Improved carbonaceous coating materials for battery electrode materials

By using petroleum-derived asphalt products, and preparing asphalt products with specific characteristics through vacuum distillation, the problem of uneven distribution of carbon coatings on lithium-ion battery electrodes is solved, and high efficiency, safety and environmentally friendly battery electrodes are achieved coating.

CN118984806APending Publication Date: 2024-11-19RAIN CARBON BV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280091101.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2021-12-13
Filing Date
2022-12-13
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The uneven distribution of existing carbon coatings on lithium-ion battery electrode materials leads to a decrease in the electrochemically active surface area. Asphalt derived from coal tar contains harmful impurities and carcinogens, affecting battery safety and environmental feasibility.

Method used

Using petroleum-derived asphalt products, the vacuum distillation process prepares asphalt products with specific melt viscosity and softening points, forming a thin and uniform carbon coating, suitable for lithium-ion battery electrodes, reducing the content of metal impurities and polycyclic aromatic hydrocarbons. Improve the quality and environmental friendliness of the coating.

Benefits of technology

The formation of a uniform thin coating on the lithium-ion battery electrode is achieved, which improves electrochemical performance and safety, reduces health and environment hazards, and provides a more efficient and reliable battery manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004981077830000081
    Figure BDA0004981077830000081
  • Figure BDA0004981077830000091
    Figure BDA0004981077830000091
  • Figure BDA0004981077830000101
    Figure BDA0004981077830000101
Patent Text Reader

Abstract

The invention relates to a coating material for coating primary particles, said coating material comprising a petroleum-derived asphalt product, characterized in that said asphalt product has a melt viscosity index log10 (visc) * 100 / SPM of between 1.2 and 3.0 at 220 DEG C and of between 1.0 and 2.5 at 240 DEG C, where visc = melt viscosity (mPa.s) and SPM = Mettler softening point (DEG C). The invention also relates to the use of said coating material for coating primary particles of an electrode material in the manufacture of battery electrodes, more particularly Li-ion batteries. Further, the present invention relates to a battery electrode comprising a coating made of said coating material, and to a battery comprising an electrode having a coating made of said coating material. Furthermore, the present invention relates to a process for obtaining a petroleum-derived asphalt product as mentioned above, said process comprising a petroleum vacuum distillation process step for obtaining a petroleum-derived distillation residue. Further, the invention relates to a method for manufacturing a battery electrode, comprising said method for producing an asphalt product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to a coating material for coating primary particles, the coating material comprising a petroleum-derived bitumen product.

[0002] Further, the present invention relates to the use of the coating material to coat a carbon surface layer on primary particles of electrode materials like graphite, silicon, silicon oxides or carbonaceous particles and composites thereof. These carbon-coated electrode materials can be used to manufacture battery electrodes, more specifically Li-ion batteries.

[0003] Furthermore, the invention relates to a battery electrode comprising an electrode material having a particle coating made of such a coating material. Background Art

[0004] Commercially available negative electrode materials for lithium-ion batteries are conventionally based on graphite, but are also increasingly based on silicon oxides, metallic silicon, silicon alloys, and composites of carbon or graphite with materials based on silicon, tin, etc.

[0005] Many of these negative electrode materials are coated with carbon coating materials using coal tar and petroleum-based pitch as precursors. Many processes are known to obtain suitable coatings. Typically, the coating is applied to the surface of the electrode material particles in a wet process by dissolving the pitch in an organic solvent or dispersing the finely ground pitch powder in water, mixing the solution or suspension with the particles and drying the mixture, and then heat treating it in an inert gas atmosphere at a high temperature of 600°C-1300°C. In addition, a dry coating process is used, in which finely ground pitch is mixed with electrode material particles. The mixture is then heated in an inert gas atmosphere to melt the pitch and form a surface carbon layer, which is eventually carbonized at high temperature and (if necessary) graphitized.

