Rare-earth-free permanent magnet high-efficiency low-noise motor structure and manufacturing method thereof

By using strontium ferrite material and casing table design in rare earth-free permanent magnet motors, combined with wet molding and pulse charging technology, the motor efficiency and noise problems are solved, and the motor structure is achieved is improved. Overall performance.

CN118983969AInactive Publication Date: 2024-11-19HUZHOU YONGCHANG BEISHITUO ELECTRIC APPLIANCE INDAL
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411464229.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing rare earth-free permanent magnet motors are difficult to meet the needs of high-quality products in terms of efficiency, noise and power consumption.

Method used

A rare earth-free permanent magnet high-efficiency low-drying motor structure is designed, using strontium ferrite material, by setting a rectangular mounting groove and strip-shaped projection on the rotor chip, and a casing table on the permanent magnet, combined with wet forming Process and pulse charging technology improve the magnetic field distribution and electromagnetic pushing force, reducing noise and loss.

Benefits of technology

Achieve more efficient magnetic field interactions, reduce noise and power consumption, and improve motor efficiency and economy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983969A_ABST
    Figure CN118983969A_ABST
Patent Text Reader

Abstract

The invention provides a rare-earth-free permanent magnet high-efficiency low-noise motor structure, a rotor in the motor structure comprises a rotor chip and a permanent magnet, the rotor chip is provided with a rectangular mounting groove for mounting the permanent magnet, the outer edge of the rotor is integrally provided with strip-shaped protruding parts located at the two sides of the rectangular mounting groove, the permanent magnet is integrally provided with a clamping table, and the clamping table is provided with a clamping groove. The clamping tables are matched with the left and right adjacent strip-shaped protruding parts, the outer side faces of the clamping tables are arc-shaped and are concentric arc faces with the same radius as the rotor, and the permanent magnets are higher than the rotor. Through the arrangement of the clamping table, the distribution of a magnetic field formed on the surface of the magnetized rotor is closer to an ideal sine wave; and the pulsation amplitude is reduced, so that the vibration and the noise are correspondingly reduced. The invention further provides a manufacturing method of the rare-earth-free permanent magnet high-efficiency low-noise motor structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of motor structure and manufacturing thereof, in particular to a rare earth-free permanent magnet high-efficiency and low-dryness motor structure, and also to a manufacturing method of the motor structure. Background Art

[0002] With the increasing use of rare earth permanent magnet materials, especially the rapid development of new energy vehicles, the price of rare earth permanent magnet materials used in their drive motors is also increasing rapidly.

[0003] The performance of permanent magnets used in motor rotors affects the economic efficiency and operating characteristics of the motor. Generally speaking, the greater the motor power, the higher the maximum efficiency of the motor. With NdFeB permanent magnet synchronous motors, the maximum efficiency can reach more than 97%, or even 98%.

[0004] When designing the motor structure, the use of rare earth permanent magnet materials can increase the body density power and also improve the motor efficiency at the same time, but its high price is unaffordable for some fields (for example: variable frequency washing machines).

[0005] Although rare earth-free permanent magnet motors have existed before, their efficiency, noise, power consumption and other indicators cannot meet the needs of high-quality products.

[0006] Therefore, we have made improvements to this and proposed a rare earth-free permanent magnet high-efficiency and low-noise motor structure and manufacturing method. Summary of the invention

[0007] The purpose of the present invention is to address the fact that the efficiency, noise, power consumption and other indicators of the existing rare earth-free permanent magnet motors are difficult to meet the needs of high-quality products.

[0008] In order to achieve the above-mentioned purpose of the invention, the present invention provides a rare earth-free permanent magnet high-efficiency and low-noise motor structure to improve the above-mentioned problem.

[0009] The specific application is as follows: A rare earth-free permanent magnet high-efficiency and low-dryness motor structure, wherein the motor rotor comprises a rotor chip and a permanent magnet, wherein a rectangular mounting groove for mounting the permanent magnet is provided on the rotor chip, and the outer edge of the rotor chip is integrally provided with strip-shaped protrusions located on both sides of the rectangular mounting groove, and a clamping platform is integrally provided on the permanent magnet; the clamping platform is adapted to two adjacent strip-shaped protrusions on the left and right, and the outer side surface of the clamping platform is arc-shaped, and is a concentric arc surface with the same radius as the rotor chip, and the height of the permanent magnet is higher than the rotor chip.

