Molecular sieve catalyst and preparation and application thereof

Through the molecular sieve catalyst modified by non-metal oxides and metal oxides, combined with thermal cracking and catalytic cracking, the problems of low DMK yield and incomplete IBA utilization in IBAN cracking are solved, efficient TMCD production is achieved, and energy consumption and equipment are reduced. Require.

CN118988387APending Publication Date: 2024-11-22DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202411040349.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, during the IBAN cracking process, the one-way yield of DMK is low, and the unreacted IBA in the condensate is not efficiently utilized, resulting in insufficient yield of TMCD, and the thermal cracking process requires high equipment investment and energy consumption.

Method used

Using a molecular sieve catalyst co-modified by non-metal oxides and metal oxides, the acid amount and acid strength of the molecular sieve are regulated by coupling thermal cracking and catalytic cracking processes. DMK is prepared with IBAN or IBA mixtures using a modified molecular sieve catalyst and passed through multi-stage The absorption and dimerization reaction process improves the yield of TMCD.

Benefits of technology

The high selective generation of DMK is achieved, the IBAN conversion rate and TMCD yield are improved, the separation loss and energy consumption are reduced, the changes in raw material composition are adapted to the changes in raw material composition, and the raw material utilization is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988387A_ABST
    Figure CN118988387A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalyst preparation, and particularly relates to a catalyst for preparing dimethyl ketene through cracking reaction of an isobutyric anhydride / isobutyric acid mixture. The invention also provides a reaction process matched with the catalyst and used for cracking an isobutyric anhydride / isobutyric acid mixture, thermal cracking and catalytic cracking processes are coupled, and dimethyl ketene generated by cracking is used as an intermediate to be finally used for producing 2, 2, 4, 4-tetramethyl-1, 3-cyclobutanedione, so that the yield of 2, 2, 4, 4-tetramethyl-1, 3-cyclobutanedione is increased. The method specifically relates to operation units of preheating, cracking, chilling, gas-liquid separation, absorption, dimerization and the like. Compared with the prior art, the method provided by the invention adopts the modified molecular sieve catalyst to catalyze high-selectivity cracking of the isobutyric anhydride / isobutyric acid mixture into the dimethyl ketene, and realizes the process of producing the 2, 2, 4, 4-tetramethyl-1, 3-cyclobutanedione by using the isobutyric anhydride / isobutyric acid mixture as the raw material in combination with the reaction process provided by the invention, so that the yield of the 2, 2, 4, 4-tetramethyl-1, 3-cyclobutanedione is improved. The potential industrial application prospect is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention discloses a method for preparing dimethyl ketone (DMK) from isobutyric anhydride (IBAN) or a mixture of IBAN and isobutyric acid (IBA) (IBAN+IBA) and further producing 2,2,4,4-tetramethyl-1,3-cyclobutanedione, and specifically relates to a modified molecular sieve catalyst for preparing dimethyl ketone from IBAN or IBAN+IBA, and a reaction process matching the catalyst for producing 2,2,4,4-tetramethyl-1,3-cyclobutanedione by using dimethyl ketone as an intermediate. Background Art

[0002] 2,2,4,4-Tetramethyl-1,3-cyclobutadione (TMCD), molecular formula C8H 12 O2, melting point 114-116℃, boiling point 208.3±15.0℃, density 0.995g / cm 3 Mainly used for hydrogenation reaction to prepare 2,2,4,4-tetramethyl-1,3-cyclobutanediol, English name 2,2,4,4-Tetramethyl-1,3-cyclobutanediol (CBDO), molecular formula C8H 16 O2. CBDO is an important aliphatic diol polyester monomer with a symmetrical structure and two isomers, cis and trans. Tritan copolyester can be produced by copolymerization of CBDO, terephthalic acid (PTA) and 1,4-cyclohexanedimethanol (CHDM). This polyester can be widely used in the production of food and sanitary utensils due to its characteristics of not containing bisphenol A, high transparency and good weather resistance. It is also widely used in the fields of medical treatment, cosmetics and optical devices. Therefore, as a key intermediate in the production of CBDO, the synthesis method of TMCD is crucial.

[0003] At present, the synthesis technology of TMCD is mastered by Eastman Company in the United States. US5258556A reports a method for preparing DMK vapor by pyrolyzing IBAN at 350-600℃. The obtained gas phase product contains both IBA and unreacted IBAN. By quenching the reactants, the mixture of IBA and IBAN can be separated from DMK. Then the DMK vapor is sent to the absorption zone, and the DMK vapor contacts with the solvent containing TMCD to complete the absorption process. The absorption liquid containing DMK finally enters the dimerization zone, and the DMK dissolved in the absorption liquid is converted into TMCD. The whole process does not use a catalyst, and the single-pass yield of TMCD is about 18-20% based on IBAN, and the conversion rate of DMK is between 43-54%. Similar to the above method, French Arkema patent US7435856B2 reported a method for cracking IBAN in a vacuum tube to produce DMK and further prepare polydimethyl ketone (PDMK). Under the conditions of cracking temperature of 484°C and residence time of 0.19s, IBAN vapor with a concentration of 15% can be completely cracked into DMK with a conversion rate of 91%. The above patent does not specifically explain how to recycle IBA produced as a byproduct after cracking IBAN into DMK.

[0004] In recent years, many domestic units have successively tackled the synthesis technology of TMCD and CBDO. Representative research institutions include: China Petroleum Liaoyang Petrochemical Company, Zhejiang University, Zhejiang Henglan Technology Co., Ltd., Taiwan Industrial Technology Research Institute, Sinopec Shanghai Petrochemical Research Institute, Wanhua Chemical Group Co., Ltd. and Suzhou Yake Technology Co., Ltd.

[0005] Patent CN105732354A reports a method for preparing TMCD by directly polymerizing the gaseous DMK product after cracking IBAN. A mixed solution of dimethyl adipate and dimethyl 1,4-cyclohexanedicarboxylate in a ratio of 1:1 to 1:3 is selected as the absorption liquid. DMK is directly polymerized at 60 to 120°C and normal pressure, eliminating the washing tower or absorption tower, reducing equipment investment; the above cracking reaction process does not use a catalyst, and the cracking conversion rate of IBAN can reach 70%, obtaining 15wt% TMCD relative to the solvent. Patent CN111718252A reports a method for preparing DMK by cracking IBAN under catalyst-free conditions. An ester reagent such as isobutyl isobutyrate is used as the absorption liquid. DMK is absorbed under low temperature conditions by bubbling and spontaneously dimerized in the solution to generate TMCD. The generated TMCD product is separated by crystallization operation, and the ester solution is recovered and utilized by distillation. Patent CN112174797B reports an efficient separation method for DMK, which reduces the separation loss of DMK and improves the separation efficiency by adding low-temperature inert gas at the outlet of the cracking reactor to quench the cracking products and shorten the residence time of the mixed gas in the heat exchanger; the examples show that with the increase in the flow rate of the added inert gas, the proportion of isobutyric anhydride in the condensate decreases from 74.6% to 52.5%, and the proportion of isobutyric acid increases from 24.5% to 46.7%; under the conditions of 500°C and 10kPa, the yield of DMK can be increased from 12.4% to 21.1% after adding nitrogen, and no catalyst is used in the cracking reaction process. Patent CN117342937A reports a method of using a mixed solution of isopropyl acetate and dimethyl ketene β-lactone dimer as a DMK absorbent. When the β-lactone dimer concentration of DMK is 7%, the recovery rate of DMK can reach 98.0%. After the absorption process lasts for 4 hours, the DMK concentration in the absorption liquid can reach 32.6%. The selectivity of TMCD in the dimerization process is 98.9%, and the TMCD yield is 98.6%. In this method, DMK is prepared by mixing diluent gas with IBAN, preheating, vaporizing, and then entering a cracking furnace for cracking. No catalyst is used in the cracking process. Patent CN117486703A discloses a method for mixing IBAN, small molecule alcohol and p-toluenesulfonic acid or methanesulfonic acid and then performing high temperature cracking. IBAN is cracked to generate DMK and IBA, wherein IBA reacts with small molecule alcohol under the catalytic action of a small amount of organic acid to generate corresponding isobutyrate, which can effectively inhibit the reaction of DMK and IBA to generate IBAN again, thereby facilitating the forward movement of chemical equilibrium, improving the conversion rate of the reaction and inhibiting carbon deposition; the cracked products are separated, the isobutyrate is recovered and used as an absorption liquid for absorbing DMK, and finally TMCD is prepared through a dimerization reaction.The disadvantage of the above method is that IBAN is mainly converted into DMK through a thermal cracking process. On the one hand, the condensate after IBAN cracking contains a large amount of unreacted IABN and IBA, and the IBA in the condensate is not efficiently utilized, resulting in a low single-pass yield of DMK, which in turn affects the yield of TMCD in the final product; on the other hand, an extremely short residence time and quenching operation are required to suppress the IBA produced in the cracking process from reacting with DMK to generate IBAN again, which requires a high investment in cracking, quenching and absorption equipment and increases the separation energy consumption.

