Doping modification method of hafnium oxide-based ferroelectric film
By adopting doping modification method in hafnium-based ferroelectric films, alternative doping states are formed, which reduces the coercive field, solves the problem of large coercive field at the nanoscale of hafnium-based ferroelectric films, and improves the reliability of the device performance and performance meet the requirements of low power consumption and high performance.
Patent Information
- Application Number
- CN202411047157.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
Hafnium-based ferroelectric film has a large coercive field at the nanoscale, resulting in device fatigue and breakdown, affecting reliability. The existing doping method is difficult to effectively reduce the coercive field and meet the requirements of low power consumption and high performance.
The doping modification method of hafnium oxide-based ferroelectric thin film is adopted to form a ferroelectric orthogonal phase through atomic layer deposition technology. Group IIA, Group IIIB or Group IIIA main group elements are selected as doping elements to form Replace doping states, regulate doping concentration and annealing temperature, and reduce coercive field.
It realizes the precise controllability of the coercive field of hafnium-based ferroelectric thin film, improves the reliability and performance of the device, meets the ferroelectricity advantages at the nanoscale, and reduces the risk of device failure.
Smart Images

Figure CN118984646A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ferroelectric material modification, and in particular relates to a doping modification method for a hafnium oxide-based ferroelectric film. Background Art
[0002] Ferroelectric memory has important application potential in automotive electronics, smart grids, aerospace and other fields due to its advantages such as fast read and write speed, non-volatility and low power consumption. As device size tends to be miniaturized and integrated, traditional perovskite ferroelectric materials are difficult to maintain ferroelectricity at the nanoscale, and there are problems such as miniaturization limit and incompatibility with CMOS devices. In contrast, hafnium-based ferroelectric films have attracted widespread attention from industry and academia due to their advantages such as good ferroelectricity at the nanoscale and full compatibility with semiconductor processes. However, compared with traditional ferroelectric materials (~0.1-0.2MV / cm), the coercive field of hafnium-based ferroelectric films is larger (~1.0-2.0MV / cm), and a larger voltage is required to complete polarization reversal, resulting in more charge injection and more defect generation, causing a series of reliability problems such as device fatigue and breakdown. In addition, the high coercive field of hafnium-based ferroelectric films is very close to their breakdown electric field, further increasing the risk of device failure. Therefore, how to reduce the coercive field of hafnium-based ferroelectric films is the key to improving the performance of hafnium-based ferroelectric devices.
[0003] Doping is an effective means of material modification. Common control methods include doping type and doping concentration. Zr doped HfO2 ferroelectric film can appropriately reduce the crystallization temperature, and when the ratio of Hf and Zr is equal, Hf 0.5 Zr 0.5 When O2(HZO) is added, the residual polarization intensity of the hafnium-based ferroelectric film HZO reaches the maximum. In the prior art, the coercive field of HZO is still relatively large (~1.4MV / cm), which is not conducive to improving the reliability of the device. In addition, the coercive field of Si-doped hafnium-based ferroelectric films can be reduced to 1.0MV / cm. Recently, trivalent doping such as Y and La can reduce the coercive field of hafnium-based ferroelectric films to 0.75MV / cm. Even so, compared with traditional perovskite-type ferroelectric materials, the coercive field of hafnium-based ferroelectric films under doping regulation is still relatively large. How to truly and effectively reduce the coercive field of hafnium-based ferroelectric films still needs to be explored. It is urgent to find a more effective and controllable doping method to reduce the coercive field of hafnium-based ferroelectric films, improve the reliability of hafnium-based ferroelectric devices, and enable hafnium-based ferroelectric films to play the ferroelectric advantages at the nanoscale to meet the requirements of low power consumption and high-performance ferroelectric memory devices.