[0010] As a preferred technical solution of the present application, the height of the permanent magnet is 4 mm to 6 mm higher than the plane height of the rotor chip.

[0011] The present application also provides a method for manufacturing the above-mentioned rare earth-free permanent magnet high-efficiency and low-dryness motor structure, comprising the following steps: S1. The permanent magnet is made of strontium ferrite material and adopts a wet molding process. During the molding and pressure holding time, the permanent magnet is pre-magnetized in a pulse manner in the vertical direction of the cross section, which is consistent with the magnetization direction of the permanent magnet embedded in the rotor chip after assembly, and the blank is sintered; S2, further processing the sintered permanent magnet so that it can be fitted into the rectangular mounting slot; S3, using a mounting device to mount the permanent magnet into the rectangular mounting groove of the rotor chip; S4. Injection molding the rotor and assemble it with the stator and other motor parts to form a motor.

[0012] As a preferred technical solution of this application, in the step S1: S1a, the strontium ferrite material is a mixture of strontium carbonate and ferric oxide, which is first added to a ball mill, 50% water is added according to weight percentage, and ball milled for 4 to 6 hours; S1b, after the ball-milled material is filtered through a filter press to remove moisture, it is put into a sagger and pre-fired in a kiln. The pre-fired temperature is kept between 1400℃ and 1420℃ for 2 to 4 hours to fully crystallize and form the required microscopic morphology; S1c, the pre-burned strontium ferrite material is coarsely crushed in a vibrating ball mill; S1d, coarsely crushed material, water, and anti-flocculant are prepared in the weight percentage of material: water: anti-flocculant = 65:34.9:0.1, and then put into a ball mill and add water for 8 to 10 hours, and filter the ball-milled slurry; S1e, forming a blank according to the permanent magnet processing drawing, and pre-magnetizing in a pulse manner in a direction perpendicular to the cross section of the permanent magnet during the forming and holding time, and the pre-magnetizing direction is consistent with the magnetizing direction of the permanent magnet embedded in the rotor after assembly; S1f. Sinter the formed blank at a temperature between 1260°C and 1275°C for 3 to 5 hours.

[0013] As a preferred technical solution of the present application, in the step S1c: after crushing, the particle size of the coarse granular powder is 1 to 5 microns, and the distribution of the particle size approaches a normal distribution. The particle size of the coarse granular powder is preferably 3 microns.

[0014] As a preferred technical solution of the present application, during the molding and holding time, three consecutive pulses are used to pre-magnetize in the direction perpendicular to the cross section of the permanent magnet. This method helps to improve the residual magnetic properties of the permanent magnet.

[0015] As a preferred technical solution of the present application, during pre-calcination, the temperature rise time of 100℃ to 300℃ is less than 30 minutes. The purpose is to quickly volatilize the remaining water after filter pressing, and the water forms air gaps in the material during the volatilization process, which is convenient for crushing.

[0016] Compared with the prior art, the present invention has the following beneficial effects: In the scheme of this application: 1. The original permanent magnet is rectangular in shape. After being installed in the rectangular installation groove, the existence of the strip-shaped protrusion causes a gap between the permanent magnet and the outer circle of the rotor chip; After magnetization, the residual magnetism of the permanent magnet forms a surface magnetic field distribution through the rotor chip, but the height difference between the outer cylindrical surface of the rotor chip and the permanent magnet reduces the magnetic field strength of the permanent magnet rotor, that is, it reduces the magnetic field interaction force between the rotor and the stator, and reduces the efficiency; at the same time, due to the height difference between the outer cylindrical surface of the rotor chip and the permanent magnet surface, the distribution of the magnetic field is changed, and the magnetic field pulsation is increased. The magnetic field pulsation directly affects vibration and noise; By setting up the card table, the magnetic field distribution formed on the rotor surface after magnetization is closer to the ideal sine wave; the pulsation amplitude is reduced, so the vibration and noise are reduced accordingly; 2. The height of the permanent magnet is 4mm to 6mm higher than the plane height of the rotor chip. The higher part of the permanent magnet and the higher part of the stator magnetizer interact to form an electromagnetic driving force, making full use of the edge of the winding, improving the efficiency of the motor and reducing losses; 3. The permanent magnet is installed in the rotor chip through the provided installation device. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A schematic diagram of the structure of a rare earth-free permanent magnet high-efficiency and low-noise motor provided in this application; Figure 2 The rare earth-free permanent magnet high-efficiency and low-noise motor structure provided in this application Figure 1 A schematic diagram of the enlarged structure at A in the middle; Figure 3 A schematic diagram of the structure of the installation device of the rare earth-free permanent magnet high-efficiency and low-dryness motor structure provided in this application; Figure 4 Schematic diagram of the rotating mechanism structure of the rare earth-free permanent magnet high-efficiency and low-noise motor structure provided in this application Figure 1 ; Figure 5 Schematic diagram of the rotating mechanism structure of the rare earth-free permanent magnet high-efficiency and low-noise motor structure provided in this application Figure 2 ; Figure 6 Schematic diagram of the installation mechanism of the rare earth-free permanent magnet high-efficiency and low-dryness motor structure provided in this application Figure 1 ; Figure 7 Schematic diagram of the installation mechanism of the rare earth-free permanent magnet high-efficiency and low-dryness motor structure provided in this application Figure 2 ; Figure 8 A structural schematic diagram of the glue spraying mechanism of the rare earth-free permanent magnet high-efficiency and low-dryness motor structure provided in this application.

