Silver-sulfur-based plastic inorganic semiconductor and method for realizing ultrahigh plastic deformation of silver-sulfur-based plastic inorganic semiconductor
By introducing Se and/or Te elements and performing multiple cold processing and annealing, the problem of brittle fracture of silver-sulfur-based inorganic semiconductors is solved, and silver-sulfur-based materials with ultra-high plastic deformation are achieved, satisfying the flexible electronics and Internet of Things fields Specific shape and size requirements.
Patent Information
- Application Number
- CN202410079496.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-01-19
AI Technical Summary
Traditional silver-sulfur-based inorganic semiconductors have brittle fractures under external forces, making it difficult to achieve ultra-high plastic deformation, which limits its processing methods and application scenarios, especially in the fields of flexible electronics and the Internet of Things, which are difficult to meet the specific shape and size requirements.
By introducing an appropriate amount of Se and/or Te elements, cold processing and multiple iterative annealing, the ratio of Ag and Cu and the annealing temperature are controlled, the formation of holes and brittle second phases are avoided, the plastic properties of silver sulfur-based materials are restored, and the ultra-supra-based materials are achieved High deformation amount.
The silver-sulfur-based plastic inorganic semiconductor material with ultra-high plastic deformation has been successfully obtained, avoiding cracking and burrs, achieving complex shape processing, and enhancing the material's flexible electronic application potential.
Smart Images

Figure CN118992987A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a plastic inorganic semiconductor material, in particular to a silver-sulfur-based plastic inorganic semiconductor and a method for achieving ultra-high plastic deformation of the silver-sulfur-based plastic inorganic semiconductor. Background Art
[0002] Due to their unique physical properties, semiconductors have been widely studied and applied in communications, the Internet of Things, health testing equipment, etc. However, traditional inorganic semiconductors usually exhibit brittle fracture under external forces, which greatly limits their processing methods and application scenarios.
[0003] In recent years, silver-sulfur-based semiconductors have been reported to have good plastic deformation ability, with compression strain exceeding 50% (Xun Shi et al.) and tensile strain exceeding 12% (Shiyang He et al.). In addition, compared with traditional organic semiconductors, silver-sulfur-based inorganic semiconductors have high electrical transport properties, with a mobility of 100-1000cm 2 / (V·s), so it has great application potential in the field of flexible electronics.
[0004] The patent application with publication number CN115096935A discloses a silver-based chalcogenide metal insulator phase change flexible semiconductor thermistor and application technology. This patent application uses silver-based chalcogenide compounds as temperature-sensitive materials, designs their thermistor coefficient, Seebeck coefficient, and metal insulator phase change characteristics through material components, and uses precision machining to make them into flexible self-supporting films and silk low-dimensional materials for further making component vertical devices or array devices. Combining the negative resistance temperature coefficient thermistor characteristics of silver-based chalcogenide compounds, metal insulator phase change, and Seebeck coefficient, temperature sensing, thermal switching, and high-precision thermal disturbance detection applications are realized. The technical method provided has considerable application value in intelligent temperature sensing, infrared detection, thermal disturbance detection, thermal switching, and surge current suppression, and can realize the flexibility of devices.
[0005] However, compared with traditional metal materials, the plastic deformation ability of the silver-sulfur-based semiconductor disclosed in the above patent application is still not outstanding, and the single plastic deformation is very limited. When the plastic deformation exceeds a certain amount, the silver-sulfur-based semiconductor will have obvious cracks, so it is difficult to use traditional plastic processing methods to obtain silver-sulfur-based semiconductors of various shapes and specific shapes.
[0006] At present, the processing method for silver-sulfur-based inorganic semiconductors is still limited to cutting, which not only brings about serious material loss and limited processing accuracy, but also makes it difficult to obtain complex shapes, and the plastic characteristics of silver-sulfur-based semiconductors have not been fully utilized.
[0007] With the rapid development of flexible electronics and the Internet of Things, there is an urgent need to obtain semiconductor products that meet specific application scenarios and specific shapes and sizes in a fast and efficient manner. Therefore, it is particularly critical and urgent to develop a method that can achieve ultra-high plastic deformation of current silver-sulfur-based plastic inorganic semiconductors. Summary of the invention
[0008] The invention provides a method for realizing ultra-high plastic deformation of a silver-sulfur-based plastic inorganic semiconductor. The method can be used to prepare a silver-sulfur-based plastic inorganic semiconductor material with ultra-high plastic deformation.
[0009] The present invention provides a preparation method for realizing ultra-high plastic deformation of a silver-sulfur-based plastic inorganic semiconductor, comprising:
[0010] (1) Cold processing of silver-sulfur based materials;
[0011] (2) annealing the cold-processed silver-sulfur-based material under an inert gas atmosphere or a vacuum environment;
[0012] (3) Repeat (1)-(2) to achieve ultra-high deformation of silver-sulfur-based plastic inorganic semiconductor materials;
[0013] The silver-sulfur-based material is Ag 2-x Cu x S 1-y M y , wherein M is Se and / or Te, x=0-0.5, y=0.2-0.7.
