Preparation method of CO catalyst, coating equipment and application

By designing the initial dry embryo module, configuring palladium salt solution and adjusting equipment parameters in the CO catalyst preparation method, combined with the introduction of WO3 and V2O5, the problems of high cost and poor stability of traditional CO catalysts in steel sintering machines are solved, and high efficiency is achieved , stable catalyst preparation and coating meets the requirements of strict working conditions.

CN118988305APending Publication Date: 2024-11-22CECEP LIUHE TIANRONG (SHANDONG) CATALYST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410977300.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The application of traditional CO catalysts in steel sintering machines has problems such as high cost, poor thermal stability, susceptibility to sulfur poisoning and inaccurate coating process, which leads to insufficient catalyst activity and stability, making it difficult to meet the strict working conditions requirements.

Method used

A CO catalyst preparation method is adopted to optimize the components and process conditions of the catalyst by designing the initial dry embryo module, configuring palladium salt solution, adjusting equipment parameters and carrying out accurate drying and calcining process, combined with the introduction of WO3 and V2O5, and to ensure the high level of the catalyst. Performance and high stability.

Benefits of technology

The high efficiency and performance of the catalyst are achieved, the thermal stability and selectivity of the catalyst are improved, the operating cost is reduced, and the life of the catalyst and the uniformity of the coating are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988305A_ABST
    Figure CN118988305A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coating, and provides a CO catalyst preparation method which comprises the following steps: S1, preparing an initial dry blank module: designing that the content of TiO2 in the initial dry blank module is 60-90%, the content of WO3 is 1-5%, the content of V2O5 is 1-5%, the balance is mainly Al2O3 and SiO2, and the content is 1-10%, preparing raw materials according to the mass percent of each component, mixing all the raw materials, putting the mixture into a mixing mill, and uniformly mixing the raw materials; adding pure water, a forming aid and ammonia water, continuously stirring for 4-5 hours to uniformly mix the raw materials, controlling the water content of the pug to be 28-30% and the pH value to be 7.0-8.0, and filtering, extruding and forming, drying, calcining and cutting the pug to obtain an initial dry blank module; s2, preparing a palladium salt solution, wherein the concentration of the palladium salt solution is 0.1-1%; s3, adjusting the equipment; s4, preparing a precious metal coating; s5, coating is carried out; and S6, drying and calcining. According to the technical scheme, the problem that the activity and the stability of the catalyst are insufficient due to lack of accurate control in the preparation process of the catalyst in related technologies is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of coating technology, and in particular to a CO catalyst preparation method, coating equipment and application. Background Art

[0002] Traditional CO catalysts are usually based on a single precious metal active component, such as platinum (Pt) and palladium (Pd). Although these catalysts have high catalytic activity, they also have problems such as high cost, poor thermal stability, and susceptibility to sulfur poisoning. In addition, the lack of precise control in the preparation process of the catalyst leads to insufficient activity and stability, making it difficult to meet the stringent working conditions required in the steel sintering process.

[0003] The flue gas produced by steel sintering machines has the characteristics of high CO concentration, high temperature, and high dust content, which puts higher requirements on the performance of CO catalysts. The catalyst needs to have good thermal stability, anti-poisoning ability and high catalytic efficiency to adapt to the working conditions of the sintering machine.

[0004] Deficiencies of the existing technology The existing CO catalyst coating process and equipment have some deficiencies in the application of steel sintering machines, mainly manifested in:

[0005] High operating costs: The use of precious metals leads to high catalyst costs, and in the high temperature and dusty environment of the sintering machine, the catalyst life may be short and require frequent replacement.

[0006] Imprecise coating process: Existing coating processes may not guarantee the uniformity and consistency of the catalyst coating, affecting catalytic efficiency. Summary of the invention

[0007] The present invention provides a CO catalyst preparation method, coating equipment and application, which solves the problem that the catalyst preparation process in the related art often lacks precise control, resulting in insufficient activity and stability of the catalyst.