[0004] In fact, in addition to the doping type and doping concentration, the doping configuration is a very important and often overlooked key factor. The doping configuration includes substitution doping and interstitial doping. Studies have found that some doping elements tend to exist in interstitial states, and some doping elements tend to exist in substitution states. Based on this, the present invention provides a doping method for regulating the coercive field of hafnium oxide-based ferroelectric thin films to solve the problems existing in the prior art and meet the needs of different application scenarios. Summary of the invention
[0005] The purpose of the present invention is to provide a doping modification method for a hafnium oxide-based ferroelectric film, which can realize more alternative doping in the main material hafnium oxide-based ferroelectric film system, realize precise adjustable and controllable coercive field, obtain a hafnium oxide-based ferroelectric film with a low coercive field, and improve the reliability of the hafnium oxide-based ferroelectric film.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] The present invention provides a doping modification method for a hafnium oxide-based ferroelectric film, wherein the hafnium oxide-based ferroelectric film is used as a skeleton material, doped by atomic layer deposition technology, and then rapidly thermally annealed in N2 to form a ferroelectric orthorhombic phase; wherein:
[0008] The hafnium oxide-based ferroelectric film is a Zr-doped HfO2 ferroelectric film with a structural formula of Hf x Zr 1-x O2, where 0<x<1;
[0009] The doping element is selected from one or a combination of two or more of Group IIA elements, Group IIIB elements or Group IIIA elements.
[0010] Preferably, the thickness of the hafnium oxide-based ferroelectric thin film is 6-20 nm.
[0011] Preferably, the doping concentration of the doping element is 2%-8%.
[0012] Preferably, the doping element is selected from one or a combination of two or more of Ca, Sr, Sc, Y, La, Al, Ga and In.
[0013] Preferably, the annealing temperature is 400-800°C.
[0014] More preferably, the structural formula of the hafnium oxide-based ferroelectric thin film is Hf 0.5 Zr 0.5 O2, the doping element is La, and the annealing temperature is 450-550℃.
[0015] More preferably, the structural formula of the hafnium oxide-based ferroelectric thin film is Hf 0.5 Zr 0.5O2, doping element is Sr, annealing temperature is 400-550℃.
[0016] More preferably, the structural formula of the hafnium oxide-based ferroelectric thin film is Hf 0.5 Zr 0.5 O2, the doping element is Al, and the annealing temperature is 550-750℃.
[0017] Preferably, the doping modification method of the hafnium oxide-based ferroelectric thin film comprises the following steps:
[0018] (1) Cleaning the Si substrate covered with SiO2 to remove surface debris;
[0019] (2) Atomic layer deposition technology is used to grow a TiN or W electrode with a thickness of 40-60 nm on a cleaned Si substrate at a growth temperature of 260-300° C. During the atomic layer deposition (ALD) growth process, Hf source and Zr source are alternately deposited in sequence, and the number of cycles of deposition of the doping element source is controlled during the deposition process to control the doping concentration for doping modification, thereby obtaining a doped-modified HZO ferroelectric film;
[0020] (3) depositing TiN or W with a thickness of 40-60 nm as a top electrode on the doped modified HZO ferroelectric film, performing photolithography patterning, and then rapidly thermally annealing in N2 for 20-40s at an annealing temperature of 400-800°C to form a ferroelectric orthorhombic phase.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1) In the hafnium-based ferroelectric thin film system, it is found through first-principles calculation that due to the different interactions between the doping elements and the surrounding oxygen atoms in the substitutional or interstitial state, the polarization reversal barrier is significantly different, and the ferroelectric film exhibits different coercive fields. The present invention uses doping elements that tend to form substitutional doping states, which is more conducive to reducing the coercive field of the hafnium-based ferroelectric film.
[0023] 2) Compared with selecting HfO2 film as the main material of the hafnium-based film, the hafnium oxide-based ferroelectric film of the present invention is Hf x Zr 1-x O2 system. In the HfO2 system, substitutional doping involves breaking of old bonds and forming new bonds, but the bond energy of Hf-O is large, so substitutional doping is not easy to achieve. x Zr 1-x O2 system has a smaller bond energy of Zr-O, which makes it easier to form substitution doping and thus reduce the coercive field. Its performance is significantly better than that of HfO2 system doped with doping elements directly. x Zr 1-xDoping in the O2 system can achieve more alternative doping and realize hafnium-based ferroelectric films with lower coercive field. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of doping method in the embodiment, 1 is Hf / Zr atoms, 2 is interstitial doping method, and 3 is substitution doping method.