[0018] Indicated in the figure: 1. rotor chip; 101. rectangular mounting groove; 102. strip-shaped protrusion; 2. Permanent magnet; 201. Card table; 3. Installation device; 31. Rotating mechanism; 311. Workbench; 312. Ratchet; 313. Rectangular slide rail; 314. Sliding block; 315. Support plate; 316. Ratchet; 317. Spring; 318. Vertical plate; 319. Inclined groove; 310. Sliding rod; 32. Installation mechanism; 321. Vertical pole; 322. Storage box; 323. Elastic rod; 324. Strip groove; 325. Rectangular groove; 326. Feeding chute; 327. Bending pipe; 328. Rectangular block; 329. Vertical slide; 33. Glue spraying mechanism; 331. Glue storage box; 332. Telescopic rod; 333. Piston plate; 334. Pipeline 1; 335. Pipeline 2; 336. One-way valve 1; 337. One-way valve 2; 338. Hose; 339. Spray nozzle. DETAILED DESCRIPTION

[0019] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0020] As described in the background art, the efficiency, noise, power consumption and other indicators of rare earth-free permanent magnet motors are difficult to meet the needs of high-quality products.

[0021] In order to solve this technical problem, the present invention provides a rare earth-free permanent magnet high-efficiency and low-noise motor structure and a manufacturing method, which are applied to the motor.

[0022] Specifically, please refer to Figure 1 and Figure 2 The rare earth-free permanent magnet high-efficiency and low-noise motor structure specifically includes: The motor rotor includes a rotor chip 1 and a permanent magnet 2. The rotor chip 1 is provided with a rectangular installation groove 101 for installing the permanent magnet 2, and the outer edge of the rotor chip 1 is integrally provided with strip-shaped protrusions 102 located on both sides of the rectangular installation groove 101. The permanent magnet 2 is integrally provided with a clamping platform 201; the clamping platform 201 is adapted to the two adjacent strip-shaped protrusions 102 on the left and right, and the outer side surface of the clamping platform 201 is arc-shaped, and is a concentric arc surface with the same radius as the rotor chip 1. The height of the permanent magnet 2 is higher than the rotor chip 1.

[0023] The height of the permanent magnet is 4 mm to 6 mm higher than the plane height of the rotor chip.

[0024] The rare earth-free permanent magnet high-efficiency and low-noise motor structure provided by the present invention makes the magnetic field distribution formed on the rotor surface after magnetization closer to the ideal sine wave by arranging a card table; the pulsation amplitude is reduced so that the vibration and noise are correspondingly reduced; the height of the permanent magnet is 4mm to 6mm higher than the plane height of the rotor chip; the raised part of the permanent magnet and the raised part of the stator higher than the stator magnetizer interact to form an electromagnetic driving force, which makes full use of the edge part of the winding, improves the efficiency of the motor and reduces the loss.

[0025] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings.

[0026] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features and technical solutions in the embodiments may be combined with each other.