[0008] The technical solution of the present invention is as follows:

[0009] A method for preparing a CO catalyst comprises the following steps:

[0010] S1. Preparation of initial dry embryo module: The TiO2 content, WO3 content, V2O5 content, and balance of Al2O3 and SiO2 in the initial dry embryo module are designed to be 60-90%, 1-5%, and 1-10%, respectively. Raw materials are prepared according to the mass percentage of each component, all raw materials are mixed and put into a mixer, pure water, molding aid, and ammonia water are added, and stirring is continued for 4-5 hours to mix the raw materials evenly, and the moisture content of the mud is controlled at 28-30%, and the pH is 7.0-8.0. The mud is filtered, extruded, dried, calcined, and cut to obtain the initial dry embryo module;

[0011] S2. Prepare palladium salt solution: the concentration of palladium salt solution is 0.1-1%;

[0012] S3, adjusting equipment: adjusting the immersion time of the immersion tank to 15-40min, adjusting the temperature of the immersion tank to 25-50°C, adjusting the drying time of the first drying tank and the second drying tank to 15-30min, and adjusting the drying temperature of the first drying tank and the second drying tank to 55-65°C;

[0013] S4. Precious metal coating: The depth of precious metal coating is 0.1-0.5mm, and the load is 0.2-1kg / m3;

[0014] S5, coating: coating the dry embryo module by the coating equipment;

[0015] S6. Drying and calcining: drying and calcining the coated dry embryo module at a calcination temperature of 380-420° C. for 20-30 hours. After the calcination, a CO catalyst is obtained.

[0016] A CO catalyst coating device, comprising a CO catalyst preparation method according to claim 1, comprising:

[0017] A liquid preparation tank, the liquid preparation tank is used to place the precious metal solution;

[0018] An impregnation tank, the impregnation tank is used to impregnate the CO catalyst module;

[0019] A first pipeline, one end of which is connected to the liquid preparation tank, and the other end of which is connected to the immersion tank;

[0020] A purge slot, the purge slot being used to purge impurities on the CO catalyst module;

[0021] a second pipeline, one end of which is connected to the impregnation tank and the other end of which is connected to the purge tank, wherein the second pipeline is used to return the precious metal solution in the purge tank to the impregnation tank;

[0022] a first drying tank, wherein the first drying tank is used to dry the CO catalyst module;

[0023] a second drying tank, the second drying tank being used to further dry the CO catalyst module;

[0024] a fourth pipeline, one end of which is connected to the impregnation tank, and the other end of which is connected to the first drying tank;

[0025] a fifth pipeline, one end of which is connected to the impregnation tank and the other end of which is connected to the second drying tank, wherein the fifth pipeline and the fourth pipeline are used to return the precious metal solution in the first drying tank and the second drying tank to the impregnation tank;

[0026] a storage tank for storing excess precious metal solution;

[0027] The sixth pipeline is connected to the storage tank at one end and to the liquid distribution tank at the other end. When the liquid level of the liquid distribution tank is higher than that of the storage tank, the sixth pipeline is used to flow the precious metal solution in the liquid distribution tank to the storage tank by gravity.

[0028] Optionally, also include:

[0029] Water tank, used to provide water source;

[0030] A water pump, one end of which is connected to the water tank and the other end of which is connected to the liquid distribution tank, and the water pump is used to pump water in the water tank into the liquid distribution tank;

[0031] A liquid pump is arranged on the sixth pipeline, and is used to extract the precious metal solution in the storage tank into the liquid preparation tank.

[0032] Optionally, also include:

[0033] a seventh pipeline, one end of which is connected to the fourth pipeline, and the other end of which is connected to the storage tank;

[0034] an eighth pipeline, one end of which is connected to the fifth pipeline, and the other end of which is connected to the storage tank;

[0035] A fourth control valve, disposed on the fourth pipeline, for controlling whether the fourth pipeline is connected to the first drying tank or not;

[0036] The fifth control valve is arranged on the fifth pipeline and is used to control whether the fifth pipeline is connected to the second drying tank or not.

[0037] Optionally, also include:

[0038] a ninth pipeline, one end of which is connected to the impregnation tank, and the other end of which is connected to the storage tank;

[0039] A circulation pump, arranged on the ninth pipeline;

[0040] A filter, arranged on the ninth pipeline;

[0041] A ninth control valve is arranged on the ninth pipeline, and the ninth control valve is used to control whether the ninth pipeline is connected or not.

[0042] Optionally, also include:

[0043] A first control valve, disposed on the first pipeline, the first control valve being used to control whether the first pipeline is connected or not;

[0044] A second control valve is arranged on the second pipeline, and the second control valve is used to control whether the second pipeline is connected or not;

[0045] A third control valve is arranged between the water pump and the liquid distribution tank, and the third control valve is used to control whether the water pump and the liquid distribution tank are connected or not;

[0046] The sixth control valve is arranged on the sixth pipeline, and the sixth control valve is used to control whether the sixth pipeline is connected or not.

[0047] An application of a CO catalyst coating device, using any one of the CO catalyst coating devices described.