[0025] Figure 2 Schematic diagram of the calculation results of the formation energy of substitutional doping Al in the HfO2 system and the HZO system in the embodiment, 1 is the substitution of Hf atoms in the HfO2 system, 2 is the substitution of Hf atoms in the HZO system, and 3 is the substitution of Zr atoms in the HZO system.
[0026] Figure 3 Schematic diagram of the calculation results of the effects of different doping methods on the polarization reversal barrier in the La-doped HZO system in the embodiment, 1 is substitutional doping, and 2 is interstitial doping.
[0027] Figure 4 Schematic diagram of the potential barriers that need to be overcome to form substitutional doping in an embodiment. DETAILED DESCRIPTION
[0028] In order to more fully understand and demonstrate the technical solutions, purposes and advantages of the present invention, the technical effects produced by the present invention are further described in detail and completely in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all. It should be pointed out that for those of ordinary skill in the art, other embodiments obtained without departing from the concept of the present invention all belong to the protection scope of the present invention.
[0029] The calculation method used in the following embodiments is a first-principle calculation based on density functional theory, and the calculation software package is the PWMAT calculation software package, but is not limited thereto, and may also be, for example, VASP, CASTEP, Gaussian, or Wien2k. The PWMAT software package provides pseudopotential files for most elements in the periodic table, uses GPU acceleration, has high calculation efficiency, and is highly practical.
[0030] Example 1
[0031] This embodiment prepares a hafnium oxide-based ferroelectric capacitor device, using a HZO ferroelectric film as a skeleton, the doping element is La, and the annealing temperature is 450-550° C. The specific method is as follows:
[0032] (1) Clean the Si substrate covered with SiO2 to remove surface impurities.
[0033] (2) Atomic layer deposition technology is used to grow TiN or W electrodes with a thickness of about 50 nm on a Si substrate at a growth temperature of 280°C. During the ALD growth process, Hf source and Zr source are alternately deposited in sequence. During the deposition process, the doping concentration is controlled by adjusting the number of cycles of the doping element La source deposition to form a doped HZO ferroelectric film.
[0034] (3) Depositing about 50 nm of TiN or W as a top electrode on the doped HZO ferroelectric film, and performing photolithography patterning, and rapidly thermal annealing in N2 for 30 seconds to form a ferroelectric orthorhombic phase.
[0035] Example 2
[0036] This embodiment prepares a hafnium oxide-based ferroelectric capacitor device, using HZO ferroelectric film as the skeleton, the doping element is Sr, and the annealing temperature is 400-550° C. The specific method is as follows:
[0037] (1) Clean the Si substrate covered with SiO2 to remove surface impurities.
[0038] (2) Atomic layer deposition technology is used to grow TiN or W electrodes with a thickness of about 50 nm on a Si substrate at a growth temperature of 280°C. During the ALD growth process, Hf source and Zr source are alternately deposited in sequence. During the deposition process, the doping concentration is controlled by adjusting the number of cycles of the doping element Sr source deposition to form a doped HZO ferroelectric film.
[0039] (3) Depositing about 50 nm of TiN or W as a top electrode on the doped HZO ferroelectric film, and performing photolithography patterning, and rapidly thermal annealing in N2 for 30 seconds to form a ferroelectric orthorhombic phase.
[0040] Example 3
[0041] This embodiment prepares a hafnium oxide-based ferroelectric capacitor device, using a HZO ferroelectric film as a skeleton, with Al as the doping element, and an annealing temperature of 550-750° C. The specific method is as follows:
[0042] (1) Clean the Si substrate covered with SiO2 to remove surface impurities.
[0043] (2) Atomic layer deposition technology is used to grow TiN or W electrodes with a thickness of about 50 nm on a Si substrate at a growth temperature of 280°C. During the ALD growth process, Hf source and Zr source are deposited alternately in sequence. During the deposition process, the doping concentration is controlled by adjusting the number of cycles of the doping element Al source deposition to form a doped HZO ferroelectric film.
[0044] (3) Depositing about 50 nm of TiN or W as a top electrode on the doped HZO ferroelectric film, and performing photolithography patterning, and rapidly thermal annealing in N2 for 30 seconds to form a ferroelectric orthorhombic phase.