[0006] Patent US6232504B1 of the University of Delaware in the United States reported a columnar monolithic SiO2 catalyst that can convert IBA into DMK at 553°C, where the conversion rate of IBA is 95%, the selectivity of DMK is 98%, and the selectivity of CO2 is less than 2%. Patent CN116751113A reported a method for preparing DMK by cracking a mixture of IBAN and IBA using an iron-chromium-aluminum alloy catalyst containing an alumina active layer on the surface. The alloy catalyst has the characteristics of high pyrolysis efficiency and good stability, and the internal mesh structure can effectively reduce the pressure drop of the cracking reaction bed. The single-pass conversion rate of isobutyric anhydride can reach up to 85.1%, and the DMK selectivity is 95%. Using ester reagents such as n-butyl acetate as absorbents, the absorbed DMK can be efficiently converted into TMCD. The metal catalytic reaction system can operate stably for more than a thousand hours. It can be seen that by using metal or non-metal oxides as catalysts, it is expected to achieve further dehydration of IBA to produce DMK under catalytic cracking conditions, thereby coupling the thermal cracking and catalytic cracking processes to convert the mixture of IBAN and IBA into DMK with high selectivity and improve the yield of TMCD products. Summary of the invention

[0007] The purpose of the present invention is to prepare DMK by coupling thermal cracking and catalytic cracking processes using IBAN or a mixture of IBAN+IBA as raw materials, the cracking process is carried out under the action of a molecular sieve catalyst modified by a non-metallic oxide and a metal oxide, the catalyst uses pseudo-boehmite as a binder and sesbania powder as a pore-forming agent, the catalyst has the characteristics of high cracking efficiency, good selectivity and resistance to carbon deposition, and provides a catalytic reaction process matched with the catalyst, the process is for the purpose of collecting the gaseous DMK product produced in the cracking process and dimerizing it into TMCD, the process includes preheating, cracking, quenching, gas-liquid separation, absorption and dimerization operation units. The reaction process is shown in Formula 1:

[0008]

[0009] The object of the present invention can be achieved by the following technical scheme: a preparation method for preparing DMK catalyst by cracking reaction of IBAN or IBAN+IBA mixture, characterized in that molecular sieves with topological structures such as commercial MFI and FAU are used as active components, pseudo-boehmite is used as a binder, and extrusion is adopted, wherein the mass of the molecular sieve accounts for 0.1 to 99% of the total mass of the catalyst, preferably 50 to 99%, and more preferably 66 to 99%.

[0010] The non-metallic oxide and metal oxide modified molecular sieve catalyst is prepared according to the following steps:

[0011] (1) mixing one or more of commercial MFI (NaZSM-5 or pure silicon Silicalite-1) or FAU (NaX, NaY or USY) molecular sieves with a certain mass of pseudo-boehmite and sesbania powder, and adding a certain amount of dilute nitric acid solution with a mass fraction of 10wt% during the mixing process, wherein the mass ratio of the molecular sieve, pseudo-boehmite, sesbania powder and dilute nitric acid is 1-20:0.1-6:0.1-5:1-10 (preferably 5-10:2-5:0.1-2:1-8, more preferably 10:3-5:1:2-5);

[0012] If Silicalite-1 pure silicon molecular sieve is used as the catalyst, 10-30wt% silica sol can be used to replace dilute nitric acid;

[0013] (2) The wet materials obtained in step (1) are mixed uniformly and then extruded into strips, dried in an oven at 80-120° C. for 1-24 h, and calcined in an air atmosphere at 300-600° C. for 1-12 h in a muffle furnace to obtain a shaped molecular sieve catalyst; preferably, dried at 90-100° C. for 12-24 h, and calcined at 450-550° C. for 4-8 h;

[0014] If Silicalite-1 pure silicon molecular sieve is used as a catalyst, it can be directly used for cracking reaction to produce DMK without the following modification steps;

[0015] (3) the Na-type shaped molecular sieve catalyst obtained in step (2) was ion exchanged three times at RT to 90° C. using a 0.1 to 2.0 mol / L NH 4 NO 3 solution at a solid-liquid ratio of 1:1.5 to 1:20, each exchange lasting 0.5 to 5 hours;

[0016] (4) Drying the catalyst obtained in step (3) at 80-120° C. for 1-24 h, and calcining at 300-600° C. for 1-12 h to obtain an H-type formed molecular sieve catalyst.

[0017] (5) The H-type molecular sieve catalyst is modified with non-metallic oxides. The main purpose of the modification is to cover a part of the acid center and reduce the acid strength of the molecular sieve. The non-metallic oxides include but are not limited to one or more of SiO2, P2O5 and B2O3. When the molecular sieve catalyst is modified with SiO2, the method is as follows: the catalyst is immersed in a cyclohexane solution containing tetraethyl orthosilicate or silicone oil by an equal volume impregnation method, sealed for 12 hours and then dried in the shade at room temperature, and calcined at a temperature of 300-600°C for 4-12 hours. The amount of tetraethyl orthosilicate or silicone oil added is calculated according to the amount of SiO2 finally decomposed, and the deposition amount of SiO2 accounts for 1-30wt% of the total mass of the catalyst.

[0018] (6) When the molecular sieve catalyst is modified with P2O5, the method is the same as step (5), and one or more of diammonium hydrogen phosphate, disodium hydrogen phosphate, sodium hypophosphite, potassium hypophosphite or ammonium hypophosphite is selected as the precursor, and water is used as the solvent. The deposition amount of P2O5 accounts for 1 to 30 wt% of the total mass of the catalyst.

[0019] (7) When the molecular sieve catalyst is modified with B2O3, the method is the same as step (5), boric acid is selected as the precursor, water or ethanol is used as the solvent, and the deposited amount of B2O3 accounts for 1 to 30 wt% of the total mass of the catalyst.

[0020] (8) The non-metallic oxide modified molecular sieve catalyst is modified with a metal oxide, wherein the metal oxide includes but is not limited to one or more of alkaline earth metal MgO and rare earth metal La2O3, CeO2, etc. The main purpose of the modification is to further reduce the acid content and acid strength of the molecular sieve and improve the acid resistance of the molecular sieve. When the molecular sieve catalyst is modified with MgO, the catalyst modified with the non-metallic oxide in step (5) is immersed in an aqueous solution containing magnesium acetate or magnesium nitrate by an equal volume impregnation method, and after being immersed at room temperature for 12 hours, it is dried at 80-120° C. for 12 hours, and calcined in a muffle furnace at a temperature of 300-600° C. for 4-12 hours to obtain a molecular sieve catalyst modified with MgO and a non-metallic oxide, wherein the deposited amount of MgO accounts for 1-30wt% of the total mass of the catalyst.

[0021] (9) When La2O3 is used to modify the molecular sieve catalyst, the method is the same as step (8), using lanthanum nitrate as a precursor and water as a solvent, and the deposited amount of La2O3 accounts for 1 to 30 wt% of the total mass of the catalyst.

[0022] (10) When the molecular sieve catalyst is modified with CeO2, the method is the same as step (8), using cerium nitrate as a precursor and water as a solvent, and the deposition amount of CeO2 accounts for 1 to 30 wt% of the total mass of the catalyst.

[0023] (11) In the above (5) to (10), the deposited amount of the non-metallic oxide is preferably 5 to 20 wt% of the total mass of the catalyst; the deposited amount of the metal oxide is preferably 5 to 20 wt% of the total mass of the catalyst.

[0024] The present invention provides a reaction process for cracking IBAN or a mixture of IBAN+IBA to produce DMK and further prepare TMCD as follows:

[0025] (1) IBAN or a mixture of IBAN+IBA is mixed with an inert carrier gas and then introduced into a preheating furnace for gasification. The feed rate in the liquid supply pipe is 0.1 to 20 ml / min, preferably 1 to 10 ml / min. The gas supply pipe uses one of N2, He, Ar, H2, CH4, CO or CO2 as an inert carrier gas, and the gas flow rate is 50 ml / min to 5 L / min. Preferably, N2 or Ar is used as the carrier gas, and the gas flow rate is preferably 100 ml / min to 2 L / min.

[0026] (2) The inner diameter of the preheating furnace is Φ20 mm, the total height of the furnace is 300 mm, the power is 1.2 kW, a stainless steel preheating tube with an inner diameter of Φ10 mm is placed in the preheating furnace, the working temperature range of the preheating furnace is 100 to 800° C., and the preferred working temperature range is 180 to 350° C.;

[0027] (3) The high-temperature cracking furnace has an inner diameter of Φ20 mm, a total furnace height of 380 mm, and a power of 1.2 kW. A quartz reaction tube with an outer diameter of Φ14 mm and an inner diameter of Φ10 mm is placed in the high-temperature cracking furnace. The operating temperature range of the high-temperature cracking furnace is 100 to 800° C., preferably 200 to 550° C. A catalyst bed with a height of 5 cm is added in the constant temperature section. The residence time of the mixed material on the catalyst bed is 0.01 s to 5 s; preferably 0.01 s to 1 s;

[0028] (4) The cracked product is passed into a condenser for quenching, and then enters a gas-liquid separation tank for gas-liquid separation. A rapid low-temperature cooling cycle machine is used to provide cooling medium for the condenser and the gas-liquid separation tank. The cooling temperature is 0 to -10°C. The condensate containing IBAN and IBA collected in the gas-liquid separation tank can be used as a cracking reaction raw material again;

[0029] (5) The gaseous DMK product is drawn out from the top of the gas-liquid separation tank and introduced into an absorption tank 1 containing 50 to 1000 ml of an ester absorbent through a bottom-inserted tube to absorb the DMK. The ester absorbent includes but is not limited to one or more of methyl isobutyrate, ethyl isobutyrate, isobutyl isobutyrate, butyl acetate or isopropyl acetate. A rapid low-temperature cooling cycle machine is used to provide a cooling medium for the absorption tank. The absorption temperature of the absorption tank is RT to -10°C.

