Multi-dimensional detection method applied to laminated material hot melting filling drilling processing
Through multi-dimensional detection methods, multiple key factors in hot melt filling drilling of laminated materials are measured and evaluated, which solves the problems of gap filling and processing poor in the prior art, and realizes the filling effect and processing health of laminated materials. Comprehensive evaluation of the product improves filling quality and hot melt drill life.
Patent Information
- Application Number
- CN202410942689.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The prior art has adverse effects such as filling gaps, rough processing surface, and wear of hot melt drills in hot melt filling drilling processing of laminated materials, making it difficult to objectively and accurately reflect the processing effect.
Using multi-dimensional detection method, measure the axial and radial filling gaps of the filling holes, the axial force and circumferential torque of the hot melt drilling processing, the processing temperature of the filling material, the wear and chip adhesion of the hot melt drilling, and the rough surface of the filling hole wall The corresponding coefficients are calculated through the system detection unit to comprehensively evaluate the filling effect and processing health of the laminated material.
The full process inspection of hot melt filling drilling processing of laminated materials is realized, and the filling effect, processing health status and filling hole wall quality is intuitively displayed, helping to optimize the working parameters, improve the filling quality and extend the life of hot melt drills.
Smart Images

Figure CN118990123A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a technology in the field of mechanical processing, specifically a multi-dimensional detection method applied to hot melt filling drilling processing of laminated materials. Background Art
[0002] The high-speed rotation of the melt drill causes the material to be plastically formed, accompanied by severe extrusion pressure and friction heat, which in turn produces adverse effects such as filling gaps, rough processing surface, and wear of the melt drill. In order to objectively and accurately reflect the processing effect of hot melt filling drilling of laminated materials, a multi-dimensional detection method needs to be proposed. Summary of the invention
[0003] In view of the above-mentioned deficiencies in the prior art, the present invention proposes a multi-dimensional detection method for hot-melt filling and drilling processing of laminated materials. The method comprehensively considers the filling effect of the laminated materials, the processing health status, and the processing quality factors of the filling hole wall, measures the axial and radial filling gaps of the filling hole, the axial force and circumferential torque of the hot-melt drill processing, the filling material processing temperature, the hot-melt drill wear and chip adhesion conditions, the surface roughness of the filling hole wall, and the burr height at the entrance and exit of the drilling hole, and detects the processing effect of the hot-melt filling and drilling of the laminated materials.
[0004] The present invention is achieved through the following technical solutions:
[0005] The present invention relates to a multi-dimensional detection method for hot melt filling drilling processing of laminated materials, comprising:
[0006] ① In the processing preparation stage, the hot melt drill is microscopically measured to record the surface morphology and original element composition of the hot melt drill;
[0007] ②Monitoring in each processing stage: The hot melt drill is subjected to axial force and circumferential torque, and the indicator analysis is performed according to the material characteristics of the hot melt drill to detect the health of the hot melt drill; monitor the processing temperature of the filling material, and perform indicator analysis according to the characteristics of the filling material to detect the health of the workpiece;
[0008] ③ At the completion stage of processing, the filled cavity is sectioned in the plane perpendicular to the axis and the plane where the axis is located, and the filling gap between the filling material and the cavity in the radial and axial directions is measured to detect the filling effect of the laminated material;
[0009] ④ Evaluation and analysis stage: after completing the hole processing, the hot melt drill is microscopically measured, compared with the initial surface morphology and original elemental composition of the hot melt drill, and the wear of the hot melt drill and the chip adhesion on the surface of the hot melt drill are detected; the surface roughness and the entrance and exit burr height of the completed filling hole are measured to detect the surface quality of the filling hole wall.