[0048] Optionally, include the following steps:

[0049] D1. Preparation stage: Open the third control valve, start the water pump, and pump the water source in the water tank into the liquid preparation tank to adjust the precious metal solution in the liquid preparation tank to the required concentration.

[0050] D2. Impregnation stage: opening the first control valve to allow the precious metal solution in the liquid preparation tank to flow into the impregnation tank, and then immersing the CO catalyst module in the impregnation tank for coating.

[0051] D3, impurity purging stage: after impregnation is completed, the first control valve is closed, the second control valve is opened, the excess precious metal solution and impurities on the CO catalyst module are purged through the purge tank, and the solution is returned to the impregnation tank for recycling.

[0052] D4, preliminary drying stage: opening the fourth control valve, transferring the CO catalyst module from the impregnation tank to the first drying tank for preliminary drying, and at the same time returning the precious metal solution in the first drying tank to the impregnation tank through the fourth pipeline.

[0053] D5, further drying stage: open the fifth control valve, transfer the CO catalyst module from the first drying tank to the second drying tank for further drying, and return the precious metal solution in the second drying tank to the impregnation tank through the fifth pipeline.

[0054] D6, solution circulation and storage stage: open the ninth control valve, circulate the precious metal solution in the impregnation tank to the storage tank through the ninth pipeline, use the circulation pump and the filter to maintain the purity and concentration of the solution, and if necessary, open the fourth control valve on the sixth pipeline to extract the precious metal solution in the storage tank back to the liquid distribution tank.

[0055] D7. Equipment end operation phase: After completing all operations, close all control valves, stop the water pump and the circulation pump, and ensure that the equipment stops operating safely.

[0056] The working principle and beneficial effects of the present invention are:

[0057] In the present invention, the preparation method of the CO catalyst achieves high efficiency and high performance of catalyst production through a series of precisely controlled process steps. In step S1, the ratio and mixing conditions of the raw materials are strictly regulated to ensure the uniform composition and physical properties of the initial dry embryo module, laying the foundation for the uniform adhesion of the precious metal coating. In step S2, the precise preparation of the palladium salt solution and the strict control of its concentration range ensure the suitability of the precious metal load in the coating, which plays a key role in the activity and selectivity of the catalyst. In step S3, the equipment parameters of the coating equipment are carefully adjusted, including the precise setting of the immersion time, temperature, and drying time and temperature, providing the best process conditions for the uniform curing of the coating and the drying of the catalyst. In step S4, the depth and loading of the precious metal coating are precisely configured, which not only ensures the performance of the catalyst, but also takes cost-effectiveness into consideration. In step S5, efficient coating equipment is used to achieve uniform coating of the dry embryo module, which not only improves production efficiency, but also ensures the quality consistency of the catalyst product. In step S6, the temperature and time of the drying and calcining process are precisely controlled, and a CO catalyst with high activity and stability is finally obtained. In addition, the introduction of WO3 (tungsten oxide), with its high melting point and thermal stability, enhances the structural and performance stability of the catalyst under high temperature conditions, and prevents the degradation of the catalyst under harsh working conditions. Pd (palladium), as the active component of the catalyst, significantly improves the efficiency of the CO oxidation reaction by virtue of its strong adsorption and activation ability for CO. At the same time, the addition of V2O5 (vanadium pentoxide) optimizes the adsorption and desorption process of the reactants by adjusting the acid-base properties of the catalyst surface, and further improves the selectivity of the catalyst. In summary, the CO catalyst preparation method of this embodiment achieves high performance and high stability of the catalyst by precisely controlling the raw material ratio, mixing conditions, solution concentration, equipment parameters, and drying and calcining process. At the same time, by adding specific compounds such as WO3 and V2O5, the thermal stability and selectivity of the catalyst are further improved, showing the broad prospects of this method in industrial catalytic applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] The preferred implementation modes will be described below in a clear and understandable manner with reference to the accompanying drawings to further illustrate the above-mentioned characteristics, technical features, advantages and implementation methods of the present invention.

[0059] Figure 1 It is a schematic diagram of the structure of the device of the present invention;

[0060] In the figure: 1, liquid distribution tank, 2, immersion tank, 3, first pipeline, 4, purge tank, 5, second pipeline, 6, first drying tank, 7, second drying tank, 8, fourth pipeline, 9, fifth pipeline, 10, storage tank, 11, sixth pipeline, 12, water tank, 13, water pump, 14, liquid pump, 15, seventh pipeline, 16, eighth pipeline, 17, fourth control valve, 18, fifth control valve, 19, ninth pipeline, 20, circulation pump, 21, filter, 22, ninth control valve, 23, first control valve, 24, second control valve, 25, third control valve, 26, sixth control valve. DETAILED DESCRIPTION

[0061] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the specific implementation methods of the present invention will be described below with reference to the accompanying drawings. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings and other implementation methods can be obtained based on these drawings without creative work.