[0030] (6) The gaseous DMK product after primary absorption is drawn out from the top of the absorption tank 1 and introduced into the absorption tank 2 containing 50-1000 ml of ester absorbent through a bottom tube for secondary absorption of DMK. The ester absorbent and absorption temperature are the same as those in step (5);

[0031] (7) The ester absorption liquid after absorbing DMK in absorption tank 1 and absorption tank 2 is mixed and poured into a stainless steel high-pressure reactor with a polytetrafluoroethylene liner, and polymerized at 50-150° C. and 0.1-1.0 MPa for 1-24 h to obtain an ester solution containing TMCD, preferably at 50-100° C. and 0.1-1.0 MPa for 2-12 h. The ester absorbent can be recovered by distillation to obtain a crude product of TMCD. Repeating the above process can reduce the impurity content and improve the purity of the TMCD product.

[0032] The present invention also provides a reaction process for cracking IBAN or IBAN+IBA mixtures matching the catalyst, coupling thermal cracking and catalytic cracking processes, and using dimethyl ketene produced by cracking as an intermediate to ultimately produce 2,2,4,4-tetramethyl-1,3-cyclobutanedione, specifically involving preheating, cracking, quenching, gas-liquid separation, absorption and dimerization operation units. Compared with the prior art, the method described in the present invention uses a modified molecular sieve catalyst to catalyze the highly selective cracking of an isobutyric anhydride / isobutyric acid mixture into dimethyl ketene, and combined with the reaction process described in the present invention, the process of producing 2,2,4,4-tetramethyl-1,3-cyclobutanedione using an isobutyric anhydride / isobutyric acid mixture as a raw material is realized, which has potential industrial application prospects.

[0033] Compared with the prior art, the advantages of the present invention are:

[0034] (1) The present invention uses a molecular sieve modified with a non-metallic oxide and a metal oxide as a catalyst for cracking IBAN or a mixture of IBAN and IBA to prepare DMK, coupling the thermal cracking process of IBAN and the catalytic cracking process of IBA. By regulating the acid amount and acid strength of the molecular sieve, the decomposition reaction and carbon deposition deactivation of DMK are effectively suppressed, a highly selective DMK product is obtained, and the single-pass conversion rate of the cracking raw material is improved.

[0035] (2) The present invention discloses a reaction process matched with a molecular sieve catalyst, which can adapt to the mixed feeding method of IBAN or a mixture of IBAN and IBA. Compared with the prior art which mainly relies on pure IBAN as a raw material, it has lower requirements on the raw material composition, wider sources of raw materials, and higher raw material utilization rate.

[0036] (3) The present invention discloses a process for absorbing DMK, which realizes an efficient absorption process of the gaseous DMK product through single-stage absorption or two-stage series absorption of the DMK gaseous product under low temperature conditions, thereby reducing the DMK content in the tail gas to the greatest extent and realizing efficient utilization of the ester absorption liquid. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 The present invention is a reaction process flow chart for preparing DMK by cracking a mixture of IBAN and IBA matched with a molecular sieve catalyst. DETAILED DESCRIPTION

[0038] The present invention will be further described below with examples. However, the scope of the present invention is not limited by these examples.

[0039] The present invention provides a reaction process matching a non-metallic oxide and a metal oxide modified molecular sieve catalyst. Figure 1 As shown, Figure 1 The symbols are: filter 1, ball valve 2, pressure reducing valve 3, flow meter 4, check valve 5, pressure gauge 6, metering pump 7, preheating furnace 8, temperature controller 9, high temperature cracking furnace 10, condenser 11, gas-liquid separation tank 12, needle valve 13, absorption tank 14. The high temperature cracking furnace has a built-in cracking reactor made of quartz tube; the condenser is a partition heat exchanger; the number of the absorption tanks is at least 2, connected in series.

[0040] The carrier gas source is connected to the lower feed pipeline of the preheating furnace 8 through the filter 1, the ball valve 2, the pressure reducing valve 3, the flow meter 4, the check valve 5 in sequence;

[0041] A pressure gauge 6 is provided on the pipeline between the ball valve 2 and the pressure reducing valve 3;

[0042] A ball valve and a branch pipeline consisting of two ball valves and a flow meter 4 therebetween are provided on the pipeline between the pressure reducing valve 3 and the check valve 5, and the branch pipeline is connected in parallel with the pipeline with a ball valve;

[0043] Isobutyric anhydride (IBAN) or a mixture of IBAN and isobutyric acid (IBA) (IBA) is connected to the lower feed pipeline of the preheating furnace 8 through a filter, a ball valve, a metering pump 7, a ball valve, and a check valve in sequence;

[0044] A pressure gauge is provided on the pipeline between the metering pump 7 and the ball valve;

[0045] The material outlet at the top of the preheating furnace 8 is connected to the material inlet at the top of the high-temperature cracking furnace 10, and the material outlet at the bottom of the high-temperature cracking furnace 10 is connected to the material inlet at the top of the gas-liquid separation tank 12 through the condenser 11;

[0046] A gas outlet is provided at the top of the gas-liquid separation tank 12, and the gas outlet is connected to the material inlet of the absorption tank 14 through a ball valve. A gas outlet is provided at the top of the absorption tank 14, and the gas outlet is connected to the material inlet of the second absorption tank through a ball valve. A gas outlet is provided at the top of the second absorption tank, and the gas outlet is connected to the atmosphere through a ball valve.

[0047] A pressure gauge is provided on the pipeline between the material outlet at the upper part of the preheating furnace 8 and the material inlet at the top of the high-temperature cracking furnace 10;

[0048] A material outlet with a needle valve 13 is provided at the bottom of the gas-liquid separation tank 12;

[0049] A material outlet with a second needle valve is provided at the bottom of the absorption tank 14;

[0050] A material outlet with a third needle valve is provided at the bottom of the second absorption tank; the filter adopts a 22 series straight-through filter produced by Xiongchuan Valve Company;

[0051] A temperature controller 9 is provided on the preheating furnace 8, and the temperature in the preheating furnace 8 is regulated by the temperature controller 9 by controlling the preheating tube (electric heating tube) therein;

[0052] A temperature controller is provided on the high temperature cracking furnace 10, and the temperature inside is regulated by controlling the electric heating element therein through the temperature controller;

[0053] The high temperature cracking furnace is provided with a cracking reactor made of a quartz tube;

[0054] The condenser is a partition type heat exchanger;

[0055] There are two absorption tanks, which are connected in series.

[0056] The reaction process of cracking IBAN or IBAN+IBA mixture to produce DMK is as follows:

[0057] (1) IBAN or a mixture of IBAN and IBA is mixed with an inert carrier gas as a liquid raw material and then introduced into a preheating furnace for gasification. The feed rate of the liquid raw material is 0.1 to 20 ml / min. The inert carrier gas is one or more of N2, He, Ar, H2, CH4, CO or CO2, and the gas flow rate is 50 ml / min to 5 L / min.

[0058] (2) The inner diameter of the preheating furnace is Φ20 mm, the total height of the furnace is 300 mm, the power is 1.2 kW, a stainless steel preheating tube with an inner diameter of Φ10 mm is placed in the preheating furnace, the working temperature range of the preheating furnace is 100 to 800° C., and the preferred working temperature range is 180 to 350° C.;

[0059] (3) The mixed material gasified in the preheating furnace enters the high-temperature cracking furnace, the high-temperature cracking furnace has an inner diameter of Φ20 mm, a total furnace height of 380 mm, and a power of 1.2 kW. A quartz reaction tube with an outer diameter of Φ14 mm and an inner diameter of Φ10 mm is placed in the high-temperature cracking furnace. The operating temperature range of the high-temperature cracking furnace is 100 to 800° C., preferably 200 to 550° C. A catalyst bed with a height of 0.5 to 5 cm is added in the constant temperature section, and the residence time of the mixed material on the catalyst bed is 0.01 s to 5 s;

[0060] (4) The cracked product is passed into a condenser for rapid cooling, and then into a gas-liquid separation tank for gas-liquid separation. A DLK-1010 rapid low-temperature cooling circulation pump produced by Ningbo Xinzhi Biotechnology Co., Ltd. is used to provide cooling medium for the condenser and the gas-liquid separation tank. The cooling medium is a Biaobang brand antifreeze liquid, which is composed of ethylene glycol diluent (freezing point -25°C), and the cooling temperature is 0 to -10°C. The condensate containing IBAN and IBA collected in the gas-liquid separation tank can be used as a cracking reaction raw material to replace part or all of the liquid raw materials and passed into the preheating furnace for gasification;

[0061] (5) The gaseous DMK product is drawn out from the top of the gas-liquid separation tank and introduced into the first absorption tank containing 50-1000 ml of ester absorbent through a bottom-inserted tube to absorb the DMK. The ester absorbent includes but is not limited to one or more of methyl isobutyrate, ethyl isobutyrate, isobutyl isobutyrate, butyl acetate or isopropyl acetate. A DLK-1010 type rapid low-temperature cooling circulation pump is used to provide cooling medium for the absorption tank. The cooling medium is a Biaobang brand antifreeze liquid, which is a glycol-type diluent (freezing point -25°C). The absorption temperature of the absorption tank is RT to -10°C.

[0062] (6) The gaseous DMK product after primary absorption is drawn out from the top of the first absorption tank and introduced into the second absorption tank containing 50-1000 ml of ester absorbent through a bottom tube for secondary absorption of DMK. The ester absorbent and absorption temperature are the same as those of the first absorption tank.