[0010] The present invention relates to a system for realizing the above method, comprising: a hot melt drill wear detection unit, a chip adhesion detection unit, a hot melt drill health detection unit, a filling material health detection unit, a filling quality detection unit and a filling hole wall surface quality detection unit, wherein: the hot melt drill wear detection unit performs a hot melt drill length comparison calculation according to the hot melt drill geometric shape change before and after processing, obtains the hot melt drill axial wear amount, performs maximum and minimum normalization on the wear amount, and obtains the wear coefficient; the chip adhesion detection unit analyzes the growth amount of the filling material characteristic elements on the hot melt drill surface according to the element composition ratio on the hot melt drill surface before and after processing, obtains the chip adhesion amount, performs maximum and minimum normalization on the chip adhesion amount, and obtains the chip adhesion amount coefficient; the hot melt drill health detection unit performs a hot melt drill health detection unit according to the hot melt drill axial force and circumferential rotation during processing, and obtains the chip adhesion amount coefficient. The moment data is compared with the allowable axial force and circumferential torque of the hot melt drill to obtain the load health status of the hot melt drill; the filling material health status detection unit compares the filling material temperature information during the processing with the thermal softening temperature and melting point of the filling material to obtain the filling material health status; the filling quality detection unit measures 10 gap values in the radial and axial directions according to the section measurement results, calculates the average value of the gap value as the filling gap of the filling material, normalizes the filling gap to the maximum and minimum, obtains the filling gap coefficient, and evaluates the filling quality of the laminated material; the filling hole wall surface quality detection unit divides the filling hole wall surface roughness by 20μm to obtain the roughness coefficient, and divides the average value of the entrance and exit burr height by 1mm to obtain the burr coefficient, and evaluates the filling hole wall surface quality. Technical Effects
[0011] The present invention conducts full-process detection for the new processing method of hot melt filling drilling of laminated materials, and reflects the three aspects of information of the filling effect of laminated materials, the processing health status, and the processing quality of the filled hole wall by detecting the axial and radial filling gaps of the filled hole, the axial force and circumferential torque of the hot melt drill processing, the processing temperature of the filling material, the wear and chip adhesion of the hot melt drill, the surface roughness of the filled hole wall, and the burr height at the entrance and exit of the drilling hole. Compared with the prior art, the present invention can intuitively display the filling effect of laminated materials, the processing health status, and the processing quality of the filled hole wall in the hot melt filling drilling of laminated materials, which is helpful to optimize the processing parameters, improve the filling quality, and extend the service life of the hot melt drill. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a schematic diagram of the process of the present invention;
[0013] Figure 2 It is a schematic diagram of hot melt drilling and filling processing of laminated materials;
[0014] Figure 3 This is the test result of hot melt drill morphology;
[0015] Figure 4 Fill radial gap detection results for transverse sectioning;
[0016] Figure 5 Fill the axial gap test results for the longitudinal section;
[0017] Figure 6 Cutting force and cutting torque data during hot melt drilling of laminated materials;
[0018] Figure 7 The data of the inlet temperature of titanium alloy drilling during the hot melt drilling process of laminated materials;
[0019] Figure 8 This is the result of optical microscope test of hot melt drill wear;
[0020] Fig. 9 This is the EDS element spectrum test result of the hot melt drill surface. DETAILED DESCRIPTION
[0021] This embodiment is aimed at Figure 2 The multi-dimensional detection method of the hot melt drilling filling process of the titanium alloy-aluminum alloy laminated material shown in the figure comprehensively considers the filling effect of the laminated material, the processing health status and the processing quality factors of the filled hole wall, such as Figure 1 Specifically shown include:
[0022] Step 1: For the TC4 titanium alloy-aluminum alloy laminated material that needs to be filled, where the filling material is TC4 titanium alloy and the cavity material is aluminum alloy, perform microscopic inspection on the hot melt drill used for processing to obtain the hot melt drill surface and the original elements of the hot melt drill, and record the hot melt drill surface morphology, hot melt drill axial length and original element composition ratio, such as Figure 3 As shown, the processing parameters are formulated so that the temperature of the contact area between the hot melt drill and the filling material is higher than the thermal softening temperature of the filling material and lower than the thermal melting point of the filling material.
[0023] Step 2: Perform hot melt drilling and filling processing of TC4 titanium alloy-aluminum alloy laminated materials. During the processing, measure the axial force and circumferential torque data of the hot melt drill, and measure the processing temperature of the filling material. Use a rotary dynamometer to measure the axial force and circumferential torque of the hot melt drill during the processing, and use an infrared thermometer to measure the processing temperature of the filling material. The temperature measurement area is the entrance position of the processing hole.
[0024] Step 3: After processing, use the sectioning measurement method to section the aluminum alloy filling cavity in the plane perpendicular to the axis and the plane where the axis is located, and measure the radial and axial filling gaps between the TC4 titanium alloy filling material and the aluminum alloy cavity; for the surface quality of the filling hole wall, test the surface roughness of the filling hole wall and the height of the burr at the entrance and exit of the drilling hole. Specifically include:
[0025] 3.1) Make a transverse section on the machined aluminum alloy filling cavity along a plane perpendicular to the axis, and use end milling to make a transverse section until the measuring surface position is reached, such as Figure 4 After the sectioning is completed, the filling condition of TC4 titanium alloy is detected by using a microscope, and the radial voids between the filling material and the filling cavity at 10 different positions are measured. The radial voids are normalized to the maximum and minimum values to obtain the radial void coefficient.