[0006] A first problem known in the art is that conventional carbon coatings are not always evenly distributed on the surface of the electrode particles, so that a relatively high amount (i.e., a relatively thick carbon film) is required to completely cover the particle surface required to reduce the BET surface area, the electrochemically active surface area wetted by the battery electrolyte, and the reactivity of the electrode material to the electrolyte. Low surface area carbon coatings improve the electrochemical parameters of carbon particles by reducing charge losses, improving battery safety and charge / discharge cycle stability. However, since the carbon formed at the particle surface contributes less to the reversible capacity of the electrode material than the particle core, and since the thickness of the carbon layer also affects the insertion rate of lithium ions into the body, thinner coatings are preferred.

[0007] The second problem is that typical asphalts derived from coal tar and petrochemical sources contain not only small carbon particles, but also metallic impurities that are harmful to the quality of the formed coating. These particulate impurities are usually measured as quinoline insoluble matter (QI content), which is an indicator of asphalt quality. In order to obtain good carbon film quality, the QI content should be low. In addition, some metallic particulate impurities like iron, copper and zinc can cause safety issues in lithium-ion batteries. The insoluble components reflected by the QI and TI values ​​are particularly unfavorable for wet coating processes, in which the asphalt is dissolved in an organic solvent like THF, toluene, xylene or hexane before being mixed into the substrate to be coated. The specific requirements for QI and TI of the coating material are related to the wet coating process.

[0008] The third problem is that the typical surface coating process based on coating the electrode particles with coal tar pitch in a dry or wet mixing process and subsequent carbonization at high temperature in an inert gas atmosphere results in a hydrophobic particle surface. This hydrophobicity leads to additional problems with the use of binders in water-based electrode manufacturing processes. To address this problem, EP3177651 (A1) proposes a non-graphite carbon coating and subsequent oxidation.

[0009] Another problem with coal tar pitch in particular is that it contains some polycyclic aromatic hydrocarbons (PAHs) that are carcinogenic and harmful to health and the environment, such as benzo[a]pyrene (B[a]P).

[0010] Furthermore, with the change in steel production away from the use of blast furnaces to reduce greenhouse gas emissions, the availability of coal tar as a raw material for coal tar pitch will significantly decrease in the future, and therefore the availability of high quality coal tar will also significantly decrease.

[0011] In view of the above, it is an object of the present invention to provide a coating material for coating primary particles, the material comprising a bituminous product having suitable characteristics for producing a thin coating, typically tens of nanometers thick.

[0012] Further, it is an object of the present invention to use a coating material for coating primary particles for the manufacture of battery electrodes, said coating material having suitable characteristics for producing a thin coating layer, typically a few tens of nanometers thick.

[0013] Without being bound by any theory, a thin uniform coating is expected, wherein the coating material shows good wetting and impregnation properties of the particle surface. This can be adjusted by the composition of the bitumen and the appropriate viscosity in the molten state.

[0014] Another object of the present invention is to use the asphalt product as a coating material which improves the quality of the carbon coating formed at the surface of primary particles for manufacturing battery electrodes.

[0015] Another object is to provide a pitch-based carbon coating suitable for water-based electrode manufacturing processes.

[0016] Another objective is to reduce safety issues and specific charge loss in lithium-ion batteries and to improve charge / discharge cycle stability.

[0017] Furthermore, it is a general object of the present invention to provide an alternative to coatings based on coal tar pitch which allows increased supply security and meets the necessary requirements for use as hydrocarbon coating material in the manufacture of battery electrodes, in particular Li-ion batteries.

[0018] Another general object of the present invention is to provide an alternative asphalt-based coating that yields similar coke values ​​and softening points, as well as similar processing and performance for battery electrodes, particularly Li-ion batteries.

[0019] Another general object of the present invention is to provide a more environmentally friendly alternative to coal tar pitch based coatings. Summary of the invention

[0020] In a first aspect, the present invention provides a coating material for coating primary particles, the material comprising a petroleum-derived bitumen product, characterised in that the bitumen product has a melt viscosity index log between 1.2 and 3.0 at 220°C and between 1.0 and 2.5 at 240°C. 10 (visc)*100 / SPM, where visc = melt viscosity (mPa.s) and SPM = Mettler softening point (in °C).