[0027] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0028] Example 1, please refer to Figure 1-2, a rare earth-free permanent magnet high-efficiency and low-dryness motor structure, including a rotor chip 1 and a permanent magnet 2; a rectangular mounting groove 101 for mounting the permanent magnet 2 is opened on the rotor chip 1, and the outer edge of the rotor chip 1 is integrally provided with strip-shaped protrusions 102 located on both sides of the rectangular mounting groove 101; the original permanent magnet 2 is rectangular in shape, and after being installed in the rectangular mounting groove 101, due to the existence of the strip-shaped protrusions 102, there is a drop between the permanent magnet 2 and the outer circle of the rotor chip 1; after magnetization, the residual magnetism of the permanent magnet 2 forms a surface magnetic field distribution through the rotor chip 1, but the drop between the outer circle surface of the rotor chip and the permanent magnet 2 reduces the magnetic field strength of the rotor of the permanent magnet 2, and also That is, the magnetic field interaction force between the rotor and the stator is reduced, and the efficiency is reduced; at the same time, due to the difference between the outer cylindrical surface of the rotor chip and the surface of the permanent magnet 2, the distribution of the magnetic field is changed, and the magnetic field pulsation is increased. The magnetic field pulsation directly affects the vibration and noise; the permanent magnet 2 is integrally provided with a clamping platform 201, and the clamping platform 201 is adapted to the two adjacent strip-shaped protrusions 102 on the left and right, and the outer side surface of the clamping platform 201 is arc-shaped, and is a concentric arc surface with the same radius as the rotor chip 1; by setting the clamping platform 201, the magnetic field distribution formed on the rotor surface after magnetization is closer to the ideal sine wave; the pulsation amplitude is reduced, so that the vibration and noise are correspondingly reduced.

[0029] The height of the permanent magnet 2 is higher than the rotor chip 1; specifically, the height of the permanent magnet 2 is 4 mm higher than the plane height of the rotor chip 1. The raised portion of the permanent magnet 2 and the raised portion of the stator above the stator magnetizer interact to form an electromagnetic driving force, which makes full use of the edge portion of the winding, improves the efficiency of the motor and reduces losses.

[0030] The difference between Example 2 and Example 1 is that the height of the permanent magnet 2 is 6 mm higher than the plane height of the rotor core sheet 1 .

[0031] Embodiment 3, a method for manufacturing a rare earth-free permanent magnet high-efficiency and low-dryness motor structure, comprising the following steps: S1. The permanent magnet is made of strontium ferrite material and adopts a wet molding process. During the molding and pressure holding time, the permanent magnet is pre-magnetized in a pulse manner in the vertical direction of the cross section, which is consistent with the magnetization direction of the permanent magnet embedded in the rotor chip after assembly, and the blank is sintered; S2, further processing the sintered permanent magnet so that it can be fitted into the rectangular mounting slot 101; S3, using the installation device 3 to install the permanent magnet into the rectangular installation groove 101 of the rotor chip; S4. Injection molding the rotor and assemble it with the stator and other motor parts to form a motor.

[0032] In the step S1: S1a, the strontium ferrite material is a mixture of strontium carbonate and ferric oxide, which is first added to a ball mill, 50% of water is added according to weight percentage, and ball milled for 4 hours; S1b, After the ball-milled material is filtered by a filter press to remove moisture, it is placed in a sagger and pre-fired in a kiln. The pre-fired temperature is kept at 1400℃ for 2 hours to fully crystallize and form the required microscopic morphology; during pre-fired, the temperature rise time of 100℃ is less than 30 minutes. The purpose is to make the remaining moisture after the filter press evaporate quickly, and the moisture forms air gaps in the material during the volatilization process, which is convenient for crushing.

[0033] S1c, the pre-burned strontium ferrite material is coarsely crushed in a vibrating ball mill; in the step S1c: after crushing, the particle size of the coarse granular powder is 1 to 5 microns, and the distribution of the particle size is close to normal distribution. The particle size of the coarse granular powder is preferably 3 microns.

[0034] S1d, coarsely crushed material, water, and anti-flocculant are prepared in the following weight percentages: material: water: anti-flocculant = 65: 34.9: 0.1, and then loaded into a ball mill and added with water for 8 hours, and the milled slurry is filtered; S1e, according to the permanent magnet processing drawings, the blank is formed, and during the forming and holding time, the vertical direction of the cross section of the permanent magnet is pre-magnetized by pulse mode, and the pre-magnetization direction is consistent with the magnetization direction of the permanent magnet embedded in the rotor after assembly; during the forming and holding time, the vertical direction of the cross section of the permanent magnet is pre-magnetized by three consecutive pulses. This method helps to improve the residual magnetic properties of the permanent magnet.