[0026] 3.2) Make a longitudinal section along the plane where the axis is located on the processed aluminum alloy filling cavity, and use side milling to make a longitudinal section until the plane where the filling hole diameter is measured is reached, such as Figure 5 After the sectioning is completed, the filling material is tested with a microscope, and the axial gaps between the filling material and the filling cavity at 10 different positions are measured. The axial gaps are normalized to the maximum and minimum values to obtain the axial gap coefficient.
[0027] 3.3) The surface roughness of three areas of the filled hole wall is measured on the longitudinally cut laminated material, and the roughness coefficient is obtained by dividing the average roughness by 20 μm.
[0028] 3.4) Measure the burr height at the entrance and exit of the drill hole on the filled laminated material. Use laser to measure the burr height at ten locations of the entrance and exit. Calculate the average burr value and divide it by 1mm to get the burr coefficient.
[0029] Step 4: Evaluate and analyze the axial force, circumferential torque and processing temperature of the hot melt drill during processing, including:
[0030] 4.1) According to the geometric structure and material properties of the melt drill, the allowable axial force and circumferential torque of the melt drill are calculated, and the appropriate range of axial force and circumferential torque is determined. In this example, the allowable axial force of the melt drill is 1200N, and the allowable circumferential torque is 0.9N·m.
[0031] 4.2) Analyze the axial force of the hot melt drill during the drilling process. According to the cutting force change trend, the cutting stage is divided by calculating the mean value of the sample point data. The entire drilling process is divided into three parts: the feed stage, the filling stage, and the retract stage. Figure 6 As shown, the average axial force in the feed stage and the filling stage is calculated, and the ratio of the average axial force to the allowable axial force is used as the axial load coefficient.
[0032] 4.3) Analyze the circumferential torque of the hot melt drill during the drilling process. According to the cutting torque change trend, the cutting stage is divided by calculating the mean value of the sample point data. The entire drilling process is divided into three parts: the feed stage, the filling stage, and the retract stage. Figure 6As shown, the average circumferential torque of the hot melt drill in all three stages is calculated, and the ratio of the average circumferential torque to the allowable circumferential torque is taken as the circumferential load factor.
[0033] 4.4) Analyze the temperature of the filling material during the drilling process. The measurement area is the drilling entrance of the filling material TC4 titanium alloy. The measured temperature is as follows: Figure 7 The temperature load coefficient is obtained by dividing the difference between the maximum temperature at the inlet of the filling material surface and the thermal softening temperature of the filling material by the difference between the melting point of the filling material and the thermal softening temperature of the filling material.
[0034] Step 5: Perform melt drill inspection on the processed melt drill to check the wear and chip adhesion of the melt drill, including:
[0035] 5.1) Use anhydrous ethanol to ultrasonically clean the hot melt drill after processing. After cleaning, check the remaining axial length of the hot melt drill after processing. Figure 8 As shown in the figure, the difference in axial length of the hot melt drill before and after processing is the wear amount of the hot melt drill. The wear amount is normalized to the maximum and minimum to obtain the wear coefficient.
[0036] 5.2) Perform element spectrum test on the surface of the hot melt drill. The test results are Fig. 9 As shown, titanium is selected as the characteristic element of the filling material, and the titanium content on the surface of the hot melt drill before and after processing is analyzed as the chip adhesion amount. The chip adhesion amount is normalized to the maximum and minimum to obtain the chip adhesion coefficient.
[0037] Step 6: Calculate the average of the axial load coefficient, circumferential load coefficient, temperature load coefficient, radial clearance coefficient, axial clearance coefficient, wear coefficient, chip adhesion coefficient, roughness coefficient, and burr coefficient to determine the comprehensive evaluation of the processing quality. The processing parameters with the smallest average coefficient have the best processing quality.
[0038] After specific practical experiments, the above method was run with the parameters in Table 1 under the specific environmental settings of hot melt filling drilling of TC4-aluminum alloy laminated materials using the FANUC ROBODRILL small machining center, and the experimental data shown in Table 2 were obtained. The detection coefficients described in Table 3 were calculated according to the above steps. It can be found that the optimal machining effect can be obtained when the feed speed is 2000rpm, the feed feed is 30mm / min, the retract speed is 500rpm, and the retract feed is 50mm / min.