[0021] In particular, the invention provides for the use of the coating material for coating primary particles for producing electrodes, and in particular battery electrodes.

[0022] In a second aspect according to the present invention, there is provided a battery electrode comprising a coating made of the asphalt product.

[0023] In a third aspect according to the present invention, there is provided a battery comprising an electrode having a coating made of the asphalt product.

[0024] In a fourth aspect according to the present invention, there is provided a method for obtaining a petroleum-derived bitumen product for use as mentioned in the first aspect, the method comprising a petroleum vacuum distillation process step for obtaining a petroleum-derived distillation residue.

[0025] In accordance with a fifth aspect of the present invention, there is provided a method for manufacturing a battery electrode, the method comprising the method for producing an asphalt product. DETAILED DESCRIPTION

[0026] In a first aspect, the present invention provides a coating material for coating primary particles, the material comprising a petroleum-derived bitumen product as coating material for primary particles, characterised in that the bitumen product has a melt viscosity index log between 1.2 and 3.0 at 220° C. and between 1.0 and 2.5 at 240° C. 10 (visc)*100 / SPM, where visc = melt viscosity (mPa.s) and SPM = Mettler softening point (°C).

[0027] In the context of the present invention, primary particles include particles of carbon, graphite, silicon, metallic silicon, silicon alloys, silicon oxides, metals, carbonaceous particles and composite materials, or any combination thereof, or any type of primary particles suitable for making battery electrode materials.

[0028] More preferably, the bitumen product has a melt viscosity index log between 1.8 and 2.5 at 220°C and between 1.5 and 2.1 at 240°C. 10 (visc)*100 / SPM, where visc = melt viscosity (mPa.s) and SPM = Mettler softening point (°C).

[0029] Even more preferably, the bitumen product has a melt viscosity index log between 2.0 and 2.5 at 220°C and between 1.7 and 2.1 at 240°C. 10 (visc)*100 / SPM, where visc = melt viscosity (mPa.s) and SPM = Mettler softening point (°C).

[0030] Using this coating material as a carbon precursor product to form a thin and uniform carbon coating at the surface of the electrode material particles with a low precursor amount is very important in the manufacture of battery electrodes, especially negative electrodes of lithium ion batteries.

[0031] In one embodiment of the present invention, the asphalt product as contained in the coating material has a melt viscosity between 100 and 500, preferably between 150 and 400 mPa.s at 220°C, and between 50 and 200, preferably between 75 and 150 mPa.s at 240°C, and has a SPM between 110°C and 130°C.

[0032] In another embodiment of the present invention, the asphalt product as included in the coating material has a melt viscosity between 500 and 5000, preferably between 1000 and 3000 mPa.s at 220°C, and between 100 and 1000, preferably between 400 and 900 mPa.s at 240°C, and has a SPM between 140°C and 160°C.

[0033] In yet another embodiment of the present invention, the asphalt product as contained in the coating material has a melt viscosity at 220°C between 5000 and 50000, preferably between 10000 and 35000 mPa.s, and between 500 and 10000, preferably between 2000 and 7000 mPa.s at 240°C, and has a SPM between 170°C and 190°C.

[0034] The adjusted melt viscosity enhances the wetting and impregnation of the particle surface, resulting in a uniformly distributed carbon film at the particle surface. The enhanced surface wetting and impregnation results in good coverage of the geometric particle surface, but also of the micropores and mesopores and roughness typically found at the particle surface.

[0035] The use as described throughout this text is provided as an alternative to the use of coal tar pitch based coatings for battery electrodes, meeting the requirements of the battery manufacturing industry and having the advantage of sufficient availability.

[0036] In one embodiment of the present invention, the petroleum-derived asphalt product contained in the coating material may contain asphaltene at a concentration of at least 70%, at least 75%, or at least 80%, as measured by the SARA method (clay-gel absorption chromatography according to ASTM D2007), so that the coke value is increased, respectively. The asphalt product ensures a dense (low porosity) uniform carbon coating on the surface of the electrode material, thereby reducing the surface reactivity to the electrolyte and the surface area of ​​the electrode material in direct contact with the battery electrolyte, and further ensures good conductivity and particle contact of the electrode material in the battery cell electrode.