[0063] (7) mixing the ester absorption liquid after absorbing DMK in the first absorption tank and the second absorption tank and pouring them into a high-pressure reactor, polymerizing for 1 to 24 hours (preferably 2 to 12 hours) at 50 to 150° C. (preferably 50 to 100° C.) and 0.1 to 3.0 MPa (preferably 0.1 to 1.0 MPa) to obtain an ester solution containing TMCD;

[0064] The ester absorbent can be recovered by distillation to obtain a crude TMCD product. Repeating the above distillation process can reduce the impurity content and improve the purity of the TMCD product.

[0065] Example 1

[0066] a. Preparation of (SiO2+MgO) / HZSM-5 catalyst

[0067] (1) 50 g NaZSM-5, 20 g pseudo-boehmite, 5 g sesbania powder and 20 ml of 10% dilute nitric acid solution were mixed uniformly;

[0068] (2) drying the extruded NaZSM-5 catalyst obtained in step (1) in an oven at 90° C. for 12 h, and calcining in a muffle furnace at 550° C. for 4 h to obtain a shaped NaZSM-5 catalyst;

[0069] (3) the NaZSM-5 catalyst obtained in step (2) was ion exchanged three times at a solid-liquid ratio of 1:10 with a 0.5 mol / L NH4NO3 solution (immersion treatment) at 70°C, each exchange lasting 3 hours;

[0070] (4) drying the ammonium ZSM-5 catalyst obtained in step (3) in an oven at 90° C. for 12 h, and calcining in a muffle furnace at 550° C. for 4 h to obtain a HZSM-5 catalyst;

[0071] (5) 10 g of HZSM-5 catalyst was immersed in a cyclohexane solution of tetraethyl orthosilicate, the amount of tetraethyl orthosilicate added was calculated based on the amount of SiO2 finally decomposed, the amount of SiO2 deposited accounted for 10 wt% of the total mass of the catalyst, and after sealing and dipping for 12 h, the mixture was dried in the shade at room temperature, and calcined at 550° C. for 4 h to obtain a SiO2 / HZSM-5 catalyst;

[0072] (6) The SiO2 / HZSM-5 catalyst obtained in step (5) is immersed in an aqueous solution of magnesium acetate, wherein the amount of magnesium acetate added is calculated based on the amount of MgO finally decomposed, and the deposition amount of MgO accounts for 5wt% of the total mass of the catalyst. After being immersed at room temperature for 12 hours, the catalyst is dried in an oven at 90°C for 12 hours, and calcined in a muffle furnace at 550°C for 6 hours to obtain a (SiO2+MgO) / HZSM-5 catalyst.

[0073] b. Using (SiO2+MgO) / HZSM-5 catalyst to crack IBAN to prepare DMK and further dimerize to synthesize TMCD

[0074] (1) 5 g (SiO2+MgO) / HZSM-5 catalyst was loaded into the constant temperature section of the cracking reaction tube and heated to 480° C. by N2;

[0075] (2) The IBAN liquid was mixed with N2 by a metering pump and then introduced into a preheating furnace. The IBAN feed rate was 5.0 ml / min, N2 was used as the carrier gas, the N2 flow rate was 500 ml / min, and the preheating furnace temperature was 320 °C;

[0076] The mixed material gasified in the preheating furnace enters the high-temperature cracking furnace. The operating temperature range of the high-temperature cracking furnace is 480°C, the catalyst bed height is about 4cm, and the residence time of the mixed material on the catalyst bed is 0.2s;

[0077] (3) The cracked product is passed into a condenser for quenching, and then passed into a gas-liquid separation tank for gas-liquid separation. The cooling temperature is -10°C. The composition of the condensate collected in the gas-liquid separation tank is analyzed by gas chromatography. The IBAN conversion rate is calculated based on the composition of the condensate. The results are shown in Appendix 1. The condensate containing IBAN and IBA collected in the gas-liquid separation tank can be used as a cracking reaction raw material to replace part or all of the liquid raw materials and passed into the preheating furnace for gasification.

[0078] (4) The gaseous DMK product was drawn out from the top of the gas-liquid separation tank, and a sampling port was set. The gas phase product composition was analyzed online by gas chromatography, and the DMK product composition was identified by GC-MS using air bag sampling. The product was mostly DMK, containing a small amount of propylene, acetone, 2,3-dimethyl-2-butene, 2,4-dimethylpentadiene, CO and CO2. The DMK selectivity in the gas phase organic product was listed in Appendix 1. The DMK was absorbed by the absorption tank 1 containing 100 ml of methyl isobutyrate using a bottom tube, and the absorption temperature of the absorption tank was -10°C;

[0079] (5) The tail gas after primary absorption is drawn out from the top of absorption tank 1 and introduced into absorption tank 2 containing 100 ml of absorbent by using a bottom-inserted tube for secondary absorption of DMK. The ester absorbent and absorption temperature are the same as those in step (4);

[0080] (6) After absorbing for 5 hours, the light yellow ester absorption liquid after absorbing DMK in absorption tank 1 and absorption tank 2 was mixed, and 50 ml was poured into a 100 ml stainless steel high-pressure reactor lined with polytetrafluoroethylene. After sealing, the gas in the reactor was replaced with N2 three times. Polymerization was carried out at 100°C and 0.3 MPa for 5 hours to obtain a colorless solution of methyl isobutyrate containing TMCD, indicating that DMK has been completely converted. The TMCD concentration in the solution was analyzed by gas chromatography, and the TMCD structure was identified by GC-MS. The TMCD concentration in the sample is listed in Appendix 1.

[0081] Example 2

[0082] a. Preparation of (SiO2+La2O3) / HZSM-5 catalyst

[0083] Steps (1) to (5) of the catalyst preparation method in this embodiment are similar to those in Example 1a (meaning the process and conditions are the same, the same below), except for step (6);

[0084] (6) 10 g of SiO2 / HZSM-5 catalyst was immersed in an aqueous solution of lanthanum nitrate. The amount of lanthanum nitrate added was calculated based on the amount of La2O3 that was finally decomposed. The deposition amount of La2O3 accounted for 10 wt% of the total mass of the catalyst. After being immersed at room temperature for 12 h, the catalyst was dried in an oven at 90°C for 12 h and calcined in a muffle furnace at 550°C for 6 h to obtain a (SiO2+La2O3) / HZSM-5 catalyst.

[0085] b. Using (SiO2+La2O3) / HZSM-5 catalyst to crack IBAN to prepare DMK and further dimerize to synthesize TMCD

[0086] (1) 5 g (SiO2+La2O3) / HZSM-5 catalyst was loaded into the constant temperature section of the cracking reaction tube, and N2 was passed through to raise the temperature to 480°C;

[0087] (2) IBAN liquid was mixed with N2 by a metering pump and then introduced into a preheating furnace, the IBAN feed rate was 8.0 ml / min, N2 was used as a carrier gas, the N2 flow rate was 800 ml / min, and the preheating furnace temperature was 320° C. The mixed material gasified in the preheating furnace entered a high-temperature cracking furnace, the operating temperature range of the high-temperature cracking furnace was 480° C., the catalyst bed height was about 4 cm, and the residence time of the mixed material on the catalyst bed was 0.12 s;

[0088] (3) The cracked product is passed into a condenser for quenching, and then passed into a gas-liquid separation tank for gas-liquid separation. The cooling temperature is -10°C. The composition of the condensate collected in the gas-liquid separation tank is analyzed by gas chromatography. The IBAN conversion rate is calculated based on the composition of the condensate. The results are shown in Appendix 1. The condensate containing IBAN and IBA collected in the gas-liquid separation tank can be used as a cracking reaction raw material to replace part or all of the liquid raw materials and passed into the preheating furnace for gasification.

[0089] (4) The gaseous DMK product was drawn out from the top of the gas-liquid separation tank, a sampling port was set, and the composition of the gas phase product was analyzed online by gas chromatography. The DMK selectivity in the gas phase organic product is listed in Appendix 1. The DMK was introduced into the absorption tank 1 containing 100 ml of ethyl isobutyrate by using a bottom tube to absorb the DMK. The absorption temperature of the absorption tank was -10°C.

[0090] (5) The tail gas after primary absorption is drawn out from the top of absorption tank 1 and introduced into absorption tank 2 containing 100 ml of absorbent by using a bottom-inserted tube for secondary absorption of DMK. The ester absorbent and absorption temperature are the same as those in step (4);

[0091] (6) After absorbing for 6 hours, the pale yellow ester absorption liquid after absorbing DMK in absorption tank 1 and absorption tank 2 was mixed, and 50 ml was poured into a 100 ml stainless steel high-pressure reactor lined with polytetrafluoroethylene. After sealing, the gas in the reactor was replaced with N2 three times. Polymerization was carried out at 80°C and 0.3MP for 12 hours to obtain a colorless solution of ethyl isobutyrate containing TMCD, indicating that DMK has been completely converted. The TMCD concentration in the solution was analyzed by gas chromatography, and the TMCD structure was identified by GC-MS. The TMCD concentration in the sample is listed in Appendix 1.