[0062] In order to simplify the drawings, only the parts related to the invention are schematically shown in each figure, and they do not represent the actual structure of the product. In addition, in order to simplify the drawings and facilitate understanding, in some figures, only one of the parts with the same structure or function is schematically shown, or only one of them is marked. In this article, "one" not only means "only one", but also means "more than one", and "several" includes "two" and "more than two".

[0063] In this document, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0064] In addition, in the description of the present application, the terms "first", "second", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.

[0065] Reference Figure 1 , is an embodiment of the present invention, and proposes

[0066] A method for preparing a CO catalyst, characterized in that it comprises the following steps:

[0067] S1. Preparation of initial dry embryo module: The TiO2 content in the initial dry embryo module is designed to be 60-90%, the WO3 content is 1-5%, the V2O5 content is 1-5%, and the balance is mainly Al2O3 and SiO2, with a content of 1-10%. Prepare the raw materials according to the mass percentage of each component, mix all the raw materials into a mixer, add pure water, molding aids, and ammonia water, and continue stirring for 4-5 hours to mix the raw materials evenly, and control the moisture content of the mud to 28-30% and the pH to 7.0-8.0. Filter, extrude, dry, calcine, and cut the mud to obtain the initial dry embryo module;

[0068] S2. Prepare palladium salt solution: the concentration of palladium salt solution is 0.1-1%;

[0069] S3, adjusting equipment: adjusting the immersion time of the immersion tank 2 to 15-40min, adjusting the temperature of the immersion tank 2 to 25-50°C, adjusting the drying time of the first drying tank 6 and the second drying tank 7 to 15-30min, and adjusting the drying temperature of the first drying tank 6 and the second drying tank 7 to 55-65°C;

[0070] S4. Precious metal coating: The depth of precious metal coating is 0.1-0.5mm, and the load is 0.2-1kg / m3;

[0071] S5, coating: coating the dry embryo module by a coating device;

[0072] S6. Drying and calcining: drying and calcining the coated dry embryo module at a calcination temperature of 380-420° C. for 20-30 hours. After the calcination, a CO catalyst is obtained.

[0073] In this embodiment, the preparation method of the CO catalyst achieves high efficiency and high performance of catalyst production through a series of precisely controlled process steps. In step S1, the ratio and mixing conditions of the raw materials are strictly regulated to ensure the uniform composition and physical properties of the initial dry embryo module, laying the foundation for the uniform adhesion of the precious metal coating. In step S2, the precise preparation of the palladium salt solution and the strict control of its concentration range ensure the suitability of the precious metal load in the coating, which plays a key role in the activity and selectivity of the catalyst.

[0074] In the S3 step, the equipment parameters of the coating equipment were carefully adjusted, including the precise setting of the dipping time, temperature, and drying time and temperature, to provide the best process conditions for the uniform curing of the coating and the drying of the catalyst. In the S4 step, the depth and loading of the precious metal coating were precisely configured, which not only ensured the performance of the catalyst, but also took into account the cost-effectiveness.

[0075] In the S5 step, efficient coating equipment is used to achieve uniform coating of the dry preform module, which not only improves production efficiency but also ensures the quality consistency of the catalyst product. In the S6 step, the temperature and time of the drying and calcining process are precisely controlled, and finally a highly active and stable CO catalyst is obtained.

[0076] In addition, the introduction of WO3 (tungsten oxide), with its high melting point and thermal stability, enhances the structural and performance stability of the catalyst under high temperature conditions, preventing the catalyst from degrading under harsh working conditions. Pd (palladium), as the active component of the catalyst, significantly improves the efficiency of the CO oxidation reaction by virtue of its strong adsorption and activation ability for CO. At the same time, the addition of V2O5 (vanadium pentoxide) optimizes the adsorption and desorption process of the reactants by adjusting the acid-base properties of the catalyst surface, further improving the selectivity of the catalyst.

[0077] In summary, the CO catalyst preparation method of this embodiment achieves high performance and high stability of the catalyst by precisely controlling the raw material ratio, mixing conditions, solution concentration, equipment parameters, and drying and calcining process. At the same time, by adding specific compounds such as WO3 and V2O5, the thermal stability and selectivity of the catalyst are further improved, showing the broad prospects of this method in industrial catalytic applications.