[0037] In one embodiment according to the present invention, the asphalt product included in the coating material may have a resin content (SARA) lower than 20%, which may contribute to its high coke yield.

[0038] In another embodiment according to the present invention, the asphalt product contained in the coating material may have a B(a)P content of less than 5000 ppm, or even less than 3000 ppm, or even less than 2000 ppm and / or a sum of 16 EPA-PAHs (polycyclic aromatic hydrocarbons according to the U.S. Environmental Protection Agency (EPA)) of less than 7% or even less than 5% by weight. Compared with pure coal tar derived asphalt products, sufficiently low B(a)P content and / or the sum of 16 EPA-PAHs obviously result in improved environmental friendliness.

[0039] In another embodiment, the asphalt product contained in the coating material can have a coke yield of at least 35% Alcan, or at least 45% Alcan, or at least 50% Alcan, or at least 55% Alcan at a Mettler softening point between 110°C and 185°C. When the coating material is converted into carbon during the carbonization process, a sufficiently high coke yield allows the high porosity in the resulting graphite particles to be avoided due to the less volatiles formed during the carbonization process. Subsequent treatment in air at a temperature of 400°C-1000°C in a fluidized bed or rotary kiln can be used to increase the hydrophilicity of the carbon surface, thereby improving the processing of carbon-coated electrode materials in water-based electrode manufacturing processes. A dense carbon layer having such a morphology can be formed that is conducive to the formation of an efficient solid electrolyte interface at the surface of the electrode particles. In addition, in addition to the electrochemically active electrode surface area in direct contact with the electrolyte of the battery cell, the properties and quality of the carbon film formed at the surface of the particles also affect the charge loss.

[0040] In further embodiments, the bituminous product comprised in the coating material may have a flash point of at least 200°C, preferably at least 220°C, thereby allowing the bituminous product to be processed according to safety requirements as may be required during hot mixing.

[0041] In an embodiment of the present invention, the bitumen product contained in the coating material may have a Mettler softening point between 110° C. and 190° C., which is a target range in the manufacture of battery electrodes.

[0042] According to the present invention, the asphalt product contained in the coating material may have a quinoline insoluble content range of less than 1% by weight and / or a toluene insoluble content of less than 40%, or less than 20% by weight. Preferably, the asphalt product may have a quinoline insoluble content range of less than 1% by weight and a toluene insoluble content of less than 5% by weight, which may improve its suitability as a coating material for primary particles in a solvent-based coating process, because a lower toluene insoluble content improves solubility.

[0043] In a preferred embodiment according to the present invention, the asphalt product contained in the coating material can have a melt viscosity between 500 and 50000 mPa.s at 220°C, a coke yield between 35% and 70% Alcan, and a quinoline insoluble content range of less than 1% by weight.

[0044] According to the invention, the coating material may comprise, in addition to the bituminous product, other petroleum-derived or coal-tar-derived components.

[0045] In a particular embodiment, the coating material may consist solely of an asphalt product.

[0046] In a particular embodiment, the coating material of the present invention consists solely of petroleum-derived components, ie, does not contain any coal tar-derived components.

[0047] In a particular embodiment, the asphalt product included in the coating material consists solely of petroleum-derived components.

[0048] In a particular embodiment, the bitumen product included in the coating material consists of a petroleum-derived distillation residue.

[0049] In another specific embodiment, the asphalt product included in the coating material does not contain any coal tar derived components.

[0050] According to a second aspect of the present invention, there is provided a battery electrode comprising a coating made of the asphalt product. 2 / g BET SSA and 15 microns average particle size of spherical natural graphite, such a coating can reduce the BET surface area by at least 40% at 5wt.% of pitch. Coated natural graphite (BET3m 2 / g) can be increased to more than 90%.

[0051] In a third aspect according to the present invention, there is provided a battery comprising an electrode having a coating made of the coating material. In particular, the performance of the lithium-ion battery can be positively affected, i.e., low specific charge loss and high coulombic efficiency, good energy and power density and specific energy and power, and cycle stability of the battery.