[0035] S1f, sinter the formed blank at a sintering temperature of 1260°C for 3 hours.

[0036] like Figures 3 to 8 The mounting device 3 includes a rotating mechanism 31 for driving the rotor 1 to rotate, a mounting mechanism 32 for mounting the permanent magnet 2 into the rectangular mounting groove 101, and a glue spraying mechanism 33 for conveying glue into the rectangular mounting groove 101. The rotating mechanism 31 includes a workbench 311, and a ratchet 312 rotatably connected to the upper surface of the workbench 311 for carrying the rotor chip 1. A rectangular slide rail 313 is fixedly installed on the upper surface of the workbench 311, and a slider 314 is slidably connected in the rectangular slide rail 313. Two support plates 315 distributed up and down are vertically fixed to the surface of the slider 314. A ratchet 316 is rotatably connected between the two support plates 315, and the ratchet 316 can mesh with the ratchet 312. A spring 317 is fixedly installed between the ratchet 316 and the slider 314.

[0037] A vertical plate 318 driven by an external driving device is inserted on the surface of the rotor chip 1. The external driving device is an electric push rod that can drive the vertical plate 318 to move up and down. A bevel groove 319 is opened on the surface of the vertical plate 318. A sliding rod 310 is vertically fixed on the side of the slider 314 away from the support plate 315. The sliding rod 310 is slidably connected in the bevel groove 319.

[0038] A manufacturing method for a rare earth-free permanent magnet high-efficiency and low-dryness motor structure is further optimized, and the installation mechanism 32 includes a vertical rod 321 vertically fixed on the upper surface of the workbench 311, and a storage box 322 is fixedly installed on the upper end of the vertical rod 321. The upper surface and the rear surface of the storage box 322 are both open, and an elastic rod 323 is arranged on the outside of the storage box 322, and both ends of the elastic rod 323 are U-shaped structures, one end of which is fixed on the front surface of the storage box 322, and the other end extends to the interior of the storage box 322. The permanent magnet 2 to be installed is stored in the storage box 322, and one end of the elastic rod 323 is against the surface of the permanent magnet 2, and the surface of the storage box 322 is provided with a strip groove 324 for the elastic rod 323 to slide.

[0039] A rectangular groove 325 is provided on one side of the storage box 322 away from the elastic rod 323, and the width of the rectangular groove 325 is smaller than the thickness of the permanent magnet 2. A discharge groove 326 is provided on the lower surface of the storage box 322 and is interconnected with the rectangular groove 325. The width of the discharge groove 326 is sufficient for the permanent magnet 2 to pass through.

[0040] A bending pipe 327 is fixedly mounted on the upper surface of the vertical plate 318 , and a rectangular block 328 is fixedly mounted on the free end of the bending pipe 327 . The rectangular block 328 is adapted to the rectangular groove 325 and the material discharge groove 326 .

[0041] A vertical slide groove 329 communicating with the inclined groove 319 is formed on the surface of the vertical plate 318 , and the inclined groove 319 is slidably adapted to the vertical slide groove 329 .

[0042] The manufacturing method of a rare earth-free permanent magnet high-efficiency and low-dryness motor structure is further optimized. The glue spraying mechanism 33 includes a glue storage box 331 located below the rotor chip 1 and with an open upper surface. The glue storage box 331 is directly placed on the ground and is at the same horizontal plane as the supporting legs of the workbench 311 during use. A telescopic rod 332 is vertically fixed to the lower surface of the vertical plate 318, and the lower end of the telescopic rod 332 is fixedly connected to a piston plate 333 located in the glue storage box 331.

[0043] By providing the telescopic rod 332 , the vertical plate 318 can drive the rectangular block 328 to move downward to the inside of the rectangular installation groove 101 before pushing the piston plate 333 to move downward.

[0044] A pipe 1 334 and a pipe 2 335 which are interconnected with the interior of the glue storage box 331 are vertically fixed on the surface of the glue storage box 331. A one-way valve 1 336 is installed on the pipe 1 334, and a one-way valve 2 337 is installed on the pipe 2 335. A hose 338 is fixedly installed between the pipe 2 335 and the bent pipe 327. The interior of the rectangular block 328 is a hollow structure and is interconnected with the bent pipe 327. Nozzles 339 are fixedly installed on both the front and rear sides of the rectangular block 328.

[0045] The number of the nozzles 339 on the same side is at least two and they are equidistantly distributed.