[0014] The present invention introduces an appropriate amount of Se and / or Te elements with a larger radius, so that the silver-sulfur-based material becomes amorphous after completing cold working with a larger deformation rate. At the same time, by adjusting the ratio of Ag and Cu, the generation of holes that affect the plastic properties of the silver-sulfur-based material after annealing is avoided, thereby better restoring the plastic properties of the silver-sulfur-based material and preparing for the next cold working. Multiple iterations are performed until the ultra-high deformation required by the present invention is obtained.
[0015] Furthermore, the annealing temperature of step (2) is above the phase transition temperature and below 750°C, and the annealing time is above 5 minutes. The phase transition temperature is the temperature at which the silver-sulfur-based material changes from an amorphous state to a crystalline state, and is obtained by DSC testing. The present invention controls the annealing temperature above the phase transition temperature so that the silver-sulfur-based material changes from an amorphous state to a crystalline state, thereby better restoring the plastic properties of the silver-sulfur-based material, and controls the annealing time to provide sufficient time for the phase transition to obtain a crystalline phase structure with better plasticity.
[0016] Furthermore, the annealing temperature of step (2) is 300-700° C. The present invention provides a suitable annealing temperature so that the amorphous structure obtained after cold working is transformed into a crystalline phase with a cubic structure, thereby restoring the plasticity of the silver-sulfur-based material and minimizing the transformation into a crystalline phase with a monoclinic structure with poor plasticity.
[0017] Furthermore, the annealing temperature of step (2) is 350-500° C., and the annealing time is 5-120 min. The present invention can further control the annealing temperature and annealing time to ensure the formation of a silver-sulfur-based material with good plasticity while avoiding the precipitation and volatilization of Ag, Cu, and S materials with low solid solubility, which affects the performance of the semiconductor material.
[0018] Furthermore, the stretching rate in step 1 is less than 50%, the rolling deformation rate is less than 200%, or the reduction of the drawing diameter is less than 50%. By controlling the deformation rate, burrs or even direct fractures of the silver-sulfur-based material are avoided after a single processing.
[0019] Furthermore, cooling methods after annealing include air cooling, water cooling and furnace cooling.
[0020] The present invention controls the cooling method so that the cooling rate is controlled within a reasonable range, so that the silver-sulfur-based material produces less brittle second phase during the phase change process, thereby making the silver-sulfur-based material have better plasticity.
[0021] Further preferably, the cooling method is air cooling and water cooling. Compared with other cooling methods, under air cooling and water cooling conditions, the second phase produced in the silver-sulfur-based material is minimal, and the production of a monoclinic structure crystal phase with poor plasticity is avoided, so the plasticity is best.
[0022] Furthermore, the pressure of the inert gas is 0-100 MPa to control the volatilization of the S / Te elements.
[0023] Furthermore, the cold working in step (2) is cold rolling, cold forging, cold drawing, cold heading or cold bending.
[0024] On the other hand, the present invention also provides a silver-sulfur-based plastic inorganic semiconductor prepared by the preparation method for achieving ultra-high plastic deformation of the silver-sulfur-based plastic inorganic semiconductor.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention provides an appropriate amount of Se and / or Te elements to make the silver-sulfur-based material undergo an amorphous transformation after cold working, and then uses an annealing process to make the amorphous silver-sulfur-based material undergo a crystalline phase transformation, thereby restoring the plasticity of the silver-sulfur-based material. At the same time, the amount of Se and / or Te elements and the amount of Cu elements are controlled to avoid affecting the plastic properties of the silver-sulfur-based material after annealing. Since plastic recovery is performed after each cold working, the silver-sulfur-based material will not produce cracks and burrs during multiple cold working processes, and the purpose of obtaining a silver-sulfur-based plastic inorganic semiconductor material with ultra-high deformation is achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A schematic diagram of the rolling operation provided for Example 1, and a photograph of the sample fracture after a single rolling deformation.
[0028] Figure 2 The images of the silver-sulfur-based inorganic semiconductors prepared at different iteration times provided in Example 1, and the images of the silver-sulfur-based inorganic semiconductors prepared under a single large-volume rolling process provided in Comparative Example 1.
[0029] Figure 3 This is a microstructure diagram of the silver-sulfur-based inorganic semiconductor prepared in Example 1.
[0030] Figure 4 A comparison chart of the plastic deformation obtained by the single stretching provided in Comparative Example 2 and the iterative stretching-annealing method provided in Example 2.
[0031] Figure 5 Schematic diagram of the pulling operation in Example 3, and a photograph of a semiconductor wire obtained by the iterative pulling-annealing method.
[0032] Figure 6 This is a photo of the semiconductor surface profile obtained by the iterative deformation-annealing method in Example 4.