[0092] Example 3

[0093] a. Preparation of (P2O5+MgO) / HZSM-5 catalyst

[0094] Steps (1) to (4) of the catalyst preparation method in this embodiment are similar to those in Example 1a, except for steps (5) and (6);

[0095] (5) 10 g of HZSM-5 catalyst was immersed in an aqueous solution of ammonium dihydrogen phosphate, the amount of ammonium dihydrogen phosphate added was calculated based on the amount of P2O5 finally decomposed, the amount of P2O5 deposited accounted for 15 wt% of the total mass of the catalyst, after being immersed at room temperature for 12 h, it was dried in an oven at 90° C. for 12 h, and calcined at 550° C. for 4 h to obtain a P2O5 / HZSM-5 catalyst;

[0096] (6) The P2O5 / HZSM-5 catalyst obtained in step (5) is immersed in an aqueous solution of magnesium acetate, wherein the amount of magnesium acetate added is calculated based on the amount of MgO finally decomposed, and the deposition amount of MgO accounts for 5wt% of the total mass of the catalyst. After being immersed at room temperature for 12 hours, the catalyst is dried in an oven at 90°C for 12 hours, and calcined in a muffle furnace at 550°C for 6 hours to obtain a (P2O5+MgO) / HZSM-5 catalyst.

[0097] b. Using (P2O5+MgO) / HZSM-5 catalyst to crack the mixture of IBAN and IBA to prepare DMK and further dimerize to synthesize TMCD

[0098] (1) 5 g (P2O5+MgO) / HZSM-5 catalyst was loaded into the constant temperature section of the cracking reaction tube, and N2 was passed through to raise the temperature to 480°C;

[0099] (2) A mixed liquid of IBAN and IBA was mixed with N2 by a metering pump and then introduced into a preheating furnace, wherein the mixed liquid composition was 80 mol% IBAN and 20 mol% IBA, the liquid feed rate was 5.0 ml / min, N2 was used as a carrier gas, the N2 flow rate was 500 ml / min, and the preheating furnace temperature was 320° C. The mixed material gasified in the preheating furnace entered a high-temperature cracking furnace, the operating temperature range of the high-temperature cracking furnace was 480° C., the catalyst bed height was about 4 cm, and the residence time of the mixed material on the catalyst bed was 0.2 s;

[0100] (3) The cracked product is passed into a condenser for quenching, and then passed into a gas-liquid separation tank for gas-liquid separation. The cooling temperature is 0° C. The composition of the condensate collected in the gas-liquid separation tank is analyzed by gas chromatography. The IBAN conversion rate is calculated based on the composition of the condensate. The results are shown in Appendix 1. The condensate containing IBAN and IBA collected in the gas-liquid separation tank can be used as a cracking reaction raw material to replace part or all of the liquid raw materials and passed into the preheating furnace for gasification.

[0101] (4) The gaseous DMK product was drawn out from the top of the gas-liquid separation tank, a sampling port was set, and the composition of the gas phase product was analyzed online by gas chromatography. The DMK selectivity in the gas phase organic product is listed in Appendix 1. The DMK was introduced into the absorption tank 1 containing 100 ml of isobutyl isobutyrate by using a bottom tube to absorb the DMK. The absorption temperature of the absorption tank was 0°C.

[0102] (5) The tail gas after primary absorption is drawn out from the top of absorption tank 1 and introduced into absorption tank 2 containing 100 ml of absorbent by using a bottom-inserted tube for secondary absorption of DMK. The ester absorbent and absorption temperature are the same as those in step (4);

[0103] (6) After absorbing for 6 hours, the light yellow ester absorption liquid after absorbing DMK in absorption tank 1 and absorption tank 2 was mixed, and 50 ml was poured into a 100 ml stainless steel high-pressure reactor lined with polytetrafluoroethylene. After sealing, the gas in the reactor was replaced with N2 three times. Polymerization was carried out at 120°C and 0.5MP for 5 hours to obtain a colorless solution of isobutyl isobutyrate containing TMCD, indicating that DMK has been completely converted. The TMCD concentration in the solution was analyzed by gas chromatography, and the TMCD structure was identified by GC-MS. The TMCD concentration in the sample is listed in Appendix 1.

[0104] Example 4

[0105] a. Preparation of (B2O3+CeO2) / HZSM-5 catalyst

[0106] Steps (1) to (4) of the catalyst preparation method in this embodiment are similar to those in Example 1a, except for steps (5) and (6);

[0107] (5) 10 g of HZSM-5 catalyst was immersed in an aqueous solution of boric acid. The amount of boric acid added was calculated based on the amount of B2O3 finally decomposed. The amount of B2O3 deposited accounted for 15 wt% of the total mass of the catalyst. After immersion at room temperature for 12 h, the catalyst was dried in an oven at 90° C. for 12 h, and calcined at 550° C. for 4 h to obtain a B2O3 / HZSM-5 catalyst.

[0108] (6) The B2O3 / HZSM-5 catalyst obtained in step (5) is immersed in an aqueous solution of cerium nitrate, wherein the amount of cerium nitrate added is calculated based on the amount of CeO2 that is finally decomposed, and the deposition amount of CeO2 accounts for 10wt% of the total mass of the catalyst. After being immersed at room temperature for 12 hours, the catalyst is dried in an oven at 90°C for 12 hours, and calcined in a muffle furnace at 550°C for 6 hours to obtain a (B2O3+CeO2) / HZSM-5 catalyst.

[0109] b. Using (B2O3+CeO2) / HZSM-5 catalyst to crack the mixture of IBAN and IBA to prepare DMK and further dimerize to synthesize TMCD

[0110] The steps in this example are similar to those in Example 3b, except that in step (1), a (B2O3+CeO2) / HZSM-5 catalyst is used to crack the mixture of IBAN and IBA. The main experimental results are listed in Appendix 1.

[0111] Example 5

[0112] a. Preparation of (SiO2+MgO) / HNaX catalyst

[0113] (1) 50 g of NaX molecular sieve, 20 g of pseudo-boehmite, 5 g of sesbania powder, and 20 ml of a 10% dilute nitric acid solution were mixed evenly;

[0114] (2) drying the extruded NaX catalyst obtained in step (1) in an oven at 90° C. for 12 h, and calcining in a muffle furnace at 550° C. for 4 h to obtain a shaped NaX catalyst;

[0115] (3) The NaX catalyst obtained in step (2) was ion exchanged three times with a 0.2 mol / L NH4NO3 solution at a solid-liquid ratio of 1:1.5 at room temperature, each exchange lasting 3 hours;

[0116] (4) drying the partially ammonium-exchanged NaX catalyst obtained in step (3) in an oven at 90° C. for 12 h, and calcining at 550° C. for 4 h to obtain an HNaX catalyst;

[0117] In steps (5) and (6), the HNaX catalyst is modified by the same method as in step a of Example 1 to obtain a (SiO2+MgO) / HNaX catalyst.

[0118] b. Using (SiO2+MgO) / HNaX catalyst to crack IBAN to prepare DMK and further dimerize to synthesize TMCD

[0119] The steps in this section are similar to those in Example 1b, except that (SiO2+MgO) / HNaX catalyst is used to crack IBAN in step (1). The main experimental results are listed in Appendix 1.

[0120] Example 6

[0121] a. Preparation of (SiO2+MgO) / HNaY catalyst

[0122] (1) 50 g of NaY molecular sieve, 20 g of pseudo-boehmite, 5 g of sesbania powder and 20 ml of a 10% dilute nitric acid solution were mixed uniformly;

[0123] (2) drying the extruded NaY catalyst obtained in step (1) in an oven at 90° C. for 12 h, and calcining in a muffle furnace at 550° C. for 4 h to obtain a shaped NaY catalyst;

[0124] (3) The NaY catalyst obtained in step (2) was ion exchanged three times at 50° C. with a 0.5 mol / L NH 4 NO 3 solution at a solid-liquid ratio of 1:5, each exchange lasting 3 hours;

[0125] (4) drying the partially ammonium-exchanged NaY catalyst obtained in step (3) in an oven at 90° C. for 12 h, and calcining at 550° C. for 4 h to obtain an HNaY catalyst;

[0126] In steps (5) and (6), the HNaY catalyst is modified by the same method as in step a of Example 1 to obtain a (SiO2+MgO) / HNaY catalyst.

[0127] b. Using (SiO2+MgO) / HNaY catalyst to crack IBAN to prepare DMK and further dimerize to synthesize TMCD

[0128] The steps in this section are similar to those in Example 1b, except that (SiO2+MgO) / HNaY catalyst is used in step (1) to crack IBAN. The main experimental results are listed in Appendix 1.

[0129] Example 7

[0130] a. Preparation of (SiO2+MgO) / USY catalyst

[0131] (1) 50 g of ultrastable Y (USY) molecular sieve, 20 g of pseudo-boehmite, 5 g of sesbania powder and 20 ml of a 10% dilute nitric acid solution were mixed uniformly;

[0132] (2) drying the extruded USY catalyst obtained in step (1) in an oven at 90° C. for 12 h, and calcining in a muffle furnace at 550° C. for 4 h to obtain a shaped USY catalyst. Since USY is H-type, ammonium exchange is not required;

[0133] (3) The same as step (5) in Example 1, to obtain SiO2 / USY catalyst;

[0134] (4) The same as step (6) in Example 1, to obtain a (SiO2+MgO) / USY catalyst;

[0135] b. Using (SiO2+MgO) / USY catalyst to crack IBAN to prepare DMK and further dimerize to synthesize TMCD

[0136] The steps in this section are similar to those in Example 1b, except that (SiO2+MgO) / USY catalyst is used in step (1) to crack IBAN. The main experimental results are listed in Appendix 1.

