific embodiments of the present application, intended to enable those skilled in the art to understand or implement the present application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application is not limited to the embodiments shown herein, but is intended to conform to the broadest scope consistent with the principles and novel features of the present application.
Claims
1. A composite film, It is characterized in that The composite membrane comprises a membrane matrix, and the components of the membrane matrix include sulfonated polyimide and polybenzimidazole, wherein the mass ratio of the sulfonated polyimide to the polybenzimidazole is (5-40):
100.
2. The composite film according to claim 1, It is characterized in that The composite film further comprises Yb-doped perovskite nanoparticles, and the Yb-doped perovskite nanoparticles are embedded in the film matrix.
3. The composite membrane according to claim 2, It is characterized in that The mass proportion of the Yb-doped perovskite nanoparticles in the composite film does not exceed 15%.
4. The composite film according to claim 2, It is characterized in that The particle size of the Yb-doped perovskite nanoparticles is 40 nm to 60 nm.
5. The composite film according to claim 1, It is characterized in that The sulfonated polyimide comprises: Wherein, n is selected from any positive integer.
6. A method for preparing a composite film, It is characterized in that The composite film is a composite film according to any one of claims 1 to 5; the method comprises: Sulfonated polyimide and polybenzimidazole are obtained; Mixing the sulfonated polyimide and polybenzimidazole in a solvent to obtain a slurry; The slurry is subjected to thin film preparation to obtain a composite membrane.
7. The method for preparing the composite membrane according to claim 6, It is characterized in that The preparation method of the sulfonated polyimide comprises: iodine, thiourea and acetophenone are heated and mixed to obtain a mixture; The mixture is dissolved in a solvent, and then neutralized and precipitated to obtain a precipitate; Recrystallizing the precipitate to obtain a monoamine; The monoamine and 2-formylbenzenesulfonic acid are mixed and reacted to obtain a sulfonated aromatic diamine; The sulfonated aromatic diamine and pyromellitic dianhydride are reacted to obtain polyamic acid; The polyamic acid, pyridine and acetic anhydride are mixed and reacted to obtain sulfonated polyimide.
8. The method for preparing the composite membrane according to claim 6, It is characterized in that The paste also includes Yb-doped perovskite nanoparticles.
9. The method for preparing the composite membrane according to claim 8, It is characterized in that The preparation method of the Yb-doped perovskite nanoparticles comprises: Strontium acetate, cerium n-butoxide and ytterbium acetate are mixed in a stearic acid solution to obtain a gel; The gel is heat treated and then sintered to obtain Yb-doped perovskite nanoparticles.
10. A fuel cell, It is characterized in that The fuel cell comprises the composite membrane according to any one of claims 1 to 5.