[0078] A CO catalyst coating device, comprising a CO catalyst preparation method according to claim 1, comprising:

[0079] A liquid preparation tank 1, the liquid preparation tank 1 is used to place the precious metal solution;

[0080] Impregnation tank 2, impregnation tank 2 is used for impregnating the CO catalyst module;

[0081] A first pipeline 3, one end of which is connected to the liquid distribution tank 1, and the other end of which is connected to the immersion tank 2;

[0082] Purge slot 4, which is used to purge impurities on the CO catalyst module;

[0083] A second pipeline 5, one end of which is connected to the impregnation tank 2, and the other end of which is connected to the purge tank 4, and the second pipeline 5 is used to return the precious metal solution in the purge tank 4 to the impregnation tank 2;

[0084] A first drying tank 6, the first drying tank 6 is used to dry the CO catalyst module;

[0085] A second drying tank 7, the second drying tank 7 is used to further dry the CO catalyst module;

[0086] A fourth pipeline 8, one end of which is connected to the dipping tank 2, and the other end of which is connected to the first drying tank 6;

[0087] A fifth pipeline 9, one end of which is connected to the impregnation tank 2, and the other end of which is connected to the second drying tank 7. The fifth pipeline 9 and the fourth pipeline 8 are used to return the precious metal solution in the first drying tank 6 and the second drying tank 7 to the impregnation tank 2;

[0088] A storage tank 10, for storing excess precious metal solution;

[0089] The sixth pipeline 11 is connected to the storage tank 10 at one end and to the liquid preparation tank 1 at the other end. When the liquid level of the liquid preparation tank 1 is higher than that of the storage tank 10 , the sixth pipeline 11 is used to transfer the precious metal solution in the liquid preparation tank 1 to the storage tank 10 by gravity.

[0090] In this embodiment, the reflux equipment formed by the first to sixth pipelines 11 realizes the recycling of precious metal solution in the process of impregnation, purging and drying, significantly reduces the waste of solution and improves the utilization efficiency of precious metal. The design of the impregnation tank 2 ensures that the CO catalyst module can be evenly coated with precious metal solution during the impregnation process, thereby improving the performance and consistency of the catalyst. The series use of the first drying tank 6 and the second drying tank 7, in conjunction with the reflux of the precious metal solution, reduces the energy consumption required to achieve the drying effect and achieves energy saving. Through the precise control of each control valve, the automation of the coating process is realized, the uncertainty of manual operation is reduced, and the production efficiency and repeatability are improved. The use of the purge tank 4 effectively removes impurities on the CO catalyst module, cooperates with the recycling of the precious metal solution, and reduces pollution to the environment. The simplicity and safety of operation are taken into account in the equipment design, and the contact between operators and harmful substances is reduced through automated control, thereby reducing the safety risks in the production process. By accurately controlling various parameters in the coating process, such as impregnation time, temperature and solution concentration, a guarantee is provided for the preparation of high-performance CO catalysts.

[0091] Optionally, also include:

[0092] A water tank 12, used to provide water;

[0093] A water pump 13, one end of which is connected to the water tank 12, and the other end of which is connected to the liquid distribution tank 1, and the water pump 13 is used to pump water in the water tank 12 into the liquid distribution tank 1;

[0094] The liquid pump 14 is disposed on the sixth pipeline 11 , and is used to extract the precious metal solution in the storage tank 10 into the liquid preparation tank 1 .

[0095] In this embodiment, the optional configuration of the CO catalyst coating device further improves the efficiency and flexibility of the device by introducing a water tank 12 and a corresponding water pump 13 and a liquid pump 14. The water tank 12 provides a stable water source for the equipment, ensuring a continuous supply of precious metal solution, while the water pump 13 ensures the smooth transfer of water from the water tank 12 to the liquid distribution tank 1, maintaining the required concentration and quantity of the solution. In addition, the liquid pump 14 is arranged on the sixth pipeline 11, which realizes the effective circulation of the precious metal solution between the storage tank 10 and the liquid distribution tank 1, which not only improves the recovery rate of precious metals, but also reduces the cost increase caused by the waste of solution. Overall, the addition of these optional components has significantly improved the ease of operation, cost-effectiveness and environmental friendliness of the entire device.