[0137] Example 8

[0138] The catalyst used in this section is the (SiO2+MgO) / HZSM-5 catalyst provided in Example 1.

[0139] In this part, (SiO2+MgO) / HZSM-5 catalyst was used to crack the mixture of IBAN and IBA to prepare DMK and further dimerize to synthesize TMCD. The composition of the mixed liquid of IBAN and IBA was 80 mol% IBAN and 20 mol% IBA. The steps were the same as step b in Example 3 (referring to the same process and conditions, the same below). The main experimental results are listed in Appendix 1.

[0140] Example 9

[0141] The catalyst used in this section is the (SiO2+MgO) / HZSM-5 catalyst provided in Example 1.

[0142] In this part, (SiO2+MgO) / HZSM-5 catalyst was used to crack the mixture of IBAN and IBA to prepare DMK and further dimerize to synthesize TMCD. The composition of the mixed liquid of IBAN and IBA was 50 mol% IBAN and 50 mol% IBA. The steps were the same as those in step b of Example 3. The main experimental results are listed in Appendix 1.

[0143] Example 10

[0144] This part mainly investigates the reaction performance of IBAN cracking to prepare DMK using only pure silicon Silicalite-1 molecular sieve as catalyst.

[0145] a. Preparation of Silicalite-1 Catalyst

[0146] (1) 50 g of commercially available Silicalite-1 molecular sieve, 20 g of pseudo-boehmite, 5 g of sesbania powder and 20 ml of 30 wt % silica sol were mixed uniformly;

[0147] (2) drying the extruded Silicalite-1 catalyst obtained in step (1) in an oven at 90° C. for 12 h, and calcining in a muffle furnace at 550° C. for 4 h to obtain a formed Silicalite-1 catalyst;

[0148] b. Using Silicalite-1 catalyst to crack IBAN to prepare DMK and further dimerize to synthesize TMCD

[0149] The steps of the IBAN cracking and DMK absorption process are similar to the steps b in Example 1, except that Silicalite-1 is added as a catalyst in the cracking reaction tube in step (1). The results are listed in Appendix 1.

[0150] Embodiment 11

[0151] This section mainly examines the effect of the feed mode of replacing IBAN or IBAN+IBA with pure IBA on the catalyst performance. The catalyst used in this section is the (SiO2+MgO) / HZSM-5 catalyst provided in Example 1. This section uses the (SiO2+MgO) / HZSM-5 catalyst to crack IBA to prepare DMK and further dimerize to synthesize TMCD. The steps are the same as the steps b in Example 1, except that pure IBA is used to replace the feed of IBAN or IBAN+IBA. The main experimental results are listed in Appendix 1.

[0152] Comparative Example 1

[0153] This section mainly examines the experimental results of using IBAN as a cracking reactant to prepare DMK and further dimerize to synthesize TMCD under the condition of no filler or catalyst. The steps are similar to the steps b in Example 1, except that no filler or catalyst is loaded in step (1). The results are listed in Appendix 2.

[0154] Comparative Example 2

[0155] This section mainly examines the experimental results of preparing DMK and further dimerizing TMCD in the absence of a catalyst by using only commercially purchased cylindrical ceramic Raschig rings with an outer diameter of 6 mm as thermal conductive fillers and using IBAN as a cracking reactant. The steps are similar to the steps b in Example 1, except that in step (1), only ceramic Raschig rings are loaded as fillers without any catalyst. The results are listed in Appendix 2.

[0156] Comparative Example 3

[0157] This section mainly examines the experimental results of preparing DMK and further dimerizing TMCD under catalyst-free conditions by using a commercially purchased metal Zr material θ mesh ring filler with an outer diameter of about 3 mm as a thermal conductive filler and IBAN as a cracking reactant. The steps are similar to the steps b in Example 1, except that in step (1), only Zr material mesh rings are loaded as fillers without any catalyst. The results are listed in Appendix 2.

[0158] Comparative Example 4

[0159] This section mainly examines the experimental results of preparing DMK and further dimerizing TMCD by using a commercially purchased 316L stainless steel θ mesh ring filler as a thermal conductive filler and IBAN as a cracking reactant under catalyst-free conditions. The steps are similar to the steps b in Example 1, except that in step (1), only the 316L stainless steel mesh ring is loaded as a filler without any catalyst. The results are listed in Appendix 2.

[0160] Comparative Example 5

[0161] This section mainly investigates the reaction performance of unmodified HZSM-5 as a catalyst for catalyzing the cracking of IBAN to prepare DMK, and further investigates the experimental results of dimerization of the DMK produced by cracking as an intermediate to synthesize TMCD. The steps are similar to the steps b in Example 1, except that in step (1), 5 g of unmodified HZSM-5 is loaded as a catalyst in the cracking reaction tube. The results are listed in Appendix 2.

[0162] Comparative Example 6

[0163] This section mainly investigates the reaction performance of HZSM-5 modified with SiO2 as the catalyst to catalyze the cracking of IBAN to prepare DMK, and further investigates the experimental results of dimerization of the DMK produced by cracking to synthesize TMCD as an intermediate. The steps of preparing the catalyst are completely consistent with steps (1) to (5) in Example 1. The steps of the cracking of IBAN and absorption of DMK are similar to the steps in Example 1b, except that 5g of SiO2 / HZSM-5 is loaded as the catalyst in the cracking reaction tube in step (1). The results are listed in Appendix 2.

[0164] Table 1 Performance of different catalysts in the cracking of IBAN and IBA to prepare DMK and dimerize to synthesize TMCD

[0165]

[0166] Table 2 Comparison of catalyst performance in the cracking of IBAN and IBA to prepare DMK and dimerize to synthesize TMCD

[0167]

[0168] Unless otherwise specified, the cracking reaction conditions were: preheating temperature 320°C, cracking temperature 480°C, normal pressure, liquid flow rate 5.0 ml / min, N2 flow rate 500 ml / min, and sampling time 5 h.

[0169] From the results of Example 1 and Example 2 in Table 1, it can be seen that when pure IBAN is used as the cracking raw material, (SiO2+MgO) / HZSM-5 is used as the catalyst, the conversion rate of IBAN reaches 15.9%, the DMK selectivity in the gaseous product after cracking reaches up to 98.6%, and the TMCD product concentration in the ester absorbent after absorption and polymerization reaches up to 9.5%. When (SiO2+La2O3) / HZSM-5 is used as the catalyst, the conversion rate of IBAN drops to 9.9%, the DMK selectivity in the gaseous product after cracking decreases slightly to 88.2%, and the TMCD product concentration in the ester absorbent is 8.5%. It shows that in the present invention, both alkaline earth metal oxides and rare earth metal oxides can effectively modify molecular sieve catalysts to obtain highly selective DMK products.

[0170] From the results of Example 5, Example 6 and Example 7 in Table 1, it can be seen that when NaX, NaY and USY molecular sieves of the FAU family are used as catalysts, the modified molecular sieve method completely consistent with that of Example 1 can also catalyze the cracking reaction of IBAN to produce DMK, and the selectivity of DMK in the gaseous product is 80.1%, 80.2% and 87.1%, respectively, and the concentration of TMCD product in the ester absorbent is 5.1%, 6.5% and 6.9%, respectively. The above results show that the method of modifying the molecular sieve catalyst with non-metallic oxides and metal oxides has good universality, and can flexibly regulate the acid amount and acid strength of the molecular sieve catalyst to achieve the purpose of catalyzing the cracking of IBAN to produce DMK without generating other byproducts.

[0171] From the results of Example 3, Example 4 and Example 8 in Table 1, it can be seen that when a mixture of 80 mol% IBAN and 20 mol% IBA is used as the cracking raw material, (P2O5+MgO) / HZSM-5, (B2O3+CeO2) / HZSM-5 and (SiO2+MgO) / HZSM-5 can be used as catalysts to catalyze the cracking reaction of IBAN and IBA to produce DMK, and the selectivity of DMK in the gaseous product is 94.2%, 93.6% and 94.1%, respectively, and the concentration of TMCD product in the ester absorbent is 8.6%, 5.3% and 7.5%, respectively. The above results show that, on the one hand, the molecular sieve catalyst modified by a variety of different combinations of non-metallic oxides and metal oxides can be adapted to the case where the IBAN raw material contains some IBA, and the catalyst modification method has a good application prospect; on the other hand, the yield of the DMK product can be improved by passing the condensate of the primary cracking reaction as a raw material into the reactor for secondary or multiple cracking.

[0172] From the results of Example 9 in Table 1, it can be seen that when 50 mol% IBAN and 50 mol% IBA are used as cracking raw materials, (SiO2+MgO) / HZSM-5 can catalyze the cracking reaction of IBAN+IBA to prepare DMK and further dimerize to synthesize TMCD. In this reaction, more low-carbon hydrocarbon by-products are generated, resulting in a DMK selectivity of 65.1%, which is lower than that when IBAN is used as a reactant. There is 5.3% TMCD in the product, indicating that the molecular sieve catalyst modified by non-metallic oxides and metal oxides has good adaptability to the raw material composition.

[0173] From the results of Example 10 in Table 1, it can be seen that when pure silicon Silicalite-1 is used as a catalyst, under the same cracking reaction and absorption experimental conditions as in Example 1, the IBAN conversion rate reaches 7.8%, the DMK selectivity reaches 82.8%, and the TMCD concentration in the final product is 6.5%, indicating that the weak acid centers such as silanol or silanests of the Silicalite-1 molecular sieve can also promote the cracking of IBAN and IBA to prepare DMK.