[0045] like Figure 1-4 As shown in the figure, by comparing the bond energies of Hf-O and Zr-O, it is found that the bond energy of Zr-O is lower, which means that compared with the HfO2 system, it is easier to achieve substitution doping by doping on the basis of the HZO main film. The present invention uses the HZO ferroelectric film as the skeleton to perform doping regulation. By calculating the polarization reversal barrier under substitution doping and gap doping, it is found that the coercive field under substitution doping is significantly reduced. x Zr 1-x Doping in the O2 system achieves more substitution doping, thereby achieving hafnium oxide-based ferroelectric films with lower coercive fields. In addition, since each doping element has different potential barriers to overcome to form a substitution form, and substitution doping involves breaking old bonds and forming new bonds, a low annealing temperature is used for doping elements with lower potential barriers, and a higher annealing temperature is used for doping elements with higher potential barriers to achieve substitution doping. Regulating the annealing temperature is an effective way to change the doping method.
[0046] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A doping modification method for a hafnium oxide-based ferroelectric thin film, characterized in that: The hafnium oxide-based ferroelectric film is used as the skeleton material, and the doping elements are deposited by atomic layer deposition for doping modification, and the ferroelectric orthorhombic phase is formed by rapid thermal annealing in N2; wherein: The hafnium oxide-based ferroelectric film is a Zr-doped HfO2 ferroelectric film with a structural formula of Hf x Zr 1-x O2, where 0<x<1; The doping element is selected from one or a combination of two or more of Group IIA elements, Group IIIB elements or Group IIIA elements.
2. The doping modification method of the hafnium oxide-based ferroelectric thin film according to claim 1, characterized in that: The thickness of the hafnium oxide-based ferroelectric film is 6-20 nm.
3. The doping modification method of the hafnium oxide-based ferroelectric thin film according to claim 1, characterized in that: The doping concentration of the doping element is 2%-8%.
4. The doping modification method of the hafnium oxide-based ferroelectric thin film according to claim 1, characterized in that: The doping element is selected from one or a combination of two or more of Ca, Sr, Sc, Y, La, Al, Ga and In.
5. The doping modification method of the hafnium oxide-based ferroelectric thin film according to claim 1, characterized in that: The annealing temperature is 400-800°C.
6. The doping modification method of the hafnium oxide-based ferroelectric thin film according to claim 1, characterized in that: The structural formula of the hafnium oxide-based ferroelectric film is Hf 0.5 Zr 0.5 O2, the doping element is La, and the annealing temperature is 450-550℃.
7. The doping modification method of the hafnium oxide-based ferroelectric thin film according to claim 1, characterized in that: The structural formula of the hafnium oxide-based ferroelectric film is Hf 0.5 Zr 0.5 O2, doping element is Sr, annealing temperature is 400-550℃.
8. The doping modification method of the hafnium oxide-based ferroelectric thin film according to claim 1, characterized in that: The structural formula of the hafnium oxide-based ferroelectric film is Hf 0.5 Zr 0.5 O2, the doping element is Al, and the annealing temperature is 550-750℃.
9. The doping modification method of the hafnium oxide-based ferroelectric thin film according to any one of claims 1 to 8, characterized in that: Using HZO ferroelectric thin film as the skeleton material, the method includes the following steps: (1) Cleaning the Si substrate covered with SiO2 to remove surface debris; (2) Atomic layer deposition technology is used to grow a TiN or W electrode with a thickness of 40-60 nm on a cleaned Si substrate at a growth temperature of 260-300° C. During the ALD growth process, Hf source and Zr source are alternately deposited in sequence. At the same time, during the deposition process, the number of cycles of the doping element source deposition is regulated to control the doping concentration for doping modification, thereby obtaining a doped-modified HZO ferroelectric film; (3) depositing TiN or W with a thickness of 40-60 nm as a top electrode on the doped modified HZO ferroelectric film, performing photolithography patterning, and then rapidly thermally annealing in N2 for 20-40s at an annealing temperature of 400-800°C to form a ferroelectric orthorhombic phase.
Citation Information
Cited By
Doped hafnium oxide-based ferroelectric film based on doping distribution regulation and control and preparation method and application of doped hafnium oxide-based ferroelectric film
CN119615117A
Electrode-free constrained annealing hafnium oxide-based ferroelectric film and preparation method and application thereof
CN119615118A