[0052] In a fourth aspect according to the present invention, a method for obtaining a petroleum-derived asphalt contained in a coating material as in the present invention comprises a petroleum vacuum distillation process step for obtaining a petroleum-derived distillation residue.

[0053] The benefit of the method according to the invention is that it may allow the amount of asphaltenes measured by SARA to be maintained at similar levels compared to known coal tar based battery electrode coating precursors. Furthermore, other asphalt properties may not be degraded compared to known coal tar coating precursors.

[0054] An additional benefit is that this method can maintain the coke value of the asphalt product at a high level, such as at least 40% ALCAN, at a target softening point (eg, Mettler softening point of 110°C-190°C).

[0055] In contrast to the production of asphalt products by the process according to the invention, conventional coal tar pitch coating precursors are produced by distillation at ambient pressure and higher temperatures, followed in some cases by air blowing. The disadvantages of these products caused by ambient pressure distillation are the high mesophase and toluene insoluble content caused by the high processing temperatures that lead to cracking and mesophase formation. Other disadvantages are low coke yield, high volatile content, high viscosity (which deteriorates the impregnation and adhesive properties of the pitch and processing), and low flash point (which can cause safety problems during electrode manufacturing).

[0056] An additional disadvantage of distillation at ambient pressure is that, due to the reactive nature of the distillation of petroleum tar, the temperatures required for distillation at atmospheric pressure already initiate conversion to solid carbon components in the heating chamber and tower, which can lead to excessively high fouling rates during bitumen production, resulting in equipment reliability problems.

[0057] In an embodiment of the present invention, the distillation process step is carried out at a vacuum level between 0.1 and 400 mbar, preferably between 0.1 and 250 mbar, and at a temperature between 200°C and 400°C, preferably between 280°C and 370°C.

[0058] The process according to the invention allows strict control and prevention of potential mesophase formation due to low secondary quinoline insolubles content in the bitumen, resulting in a thin uniform coating at the particle surface.

[0059] Furthermore, the process according to the invention provides a high reliability level by reaching the desired softening point and viscosity of the bitumen product at lower temperatures compared to conventional ambient pressure distillation and thus results in better equipment reliability. The lower distillation temperatures used in the vacuum distillation process avoid degradation reactions like mesophase and coke formation that lead to equipment fouling and scheduled shutdowns.

[0060] Furthermore, the method of the present invention can obtain a high-quality and reliable asphalt product for battery electrodes, which shows a sufficiently high coking value and a low 16-item EPA PAH content at a low viscosity. The 16-item EPA PAH level of the resulting binder is lower than that of pure coal tar-derived products, thereby producing a more environmentally friendly material. Examples 1-6:

[0061] Table 1 below shows examples of petroleum-derived asphalt products and properties contained in coating materials according to embodiments of the present invention. Table 1

[0062] Table 2 further illustrates the properties of the coated natural graphite material obtained by coating with a coating material consisting of the bitumen products of Examples 3 and 4 and subsequently carbonizing at 1100°C: Table 2:

[0063] The following table provides an overview of the analytical procedures for the product parameters as used in this text:

[0064] Example 7: -Preparation of coated natural graphite samples: Spherical natural graphite was mixed with asphalt powder obtained from a petroleum-derived asphalt product as described throughout this text in an intensive mixer at room temperature for 5 min and ground to an average particle size of about 3-5 μm. The mixture was heat treated at 1100° C. in a nitrogen atmosphere at a heating rate of 100° C. / h for 5 h. -Electrochemical testing of carbon-coated natural graphite materials: The graphite sample was dispersed in a solution of carboxymethyl cellulose (CMC) in water, and then an SBR latex binder material was added to obtain a final composition of 96wt.% graphite, 2wt.% CMC, and 2wt.% SBR. The aqueous slurry was deposited on a copper foil by a doctor blade method, and the resulting coated foil was dried at 120°C. The dried sheet was rolled, and then a final electrode with a diameter of 17mm was punched out of the sheet. A copper foil with a diameter of approximately 8.5mg / cm 2 The mass loading is about 1.65 g / cm 3Electrodes with a density of 100 μm and a thickness of about 70 μm were dried in vacuum at 100°C and tested in lithium coin half-cells using 1M LiPF6 EC / DEC (1:1 by weight) electrolyte and porous polypropylene separator. The first cycle coulombic efficiency and reversible specific charge of the electrode were measured by discharging the half-cell to 5 mV at 0.1C relative to Li / Li+ and holding the cell at this potential until the current dropped to 0.7 mA, and then charging the cell to 1.5 V relative to Li / Li+ and holding it at this potential until the cell current dropped to 0.7 mA. The coulombic efficiency of the first charge / discharge cycle is calculated by reversible specific charge / (reversible specific charge+irreversible specific charge)=measured mAh (1st cycle charge) / measured mAh (1st cycle discharge) (in percentage).