[0096] Optionally, also include:

[0097] A seventh pipeline 15, one end of which is connected to the fourth pipeline 8, and the other end of which is connected to the storage tank 10;

[0098] an eighth pipeline 16, one end of which is connected to the fifth pipeline 9, and the other end of which is connected to the storage tank 10;

[0099] A fourth control valve 17, disposed on the fourth pipeline 8, for controlling whether the fourth pipeline 8 is connected to the first drying tank 6 or not;

[0100] The fifth control valve 18 is disposed on the fifth pipeline 9 and is used to control whether the fifth pipeline 9 is connected to the second drying tank 7 or not.

[0101] Optionally, also include:

[0102] A ninth pipeline 19, one end of which is connected to the impregnation tank 2, and the other end of which is connected to the storage tank 10;

[0103] A circulation pump 20 is arranged on the ninth pipeline 19;

[0104] A filter 21 is provided on the ninth pipeline 19;

[0105] The ninth control valve 22 is disposed on the ninth pipeline 19 , and is used to control whether the ninth pipeline 19 is connected or not connected.

[0106] Optionally, also include:

[0107] A first control valve 23 is provided on the first pipeline 3, and the first control valve 23 is used to control whether the first pipeline 3 is connected or not;

[0108] A second control valve 24 is provided on the second pipeline 5, and the second control valve 24 is used to control whether the second pipeline 5 is connected or not;

[0109] The third control valve 25 is disposed between the water pump 13 and the liquid distribution tank 1. The third control valve 25 is used to control whether the water pump 13 and the liquid distribution tank 1 are connected or not;

[0110] The sixth control valve 26 is disposed on the sixth pipeline 11 , and is used to control whether the sixth pipeline 11 is connected or disconnected.

[0111] In this embodiment, through the additional pipelines and control valves, the CO catalyst coating equipment achieves more sophisticated process control and efficient resource management. The introduction of the seventh and eighth pipelines 16, which are connected to the fourth pipeline 8 and the fifth pipeline 9 respectively, allows the precious metal solution to flow directly back between the drying tank and the storage tank 10, optimizes the recycling of the solution and reduces unnecessary flow in the equipment. The setting of the sixth control valve 26 and the fifth control valve 18 provides precise control of the flow direction of the solution, ensuring the efficiency of the drying process and the uniform distribution of the solution. The ninth pipeline 19 cooperates with the circulation pump 20 and the filter 21 to further ensure the purity and continuous supply of the precious metal solution in the immersion tank 2, while the ninth control valve 22 allows the operator to flexibly control the circulation of the solution as needed. In addition, the setting of the first control valve 23, the second control valve 24 and the third control valve 25 provides multi-level control for the equipment, so that the entire coating process can be flexibly adjusted according to actual production needs, thereby improving the adaptability of the equipment and the convenience of operation. Overall, the addition of these optional components significantly improves the automation level and operating efficiency of the equipment, while reducing production costs and enhancing the stability and reliability of the equipment.

[0112] An application of a CO catalyst coating device, using any one of the CO catalyst coating devices.

[0113] Optionally, include the following steps:

[0114] D1. Preparation stage: Open the third control valve 25, start the water pump 13, and pump the water source in the water tank 12 into the liquid preparation tank 1 to adjust the precious metal solution in the liquid preparation tank 1 to the required concentration.

[0115] D2, impregnation stage: open the first control valve 23 to allow the precious metal solution in the liquid preparation tank 1 to flow into the impregnation tank 2, and then immerse the CO catalyst module into the impregnation tank 2 for coating.

[0116] D3, impurity purging stage: After the impregnation is completed, the first control valve 23 is closed, and the second control valve 24 is opened to purge the excess precious metal solution and impurities on the CO catalyst module through the purge tank 4, and the solution is returned to the impregnation tank 2 for recycling.

[0117] D4, preliminary drying stage: open the fourth control valve 17, transfer the CO catalyst module from the impregnation tank 2 to the first drying tank 6 for preliminary drying, and at the same time return the precious metal solution in the first drying tank 6 to the impregnation tank 2 through the fourth pipeline 8.

[0118] D5, further drying stage: open the fifth control valve 18, transfer the CO catalyst module from the first drying tank 6 to the second drying tank 7 for further drying, and return the precious metal solution in the second drying tank 7 to the impregnation tank 2 through the fifth pipeline 9.

[0119] D6, solution circulation and storage stage: open the ninth control valve 22, circulate the precious metal solution in the impregnation tank 2 to the storage tank 10 through the ninth pipeline 19, use the circulation pump 20 and the filter 21 to maintain the purity and concentration of the solution, and if necessary, open the fourth control valve 17 on the sixth pipeline 11 to extract the precious metal solution in the storage tank 10 back to the liquid preparation tank 1.