[0039] Experimental data
[0040] Table 1 Processing experiment parameters
[0041] Table 2 Experimental data table
[0042] Table 3 Test coefficient table
[0043] Compared with the prior art, the present invention adopts radial void coefficient and axial void coefficient to reflect the filling effect of laminated materials, adopts axial load coefficient, circumferential load coefficient, temperature load coefficient, wear coefficient and chip adhesion coefficient to reflect the processing health, and adopts roughness coefficient and burr coefficient to reflect the processing quality of filled hole wall. The above three aspects can be combined to determine the quality of laminated filling hole making, and complete the multi-dimensional detection of hot melt filling drilling processing of titanium alloy-aluminum alloy laminated materials.
[0044] The above-mentioned specific implementation can be partially adjusted in different ways by those skilled in the art without departing from the principle and purpose of the present invention. The protection scope of the present invention shall be based on the claims and shall not be limited by the above-mentioned specific implementation. Each implementation scheme within its scope shall be subject to the constraints of the present invention.
Claims
1. A multi-dimensional detection method for hot melt filling drilling processing of laminated materials, characterized in that: include: ①In the processing preparation stage, the hot melt drill is microscopically measured to record the surface morphology and original element composition of the hot melt drill; ②Monitoring in each processing stage: The hot melt drill is subjected to axial force and circumferential torque, and the indicator analysis is performed according to the material characteristics of the hot melt drill to detect the health of the hot melt drill; monitor the processing temperature of the filling material, and perform indicator analysis according to the characteristics of the filling material to detect the health of the workpiece; ③ At the completion stage of processing, the filled cavity is sectioned in the plane perpendicular to the axis and the plane where the axis is located, and the filling gap between the filling material and the cavity in the radial and axial directions is measured to detect the filling effect of the laminated material; ④ Evaluation and analysis stage: after hole processing is completed, the hot melt drill is microscopically measured, compared with the initial surface morphology and original element composition of the hot melt drill, and the wear of the hot melt drill and the chip adhesion on the surface of the hot melt drill are detected; The surface roughness and inlet and outlet burr height of the machined filling hole are measured to detect the surface quality of the filling hole wall.
2. The multi-dimensional detection method for hot melt filling drilling processing of laminated materials according to claim 1 is characterized in that: The processing preparation stage is specifically as follows: for the TC4 titanium alloy-aluminum alloy laminated material that needs to be filled, wherein the filling material is TC4 titanium alloy and the cavity material is aluminum alloy, a microscopic inspection is performed on the hot melt drill used for processing to obtain the hot melt drill surface and the original elements of the hot melt drill, the surface morphology of the hot melt drill, the axial length of the hot melt drill and the original element composition ratio are recorded, and the processing parameters are formulated so that the temperature of the contact area between the hot melt drill and the filling material is higher than the thermal softening temperature of the filling material and lower than the thermal melting point of the filling material.
3. The multi-dimensional detection method for hot melt filling drilling processing of laminated materials according to claim 1 is characterized in that: The processing stage is specifically as follows: hot melt drilling and filling processing of TC4 titanium alloy-aluminum alloy laminated materials is carried out. During the processing, the axial force and circumferential torque data of the hot melt drill are measured, and the processing temperature of the filling material is measured. A rotary dynamometer is used to measure the axial force and circumferential torque of the hot melt drill during the processing, and an infrared thermometer is used to measure the processing temperature of the filling material. The temperature measurement area is the entrance position of the processing hole.
4. The multi-dimensional detection method for hot melt filling drilling processing of laminated materials according to claim 1 is characterized in that: In the processing completion stage, the aluminum alloy filling cavity is sectioned in a plane perpendicular to the axis and in a plane where the axis is located, respectively, using a sectioning measurement method to measure the radial and axial filling gaps between the TC4 titanium alloy filling material and the aluminum alloy cavity; for the surface quality of the filling hole wall, the surface roughness of the filling hole wall and the burr height at the drilling entrance and exit are tested.
5. The multi-dimensional detection method for hot melt filling drilling processing of laminated materials according to claim 1 or 4 is characterized in that: The processing completion stage specifically includes: 3.1) The processed aluminum alloy filling cavity is transversely sectioned along a plane perpendicular to the axis, and the transverse sectioning is performed by end milling to the measurement surface position, as shown in FIG4 ; after the sectioning is completed, the TC4 titanium alloy filling condition is detected using a microscope, and the radial gaps between the filling material and the filling cavity at different positions of 10 groups are measured; 3.2) The processed aluminum alloy filling cavity is longitudinally sectioned along the plane where the axis is located, and the longitudinal sectioning is performed by side milling to the plane where the filling hole diameter is measured. After the sectioning is completed, the filling material is inspected using a microscope, and the axial gaps between the filling material and the filling cavity at 10 different positions are measured; 3.3) Measure the surface roughness of three areas of the filled hole wall on the longitudinally sectioned laminated material, and divide the average roughness by 20 μm to obtain the roughness coefficient; 3.4) Measure the burr height at the entrance and exit of the drill hole on the filled laminated material. Use laser to measure the burr height at ten locations of the entrance and exit. Calculate the average burr value and divide it by 1mm to get the burr coefficient.