[0174] It can be seen from the results of Example 11 in Table 1 that when pure IBA is used instead of IBAN or IBAN+IBA as feed and (SiO2+MgO) / HZSM-5 catalyst is used, the IBA conversion rate is 2.7% and the DMK selectivity is 25.1%. Due to the poor DMK selectivity, the TMCD concentration in the product is 1.5%.

[0175] From the results of Comparative Example 1 in Table 2, it can be seen that, without filler or catalyst, only 3.7% of IBAN can be converted by thermal cracking alone, resulting in a decrease in the selectivity of DMK in the gas phase product to 55.1%. Under the same cracking reaction and absorption experimental conditions as Example 1, the TMCD concentration in the product decreased from 9.5% to 2.1%. This shows that the catalytic cracking method is better than the thermal cracking method alone.

[0176] From the results of Comparative Example 2 in Table 2, it can be seen that under the same cracking reaction and absorption experimental conditions as Example 1, the cracking efficiency of IBAN is not as good as that of (SiO2+MgO) / HZSM-5 catalyst, and the concentration of TMCD in the final product is 1.3%; this result is also lower than the corresponding results after using the catalyst in Examples 2, 3 and 4. It shows that the effect of using the molecular sieve catalyst modified by non-metallic oxides and metal oxides to crack IBAN and IBAN+IBA mixture to prepare DMK is better than that of using ceramic fillers.

[0177] From the results of Comparative Examples 3 and 4 in Table 2, it can be seen that under the same cracking reaction and absorption experimental conditions as Example 1, the cracking conversion rate of IBAN is still low at 4.9%, and the DMK selectivity in the gas phase product is 44.1% and 17.0%, respectively. The TMCD concentrations in the final products are 1.8% and 0.8%, respectively. This indicates that metal fillers may promote the decomposition of DMK into olefins, carbon oxides or acetone, etc., reducing the DMK yield in the final product.

[0178] From the results of Comparative Example 5 in Table 2, it can be seen that under the same cracking reaction and absorption experimental conditions as Example 1, although the IBAN conversion rate is as high as 9.3%, the selectivity of DMK is only 0.2%, indicating that the unmodified HZSM-5 has too strong acidity, which causes deep cracking of IBAN, affecting the yield of DMK products, and making it impossible to detect DMK or TMCD in the final absorption liquid. Based on the results of Example 1 and Comparative Example 5, the molecular sieve catalyst should have appropriate acidity, and deep cracking is prone to occur when the acidity is too strong.

[0179] From the results of Comparative Example 6 in Table 2, it can be seen that under the same cracking reaction and absorption experimental conditions as Example 1, the selectivity of DMK is 35.1%, which is higher than that of Comparative Example 5 but lower than that of Example 1, and also affects the yield of DMK product, resulting in a TMCD concentration of 1.5% in the final product. Based on the results of Example 1, Comparative Example 5 and Comparative Example 6, the synergistic modification of non-metallic oxides and metal oxides is necessary, which helps to further improve the cracking reaction selectivity of the molecular sieve catalyst.

Claims

1. A method for preparing a molecular sieve catalyst, characterized in that: Including non-metal and metal oxide modified molecular sieve catalysts or pure silicon Silicalite-1 shaped molecular sieve catalysts The process is as follows, (1) mixing one or more of MFI (NaZSM-5 or pure silicon Silicalite-1) or FAU (NaX, NaY or USY) molecular sieves with pseudo-boehmite and sesbania powder, and adding a dilute nitric acid solution with a mass fraction of 10 to 20 wt% during the mixing process, wherein the mass ratio of the molecular sieve, pseudo-boehmite, sesbania powder and dilute nitric acid is 1 to 20: 0.1 to 6: 0.1 to 5: 1 to 10 (preferably 5 to 10: 2 to 5: 0.1 to 2: 1 to 8, more preferably 10: 3 to 5: 1: 2 to 5); obtaining a wet material; (2) the wet materials obtained in step (1) are mixed uniformly and then extruded into strips, dried at 80-120° C. (preferably 90-100° C.) for 1-24 h (preferably 12-24 h), and calcined in air at 300-600° C. (preferably 450-550° C., more preferably 500-540° C.) for 1-12 h (preferably 4-8 h, more preferably 4 h) to obtain a Na-type shaped molecular sieve catalyst; (3) the Na-type shaped molecular sieve catalyst obtained in step (2) is ion exchanged 1-5 times at a solid-liquid ratio of 1:1.5-1:20 (preferably 1:5-1:15, more preferably 1:10) with a 0.1-2.0 mol / L NH4NO3 solution at RT (room temperature) to 90°C, each exchange lasting 0.5-5h (preferably 1-4h, more preferably 3h); (4) drying the ion-exchanged catalyst obtained in step (3) at 80-120° C. (preferably 90-100° C.) for 1-24 h (preferably 12-24 h), and calcining at 300-600° C. (preferably 450-550° C., more preferably 500-540° C.) for 1-12 h (preferably 4-8 h, more preferably 4 h) to obtain an H-type shaped molecular sieve catalyst; (5) modifying the H-type molecular sieve catalyst obtained in step (4) with a non-metallic oxide, wherein the non-metallic oxide includes but is not limited to one or more of SiO2, P2O5 and B2O3, and the modification amount of the non-metallic oxide accounts for 1 to 30 wt% (preferably 5 to 20 wt%, more preferably 5 to 10 wt%) of the total mass of the catalyst after the non-metallic oxide modification; The specific process is: immersing the catalyst into a solution containing a non-metallic oxide precursor by an impregnation method, sealing for 12 to 24 hours and then drying in the shade at room temperature, and calcining at a temperature of 300 to 600° C. (preferably 450 to 550° C., more preferably 500 to 540° C.) for 4 to 12 hours (preferably 4 to 8 hours, more preferably 4 hours); (6) modifying the non-metallic oxide-modified molecular sieve catalyst with a metal oxide, wherein the metal oxide includes but is not limited to one or more of alkaline earth metal MgO and rare earth metal La2O3, CeO2, etc., and the modification amount of the metal oxide accounts for 1 to 30 wt% (preferably 5 to 20 wt%, more preferably 5 to 10 wt%) of the total mass of the catalyst after the metal oxide modification; The specific process is: the catalyst modified by the non-metallic oxide is immersed in a solution containing a metal oxide precursor by an impregnation method at room temperature for 12 to 24 hours, and then dried at 80 to 120° C. for 12 hours, and calcined in a muffle furnace at a temperature of 300 to 600° C. (preferably 450 to 550° C., and more preferably 500 to 540° C.) for 4 to 12 hours (preferably 4 to 8 hours, and more preferably 4 hours) to obtain the desired non-metallic and metal oxide modified molecular sieve catalyst; or, a. Mix pure silicon Silicalite-1 with pseudo-boehmite and sesbania powder, and add 10-30wt% silica sol or 10-20wt% dilute nitric acid solution during the mixing process, wherein the mass ratio of molecular sieve, pseudo-boehmite, sesbania powder and silica sol (or dilute nitric acid solution) is 1-20:0.1-6:0.1-5:1-10 (preferably 5-10:2-5:0.1-2:1-8, more preferably 10:3-5:1:2-5); b. The wet materials obtained in step a are mixed evenly and then extruded into strips, dried at 80-120° C. (preferably 90-100° C.) for 1-24 h (preferably 12-24 h), and calcined in air at 300-600° C. (preferably 450-550° C., more preferably 500-540° C.) for 1-12 h (preferably 4-8 h, more preferably 4 h) to obtain a molecular sieve catalyst formed of pure silicon Silicalite-1.

2. The method according to claim 1, characterized in that: In the step (5), the H-type molecular sieve catalyst is modified with non-metallic oxides, the main purpose of which is to cover a portion of the acid center and reduce the acid strength of the molecular sieve, and the non-metallic oxides include but are not limited to one or more of SiO2, P2O5 and B2O3; When the molecular sieve catalyst is modified with SiO2, the method is as follows: the catalyst is immersed in a cyclohexane solution containing tetraethyl orthosilicate and / or silicone oil by an equal volume impregnation method, sealed for 12 to 24 hours after immersion, and then dried in the shade at room temperature, and calcined at a temperature of 300 to 600° C. (preferably 450 to 550° C., more preferably 500 to 540° C.) for 4 to 12 hours (preferably 4 to 8 hours, more preferably 4 hours), the amount of tetraethyl orthosilicate and / or silicone oil added is calculated according to the amount of SiO2 finally decomposed, and the deposition amount of SiO2 accounts for 1 to 30wt% (preferably 5 to 20wt%, more preferably 5 to 15wt%) of the total mass of the catalyst; Or, when the molecular sieve catalyst is modified with P2O5, the method is the same as the process of modifying the molecular sieve catalyst with SiO2, and one or more of diammonium hydrogen phosphate, disodium hydrogen phosphate, sodium hypophosphite, potassium hypophosphite or ammonium hypophosphite are selected as precursors, water is used as solvent, and the catalyst is immersed in the solvent solution containing the precursor by an equal volume impregnation method, and after immersion, it is sealed for 12 to 24 hours and then dried in the shade at room temperature, and calcined at a temperature of 300 to 600°C (preferably 450 to 550°C, more preferably 500 to 540°C) for 4 to 12 hours (preferably 4 to 8 hours, more preferably 4 hours); the deposition amount of P2O5 accounts for 1 to 30wt% (preferably 5 to 20wt%, more preferably 5 to 15wt%) of the total mass of the catalyst; Or, when the molecular sieve catalyst is modified with B2O3, the method is the same as the process of modifying the molecular sieve catalyst with SiO2, boric acid is selected as the precursor, water and / or ethanol are used as the solvent, and the catalyst is immersed in the solvent solution containing the precursor by the equal volume impregnation method. After immersion, it is sealed for 12 to 24 hours and then dried in the shade at room temperature, and calcined at a temperature of 300 to 600°C (preferably 450 to 550°C, more preferably 500 to 540°C) for 4 to 12 hours (preferably 4 to 8 hours, more preferably 4 hours); the deposition amount of B2O3 accounts for 1 to 30wt% (preferably 5 to 20wt%, more preferably 5 to 15wt%) of the total mass of the catalyst.