[0046] The use process of the method for manufacturing the rare earth-free permanent magnet high-efficiency and low-dryness motor structure provided by the present invention is as follows: In the initial state, there is no permanent magnet 2 in the storage box 322 , the sliding rod 310 is located at the lower end of the vertical sliding groove 329 , and the rectangular block 328 is located above the storage box 322 .

[0047] The vertical plate 318 is driven upward by an external electric push rod, and the inner wall of the inclined groove 319 on the vertical plate 318 can push the sliding rod 310 to move in the horizontal direction. The sliding rod 310 can drive the ratchet 316 to move in the horizontal direction through the support plate 315. The ratchet 316 can gradually engage with the ratchet 312 and drive the ratchet 312 to rotate. The ratchet 312 can drive the rotor chip 1 to rotate, so that one of the rectangular mounting grooves 101 on the rotor chip 1 rotates to the bottom of the rectangular block 328.

[0048] When the vertical plate 318 moves downward, the ratchet teeth 316 move back, and at this time the ratchet teeth 316 cannot drive the ratchet wheel 312 to rotate.

[0049] Then the external electric push rod drives the vertical plate 318 to continue to move downward. At this time, the sliding rod 310 is located in the vertical slide groove 329 and will not move in the horizontal direction. At the same time, the vertical plate 318 can drive the rectangular block 328 to move downward through the bending pipe 327. When the rectangular block 328 moves downward to one of the rectangular mounting grooves 101, the telescopic rod 332 is shortened to the extreme position. When the vertical plate 318 continues to move downward, the telescopic rod 332 can drive the piston plate 333 to move downward, and the glue stored in the glue storage box 331 is transported to the rectangular block 328 through the pipe 2 335 and the hose 338, and sprayed inside the rectangular mounting groove 101 through the nozzle 339.

[0050] After all the rectangular installation grooves 101 are sprayed with glue, the permanent magnet 2 to be installed is placed in the storage box 322 , and one end of the elastic rod 323 presses against the permanent magnet 2 .

[0051] Since the rectangular installation groove 101 is located directly below the rectangular block 328 , when the rectangular block 328 moves downward, it can push one of the permanent magnets 2 to move downward through the discharge groove 326 into the rectangular installation groove 101 , thereby completing the installation of the permanent magnet 2 .

[0052] Embodiment 4 is different from Embodiment 3 in that: In the step S1: S1a, the strontium ferrite material is a mixture of strontium carbonate and ferric oxide, which is first added to a ball mill, 50% of water is added according to weight percentage, and ball milled for 6 hours; S1b, After the ball-milled material is filtered through a filter press to remove moisture, it is placed in a sagger and pre-fired in a kiln. The pre-fired temperature is kept at 1420℃ for 4 hours to fully crystallize and form the required microscopic morphology; during pre-fired, the temperature rise time at 300℃ is less than 30 minutes. The purpose is to make the remaining moisture after the filter press evaporate quickly, and the moisture forms air gaps in the material during the volatilization process, which is convenient for crushing.

[0053] S1c, the pre-burned strontium ferrite material is coarsely crushed in a vibrating ball mill; in the step S1c: after crushing, the particle size of the coarse granular powder is 1 to 5 microns, and the distribution of the particle size is close to normal distribution. The particle size of the coarse granular powder is preferably 3 microns.

[0054] S1d, coarsely crushed material, water, and anti-flocculant are prepared in the following weight percentages: material: water: anti-flocculant = 65: 34.9: 0.1, and then loaded into a ball mill and added with water for 10 hours, and the milled slurry is filtered; S1e, according to the permanent magnet processing drawings, the blank is formed, and during the forming and holding time, the vertical direction of the cross section of the permanent magnet is pre-magnetized by pulse mode, and the pre-magnetization direction is consistent with the magnetization direction of the permanent magnet embedded in the rotor after assembly; during the forming and holding time, the vertical direction of the cross section of the permanent magnet is pre-magnetized by three consecutive pulses. This method helps to improve the residual magnetic properties of the permanent magnet.

[0055] S1f. Sinter the formed blank at a sintering temperature of 1275°C for 5 hours.