6. The multi-dimensional detection method for hot melt filling drilling processing of laminated materials according to claim 1 is characterized in that: In the evaluation and analysis stage, after evaluating and analyzing the axial force, circumferential torque and processing temperature of the hot melt drill during the processing, the hot melt drill is tested for wear and chip adhesion.
7. The multi-dimensional detection method for hot melt filling drilling processing of laminated materials according to claim 1 or 6 is characterized in that: The evaluation and analysis phase specifically includes: a) Calculate the allowable axial force and circumferential torque during the hot melt drilling process according to the hot melt drilling geometry and hot melt drilling material properties, and determine the appropriate axial force and circumferential torque range; b) Analyze the axial force of the hot melt drill during the drilling process. According to the cutting force change trend, the cutting stage is divided by calculating the mean value of sample point data. The entire drilling process is divided into three parts: the feed stage, the filling stage, and the retracting stage. The average axial force in the feed stage and the filling stage is calculated, and the ratio of the average axial force to the allowable axial force is used as the axial load coefficient. c) Analyze the circumferential torque of the hot melt drill during the drilling process. According to the cutting torque change trend, the cutting stage is divided by calculating the mean value of sample point data. The entire drilling process is divided into three parts: the feed stage, the filling stage, and the retracting stage. The average circumferential torque of the hot melt drill in all three stages is calculated, and the ratio of the average circumferential torque to the allowable circumferential torque is used as the circumferential load coefficient. d) Analyze the temperature of the filling material during the drilling process. The measurement area is the drilling entrance of the filling material TC4 titanium alloy. The temperature is measured, and the difference between the maximum temperature at the entrance of the filling material surface and the thermal softening temperature of the filling material is divided by the difference between the melting point of the filling material and the thermal softening temperature of the filling material as the temperature load coefficient; e) using anhydrous ethanol to ultrasonically clean the melt drill after processing, and after cleaning, detecting the remaining axial length of the melt drill after processing. The difference in axial length of the melt drill before and after processing is the wear amount of the melt drill; f) Perform element spectrum detection on the surface of the hot melt drill, select titanium as the characteristic element of the filling material, and analyze the titanium content on the surface of the hot melt drill before and after processing as the amount of chip adhesion.
8. A multi-dimensional detection system for implementing the method described in any one of claims 1 to 7, characterized in that: include: The hot melt drill wear detection unit, the chip adhesion detection unit, the hot melt drill health detection unit, the filling material health detection unit, the filling quality detection unit and the filling hole wall surface quality detection unit, wherein: the hot melt drill wear detection unit compares and calculates the hot melt drill length according to the change of the hot melt drill geometry before and after processing, and obtains the axial wear amount of the hot melt drill; the chip adhesion detection unit analyzes the growth amount of the filling material characteristic elements on the hot melt drill surface according to the element composition ratio on the hot melt drill surface before and after processing, and obtains the chip adhesion amount; the hot melt drill health detection unit calculates the hot melt drill axial force and circumferential torque data during processing, and compares them with the allowable axial force and circumferential torque of the hot melt drill. The torque is compared to obtain the load health of the hot melt drill; the filling material health detection unit obtains the filling material health by comparing the filling material temperature information during the processing with the thermal softening temperature and melting point of the filling material; the filling quality detection unit measures 10 gap values in the radial and axial directions according to the section measurement results, calculates the average value of the gap values as the filling material filling gap, and obtains the filling quality of the laminated material; the filling hole wall surface quality detection unit obtains the roughness coefficient by dividing the filling hole wall surface roughness by 20μm and the entrance and exit burr height information according to the filling hole wall surface roughness.
Citation Information
Patent Citations
Cutter performance detection device and detection method
CN107052908A
Quantitative evaluation method for drilling defects of carbon fiber composite materials
CN110794037A
Numerical control machine tool cutter wear loss online prediction method based on spindle currents and vibration signals
CN111300146A
CFRTP / Ti laminated drilling force and material removal mechanism analysis method
CN113779836A
Processing method of titanium-aluminum composite material
CN117696946A