[0120] D7. Equipment end operation phase: After completing all operations, close all control valves, stop the water pump 13 and the circulation pump 20, and ensure that the equipment stops operating safely.

[0121] In this embodiment, the application of the coating equipment for CO catalyst achieves high efficiency and environmental protection of catalyst production through a series of precisely controlled steps. In the preparation stage, the concentration of the precious metal solution in the liquid distribution tank 1 is quickly adjusted through the coordinated work of the third control valve 25 and the water pump 13, ensuring the uniformity and consistency of the solution. In the impregnation stage, the first control valve 23 is used to accurately control the flow direction of the solution to ensure the uniform coating of the CO catalyst module. In the impurity purge stage, the second control valve 24 is opened to effectively remove the excess solution and impurities on the module, and the solution is recycled through the reflux equipment, reducing resource waste. In the drying stage, the timely opening of the fourth and fifth control valves 18 not only ensures the full drying of the catalyst module, but also further improves the utilization efficiency of the solution through the pipeline reflux equipment. In the solution circulation and storage stage, the coordinated use of the ninth control valve 22, the circulation pump 20 and the filter 21 realizes the continuous purification and circulation of the solution, maintains the quality of the solution, and at the same time, through the adjustment of the fourth control valve 17, the storage and recovery of the solution are flexibly managed, optimizing the production process. Finally, at the end of the equipment operation, all control valves were closed in an orderly manner and the pumps were stopped to ensure safe shutdown of the equipment. The automation and intelligent design of the entire application process significantly improved production efficiency and reduced energy consumption and production costs.

[0122] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a CO catalyst, characterized in that: The following steps are involved: S1. Preparation of initial dry embryo module: The TiO2 content, WO3 content, V2O5 content, and balance of Al2O3 and SiO2 in the initial dry embryo module are designed to be 60-90%, 1-5%, and 1-10%, respectively. Raw materials are prepared according to the mass percentage of each component, all raw materials are mixed and put into a mixer, pure water, molding aid, and ammonia water are added, and stirring is continued for 4-5 hours to mix the raw materials evenly, and the moisture content of the mud is controlled at 28-30%, and the pH is 7.0-8.

0. The mud is filtered, extruded, dried, calcined, and cut to obtain an initial dry embryo module; S2. Prepare palladium salt solution: the concentration of palladium salt solution is 0.1-1%; S3, adjusting equipment: adjusting the immersion time of the immersion tank to 15-40min, adjusting the temperature of the immersion tank to 25-50°C, adjusting the drying time of the first drying tank and the second drying tank to 15-30min, and adjusting the drying temperature of the first drying tank and the second drying tank to 55-65°C; S4. Precious metal coating: The depth of precious metal coating is 0.1-0.5mm, and the load is 0.2-1kg / m3; S5, coating: coating the dry embryo module by the coating equipment; S6. Drying and calcining: drying and calcining the coated dry embryo module at a calcination temperature of 380-420° C. for 20-30 hours. After the calcination, a CO catalyst is obtained.

2. A CO catalyst coating device, comprising a CO catalyst preparation method according to claim 1, characterized in that: include: A liquid preparation tank (1), wherein the liquid preparation tank (1) is used to place a precious metal solution; An impregnation tank (2), wherein the impregnation tank (2) is used to impregnate the CO catalyst module; A first pipeline (3), one end of which is connected to the liquid preparation tank (1), and the other end of which is connected to the immersion tank (2); A purge groove (4), the purge groove (4) being used to purge impurities on the CO catalyst module; a second pipeline (5), one end of which is connected to the impregnation tank (2) and the other end of which is connected to the purge tank (4), the second pipeline (5) being used to return the precious metal solution in the purge tank (4) to the impregnation tank (2); a first drying tank (6), the first drying tank (6) being used for drying the CO catalyst module; a second drying tank (7), wherein the second drying tank (7) is used to further dry the CO catalyst module; a fourth pipeline (8), one end of which is connected to the impregnation tank (2), and the other end of which is connected to the first drying tank (6); a fifth pipeline (9), one end of which is connected to the impregnation tank (2) and the other end of which is connected to the second drying tank (7); the fifth pipeline (9) and the fourth pipeline (8) are used to return the precious metal solution in the first drying tank (6) and the second drying tank (7) to the impregnation tank (2); A storage tank (10) for storing excess precious metal solution; A sixth pipeline (11) is connected to the storage tank (10) at one end and to the liquid distribution tank (1) at the other end. When the liquid level of the liquid distribution tank (1) is higher than that of the storage tank (10), the sixth pipeline (11) is used to flow the precious metal solution in the liquid distribution tank (1) into the storage tank (10) by gravity.