[0056] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0057] Obviously, the embodiments described above are only some embodiments of the present invention, rather than all embodiments. The preferred embodiments of the present invention are given in the accompanying drawings, but they do not limit the patent scope of the present invention. The present invention can be implemented in many different forms. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive. Although the present invention has been described in detail with reference to the aforementioned embodiments, for those skilled in the art, it is still possible to modify the technical solutions recorded in the aforementioned specific embodiments, or to perform equivalent replacements for some of the technical features therein. Any equivalent structure made using the contents of the specification and drawings of the present invention, directly or indirectly used in other related technical fields, is also within the scope of patent protection of the present invention.

Claims

1. A rare earth-free permanent magnet high-efficiency and low-dryness motor structure, characterized in that: The motor rotor comprises a rotor chip (1) and a permanent magnet (2); the rotor chip (1) is provided with a rectangular installation groove (101) for installing the permanent magnet (2); the outer edge of the rotor chip (1) is integrally provided with strip-shaped protrusions (102) located on both sides of the rectangular installation groove (101); the permanent magnet (2) is integrally provided with a clamping platform (201); the clamping platform (201) is adapted to two adjacent strip-shaped protrusions (102) on the left and right, and the outer side surface of the clamping platform (201) is arc-shaped and is a concentric arc surface with the same radius as the rotor chip (1); the height of the permanent magnet (2) is higher than that of the rotor chip (1).

2. The rare earth-free permanent magnet high-efficiency and low-dryness motor structure according to claim 1 is characterized in that: The height of the permanent magnet is 4 mm to 6 mm higher than the plane height of the rotor chip.

3. A method for manufacturing a rare earth-free permanent magnet high-efficiency and low-dryness motor structure as claimed in claim 2, characterized in that: The steps include: S1. The permanent magnet is made of strontium ferrite material and adopts a wet molding process. During the molding and pressure holding time, the permanent magnet is pre-magnetized in a pulse manner in the vertical direction of the cross section, which is consistent with the magnetization direction of the permanent magnet embedded in the rotor chip after assembly, and the blank is sintered; S2, further processing the sintered permanent magnet so that it can be fitted into the rectangular mounting groove (101); S3, using the installation device (3) to install the permanent magnet into the rectangular installation groove (101) of the rotor chip; S4. Injection molding the rotor and assemble it with the stator and other motor parts to form a motor.

4. The manufacturing method according to claim 3, characterized in that: In the step S1: S1a, the strontium ferrite material is a mixture of strontium carbonate and ferric oxide, which is first added to a ball mill, 50% water is added according to weight percentage, and ball milled for 4 to 6 hours; S1b, after the ball-milled material is filtered through a filter press to remove moisture, it is put into a sagger and pre-fired in a kiln. The pre-fired temperature is kept between 1400℃ and 1420℃ for 2 to 4 hours to fully crystallize and form the required microscopic morphology; S1c, the pre-burned strontium ferrite material is coarsely crushed in a vibrating ball mill; S1d, coarsely crushed material, water, and anti-flocculant are prepared in the weight percentage of material: water: anti-flocculant = 65:34.9:0.1, and then put into a ball mill and add water for 8 to 10 hours, and filter the ball-milled slurry; S1e, forming a blank according to the permanent magnet processing drawing, and pre-magnetizing in a pulse manner in a direction perpendicular to the cross section of the permanent magnet during the forming and holding time, and the pre-magnetizing direction is consistent with the magnetizing direction of the permanent magnet embedded in the rotor after assembly; S1f. Sinter the formed blank at a temperature between 1260°C and 1275°C for 3 to 5 hours.

5. The manufacturing method according to claim 4, characterized in that: In the step S1d, the particle size of the powder after ball milling is 1 to 5 microns, and the distribution of the particle size approaches a normal distribution.

6. The manufacturing method according to claim 4, characterized in that: In the step S1b: during pre-firing, the temperature rise time from 100°C to 300°C is less than 30 minutes.

7. The manufacturing method according to claim 4, characterized in that: In the step S1e: during the molding and holding time, pre-magnetization is performed in a direction perpendicular to the cross section of the permanent magnet using three consecutive pulses.

Citation Information

Patent Citations

  • Method for producing permanent ferrite magnet with less shrinkage

    CN108101529A

  • Rotor and rotating electrical machine

    CN116325432A

  • Permanent magnet embedded rotor, manufacturing method and permanent magnet motor with rotor

    CN118589726A

  • Stator structure, winding method, motor and rotor manufacturing die

    CN118739681A

  • Bio-oxygen air disinfection and sterilization system used in multiple use facilities

    KR102201416B1