Claims

1. A coating material for coating primary particles, the coating material comprising a petroleum-derived bitumen product, characterized in that The bitumen product has a melt viscosity index log between 1.2 and 3.0 at 220°C and between 1.0 and 2.5 at 240°C. 10 (visc)*100 / SPM, where visc = melt viscosity (in mPa.s) and SPM = Mettler softening point (in °C).

2. The coating material according to claim 1, wherein The bitumen product has a melt viscosity between 100 and 500 mPa.s at 220°C and between 50 and 200 mPa.s at 240°C, while having a SPM between 110°C and 130°C.

3. The coating material according to claim 1, wherein The bitumen product has a melt viscosity between 500 and 5000 mPa.s at 220°C and between 100 and 1000 mPa.s at 240°C, while having a SPM between 140°C and 160°C.

4. The coating material according to claim 1, wherein The bitumen product has a melt viscosity between 5000 and 50000 mPa.s at 220°C and between 500 and 10000 at 240°C, while having a SPM between 170°C and 190°C.

5. The coating material according to claim 1, wherein The asphalt product has a coke yield of at least 35% Alcan.

6. The coating material according to claim 1, wherein The asphalt product has a quinoline insoluble content range of less than 1% by weight and / or a toluene insoluble content range of less than 40% by weight.

7. The coating material according to claim 1, wherein The pitch product has a coke yield between 35% and 70% Alcan, and a quinoline insoluble content range of less than 1% by weight.

8. A coating material according to any one of the preceding claims, wherein: The bitumen product has a resin content (SARA) below 20%.

9. A coating material according to any one of the preceding claims, wherein: The asphalt product has a B(a)P content of less than 5000 ppm and / or a sum of 16 EPA-PAHs of less than 7% by weight.

10. A coating material according to any one of the preceding claims, wherein: The bitumen products consist of distillation residues derived from petroleum.

11. Use of a coating material according to any one of the preceding claims for coating primary particles for producing battery electrodes.

12. The method according to claim 11, for coating and / or binding particles of electrode material for negative electrodes of lithium-ion batteries.

13. Use according to claim 11 or 12 in a solvent-based coating process, wherein: The asphalt has a quinoline insoluble content range of less than 1% by weight and a toluene insoluble content range of less than 5% by weight.

14. A battery electrode comprising an electrode material having a coating of particles made from a bituminous product as used in any one of the preceding claims.

15. A lithium ion battery comprising the electrode according to claim 14.

16. A method for obtaining a petroleum derived bitumen product as contained in a coating material according to claims 1 to 10, said method comprising a petroleum vacuum distillation process step for obtaining a petroleum derived distillation residue.

17. The method according to claim 16, wherein: The distillation process step is carried out at a vacuum level between 0.1 and 250 mbar and at a temperature between 200°C and 370°C.

18. A method for producing a battery electrode, the method comprising the method according to claims 16 to 17.

Citation Information

Patent Citations

  • Hydrophilic surface-modified carbonaceous particulate material

    EP3177651A1

  • Highly aromatic petroleum pitches, their preparation and use in the manufacture of electrodes

    EP1130077A2

  • Negative electrode material for high performance lithium ion secondary battery and its manufacturing method

    JP2004047350A