3. A CO catalyst coating device according to claim 1, characterized in that: Also includes: A water tank (12), used for providing a water source; A water pump (13), one end of which is connected to the water tank (12) and the other end of which is connected to the liquid distribution tank (1), the water pump (13) being used to pump water from the water tank (12) into the liquid distribution tank (1); A liquid extraction pump (14) is arranged on the sixth pipeline (11), and the liquid extraction pump (14) is used to extract the precious metal solution in the storage tank (10) into the liquid preparation tank (1).

4. A CO catalyst coating device according to claim 1, characterized in that: Also includes: a seventh pipeline (15), one end of which is connected to the fourth pipeline (8), and the other end of which is connected to the storage tank (10); an eighth pipeline (16), one end of which is connected to the fifth pipeline (9), and the other end of which is connected to the storage tank (10); a fourth control valve (17), arranged on the fourth pipeline (8), and used to control whether the fourth pipeline (8) and the first drying tank (6) are connected or not connected; A fifth control valve (18) is provided on the fifth pipeline (9) and is used to control whether the fifth pipeline (9) and the second drying tank (7) are connected or not connected.

5. A CO catalyst coating device according to claim 1, characterized in that: Also includes: a ninth pipeline (19), one end of which is connected to the impregnation tank (2) and the other end of which is connected to the storage tank (10); A circulation pump (20) arranged on the ninth pipeline (19); A filter (21) disposed on the ninth pipeline (19); A ninth control valve (22) is arranged on the ninth pipeline (19), and the ninth control valve (22) is used to control whether the ninth pipeline (19) is connected or not connected.

6. A CO catalyst coating device according to claim 2, characterized in that: Also includes: A first control valve (23) is arranged on the first pipeline (3), and the first control valve (23) is used to control whether the first pipeline (3) is connected or not connected; a second control valve (24), arranged on the second pipeline (5), the second control valve (24) being used to control whether the second pipeline (5) is connected or not connected; A third control valve (25) is arranged between the water pump (13) and the liquid distribution tank (1), and the third control valve (25) is used to control whether the water pump (13) and the liquid distribution tank (1) are connected or not connected; A sixth control valve (26) is arranged on the sixth pipeline (11), and the sixth control valve (26) is used to control whether the sixth pipeline (11) is connected or disconnected.

7. Application of a CO catalyst coating device, using the CO catalyst coating device according to any one of claims 2 to 6.

8. The use of a coating device for a CO catalyst according to claim 6, characterized in that: The following steps are involved: D1, preparation stage: opening the third control valve (25), starting the water pump (13), and pumping the water source in the water tank (12) into the liquid preparation tank (1) to adjust the precious metal solution in the liquid preparation tank (1) to a desired concentration; D2, impregnation stage: opening the first control valve (23) to allow the precious metal solution in the liquid preparation tank (1) to flow into the impregnation tank (2), and then immersing the CO catalyst module in the impregnation tank (2) for coating; D3, impurity purging stage: after the impregnation is completed, the first control valve (23) is closed, the second control valve (24) is opened, the excess precious metal solution and impurities on the CO catalyst module are purged through the purge tank (4), and the solution is returned to the impregnation tank (2) for recycling; D4, preliminary drying stage: opening the fourth control valve (17), transferring the CO catalyst module from the impregnation tank (2) to the first drying tank (6) for preliminary drying, and at the same time returning the precious metal solution in the first drying tank (6) to the impregnation tank (2) through the fourth pipeline (8); D5, further drying stage: opening the fifth control valve (18), transferring the CO catalyst module from the first drying tank (6) to the second drying tank (7) for further drying, and returning the precious metal solution in the second drying tank (7) to the impregnation tank (2) through the fifth pipeline (9); D6, solution circulation and storage stage: the ninth control valve (22) is opened to circulate the precious metal solution in the impregnation tank (2) to the storage tank (10) through the ninth pipeline (19), and the purity and concentration of the solution are maintained by using the circulation pump (20) and the filter (21). If necessary, the precious metal solution in the storage tank (10) is pumped back to the liquid preparation tank (1) by opening the fourth control valve (17) on the sixth pipeline (11); D7, equipment end operation phase: after all operations are completed, all control valves are closed, the water pump (13) and the circulation pump (20) are stopped, and the equipment is ensured to stop operating safely.