3. The method according to claim 1, characterized in that: In the step (6), the non-metallic oxide modified molecular sieve catalyst is modified with a metal oxide, wherein the metal oxide includes but is not limited to one or more of alkaline earth metal MgO and rare earth metal La2O3, CeO2, etc. The main purpose of the modification is to further reduce the acid amount and acid strength of the molecular sieve and improve the acid resistance of the molecular sieve; When the molecular sieve catalyst is modified with MgO, the catalyst modified with the non-metallic oxide is immersed in an aqueous solution containing magnesium acetate and / or magnesium nitrate by an equal volume impregnation method, and after being impregnated at room temperature for 12 to 24 hours, it is dried at 80 to 120° C. for 12 to 24 hours, and calcined in a muffle furnace at a temperature of 300 to 600° C. (preferably 450 to 550° C., more preferably 500 to 540° C.) for 4 to 12 hours (preferably 4 to 8 hours, more preferably 4 hours) to obtain a molecular sieve catalyst modified with MgO and the non-metallic oxide, wherein the deposition amount of MgO accounts for 1 to 30 wt% (preferably 5 to 20 wt%, more preferably 5 to 10 wt%) of the total mass of the catalyst after the metal oxide modification; Or, when La2O3 is used to modify the molecular sieve catalyst, the method is the same as the process of modifying the molecular sieve catalyst with MgO, using lanthanum nitrate as a precursor and water as a solvent, and the catalyst is immersed in a solvent solution containing the precursor by an equal volume impregnation method, and after being impregnated at room temperature for 12 to 24 hours, it is dried at 80 to 120°C for 12 to 24 hours, and calcined in a muffle furnace at a temperature of 300 to 600°C (preferably 450 to 550°C, more preferably 500 to 540°C) for 4 to 12 hours (preferably 4 to 8 hours, more preferably 4 hours) to obtain a molecular sieve catalyst modified with La2O3 and a non-metallic oxide, and the deposition amount of La2O3 accounts for 1 to 30wt% (preferably 5 to 20wt%, more preferably 5 to 10wt%) of the total mass of the catalyst after metal oxide modification; Or, when the molecular sieve catalyst is modified with CeO2, the method is the same as the process of modifying the molecular sieve catalyst with MgO, using cerium nitrate as a precursor and water as a solvent, and the catalyst is immersed in a solvent solution containing the precursor by an equal volume impregnation method. After being impregnated at room temperature for 12 to 24 hours, it is dried at 80 to 120°C for 12 to 24 hours, and calcined in a muffle furnace at a temperature of 300 to 600°C (preferably 450 to 550°C, more preferably 500 to 540°C) for 4 to 12 hours (preferably 4 to 8 hours, more preferably 4 hours) to obtain a molecular sieve catalyst modified with CeO2 and a non-metallic oxide, and the deposition amount of CeO2 accounts for 1 to 30wt% (preferably 5 to 20wt%, more preferably 5 to 10wt%) of the total mass of the catalyst after metal oxide modification.

4. A molecular sieve catalyst modified by non-metal and metal oxides or a molecular sieve catalyst in the form of pure silicon Silicalite-1 obtained by the preparation method according to any one of claims 1 to 3.

5. The catalyst according to claim 4, characterized in that: The catalyst uses one or more molecular sieves with topological structures such as MFI and FAU as active components, pseudo-boehmite as a binder, and is formed by extrusion, wherein the mass of the molecular sieve accounts for 0.1-99% of the total mass of the catalyst, preferably 50-99%, and more preferably 66-99%.

6. An application of the molecular sieve catalyst according to any one of claims 4 to 5, characterized in that: It can be used to catalyze the cracking reaction of isobutyric anhydride (IBAN) or a mixture of IBAN and isobutyric acid (IBA) (IBAN+IBA) to prepare dimethyl ketone (DMK); wherein the molar ratio of IBAN in the mixture of IBAN+IBA or the raw material is not less than 10%, preferably not less than 50%, and more preferably not less than 80%.

7. The use according to claim 6, characterized in that: The reaction process of cracking IBAN or IBAN+IBA mixture to produce DMK is as follows: (1) IBAN or a mixture of IBAN and IBA is mixed with an inert carrier gas as a liquid raw material and then introduced into a preheating furnace for gasification. The feed rate of the liquid raw material is 0.1 to 20 ml / min. The inert carrier gas is one or more of N2, He, Ar, H2, CH4, CO or CO2, and the gas flow rate is 50 ml / min to 5 L / min. (2) The inner diameter of the preheating furnace is Φ20 mm, the total height of the furnace is 300 mm, the power is 1.2 kW, a stainless steel preheating tube with an inner diameter of Φ10 mm is placed in the preheating furnace, the working temperature range of the preheating furnace is 100 to 800° C., and the preferred working temperature range is 180 to 350° C.; (3) The mixed material gasified in the preheating furnace enters the high-temperature cracking furnace, the high-temperature cracking furnace has an inner diameter of Φ20 mm, a total furnace height of 380 mm, and a power of 1.2 kW. A quartz reaction tube with an outer diameter of Φ14 mm and an inner diameter of Φ10 mm is placed in the high-temperature cracking furnace. The operating temperature range of the high-temperature cracking furnace is 100 to 800° C., preferably 200 to 550° C. A catalyst bed with a height of 0.5 to 5 cm is added in the constant temperature section, and the residence time of the mixed material on the catalyst bed is 0.01 s to 5 s; (4) The cracked product is passed into a condenser for quenching, and then into a gas-liquid separation tank for gas-liquid separation. A fast low-temperature cooling circulation pump (model DLK-1010 produced by Ningbo Xinzhi Biotechnology Co., Ltd.) is used to provide cooling medium for the condenser and the gas-liquid separation tank. The cooling temperature is 0 to -10°C. The condensate containing IBAN and IBA collected in the gas-liquid separation tank can be used as a cracking reaction raw material to replace part or all of the liquid raw materials and passed into the preheating furnace for gasification; (5) The gaseous DMK product is drawn out from the top of the gas-liquid separation tank and introduced into the first absorption tank containing 50-1000 ml of ester absorbent through a bottom-inserted tube to absorb DMK. The ester absorbent includes but is not limited to one or more of methyl isobutyrate, ethyl isobutyrate, isobutyl isobutyrate, butyl acetate or isopropyl acetate. A DLK-1010 type rapid low-temperature cooling circulation pump is used to provide cooling medium for the absorption tank. The absorption temperature of the absorption tank is RT to -10°C. (6) The gaseous DMK product after primary absorption is drawn out from the top of the first absorption tank and introduced into the second absorption tank containing 50-1000 ml of ester absorbent through a bottom tube for secondary absorption of DMK. The ester absorbent and absorption temperature are the same as those of the first absorption tank.

8. The use according to claim 7, characterized in that: The ester absorption liquid after absorbing DMK in the first absorption tank and / or the second absorption tank is mixed and poured into a high-pressure reactor, and polymerized for 1 to 24 hours (preferably 2 to 12 hours) at 50 to 150° C. (preferably 50 to 100° C.) and 0.1 to 3.0 MPa (preferably 0.1 to 1.0 MPa) to obtain an ester solution containing 2,2,4,4-tetramethyl-1,3-cyclobutanedione (TMCD); The ester absorbent can be recovered by distillation to obtain a crude TMCD product. Repeating the above distillation process can reduce the impurity content and improve the purity of the TMCD product.

9. The use according to claim 7, characterized in that: The high temperature cracking furnace is provided with a cracking reactor made of a quartz tube; The condenser is a partition type heat exchanger; The number of the absorption tanks is at least 2 and they are connected in series.

10. The method according to claim 7, characterized in that: In step (1), the feed rate of the liquid supply pipe is preferably 1 to 10 ml / min, the gas supply pipe is preferably N2 and / or Ar as carrier gas, and the gas flow rate is preferably 100 ml / min to 2 L / min; The residence time of the mixed material on the catalyst bed in step (3) is preferably in the range of 0.01s to 1s.

Citation Information

Patent Citations

  • Method for synthesis of 2, 2, 4, 4-tetramethyl-1, 3-cyclobutanedione

    CN105732354A

  • Method of synthesizing 2,2,4,4-tetramethyl-1,3-cyclobutadione

    CN111718252A

  • A Highly Efficient Separation Method for Dimethyl Ketone

    CN112174797B

  • Preparation method of 2, 2, 4, 4-tetramethyl-1, 3-cyclobutanedione

    CN116751113A

  • Method for preparing 2, 2, 4, 4-tetramethyl-1, 3-cyclobutanedione and application of 2, 2, 4, 4-tetramethyl-1, 3-cyclobutanedione

    CN117342937A