[0033] Figure 7 The XRD spectrum and microstructure of the silver-sulfur-based inorganic semiconductor prepared in Example 10.
[0034] Figure 8 The following are the XRD patterns and optical photographs of the silver-sulfur-based inorganic semiconductor prepared in Example 11.
[0035] Fig. 9 This is an optical photograph of the silver-sulfur-based inorganic semiconductor prepared in Comparative Example 3.
[0036] Fig.10 The XRD spectrum and microstructure diagram of the silver-sulfur-based inorganic semiconductor prepared in Comparative Example 4.
[0037] Fig.11This is a morphology photograph of the silver-sulfur-based inorganic semiconductor prepared in Comparative Example 5 after rolling.
[0038] Fig.12 The XRD spectrum, microstructure diagram and compressive stress-strain curve diagram of the silver-sulfur-based inorganic semiconductor prepared in Comparative Example 6. DETAILED DESCRIPTION
[0039] The present invention is further described in detail below with reference to the embodiments.
[0040] Example 1
[0041] Rolling can cause continuous plastic deformation of the material, as shown in the schematic diagram. Figure 1 The original size of Ag2Te is 2mm×6mm×10mm. 0.6 S 0.4 The semiconductor samples were rolled at room temperature using a rolling mill (Hefei Kejing, MSK-HRP-04UL).
[0042] When Ag2Te 0.6 S 0.4 The rolling deformation rate of the semiconductor sample is 141%, that is, the rolling is stopped after it decreases from 2.05 mm to 0.85 mm. The sample is transferred to a quartz tube, sealed under an argon atmosphere, placed in a muffle furnace and heated to 400 °C for annealing for 20 minutes, and cooled to room temperature in air at a cooling rate of about 50 K / min after four iterations of rolling-annealing. Figure 2 The dimensional changes of the samples after each rolling-annealing process and the final state are shown. 0.6 S 0.4 The final thickness of the semiconductor sample reaches 0.02mm, the plastic elongation reaches 10150%, and the edge is smooth without cracks. Its plastic deformation is much higher than that of the sample after a single rolling. Figure 2 The final Ag2Te 0.6 S 0.4 The crystal structure of semiconductor samples is Figure 3 As shown in (a) and (b), the EDS results show that the composition of Ag, Te, and S is basically in line with the nominal ratio, proving that the metal elements and S elements are less volatile, such as Figure 3 As shown in (c) and (d), the synthesized silver-sulfur-based inorganic semiconductor is a crystalline phase with a cubic structure, but after cold working, the diffraction peak disappears and an amorphous transformation occurs.
[0043] Comparative Example 1
[0044] Rolling can cause continuous plastic deformation of the material, as shown in the schematic diagram. Figure 1 The original size of Ag2Te is 2mm×6mm×10mm. 0.6 S 0.4The semiconductor sample was rolled at room temperature by a rolling mill (Hefei Kejing, MSK-HRP-04UL). The semiconductor sample deformed by a single rolling process broke after the rolling deformation rate reached 1100%, and dense cracks appeared at the edge of the sample, such as Figure 2 as shown in (b).
[0045] Example 2
[0046] For Ag2Te 0.6 S 0.4 The semiconductor was subjected to room temperature biaxial stretching. The dimensions of the deformation area were: thickness 1.2 mm, width 4 mm, and length 8 mm.
[0047] When Ag2Te 0.6 S 0.4 The tensile deformation rate of the deformed area of the semiconductor reached 30%, that is, the stretching was stopped after it was elongated from 8mm to 11mm. The sample was transferred to a quartz tube, sealed under an argon atmosphere, placed in a muffle furnace and heated to 360°C for annealing for 5 minutes, and cooled to room temperature in air. After three iterative stretching-annealing, the tensile deformation rate was close to 100% fracture, and its plastic deformation was twice the elongation of the single stretching sample.
[0048] Comparative Example 2
[0049] For Ag2Te 0.6 S 0.4 Semiconductor is subjected to room temperature biaxial stretching. The size of the deformation region (in Figure 4 The sample is circled in the figure): thickness 1.2 mm, width 4 mm, length 8 mm. The sample is stretched using Shanghai Jujing JVJ-20S universal mechanical testing machine. After a single stretching deformation, the sample's tensile deformation rate is close to 50% and breaks. Figure 4 As shown in (a).
[0050] Example 3
[0051] The Ag2Te with a diameter of 2.6 mm and a length of 20 mm 0.6 S 0.4 The semiconductor sample is drawn at room temperature through a wire drawing plate. The drawing diagram is shown in Figure 5 As shown in (a). When the diameter is reduced by 20%, that is, from 2.6 mm to 2.0 mm, the sample is transferred to a quartz tube, sealed in an argon atmosphere, placed in a muffle furnace and heated to 400 ° C for annealing for 10 minutes, and then cooled to room temperature in air. After three iterations of drawing-annealing, the diameter of the sample can reach 0.45 mm, and the obtained semiconductor wire still shows good plasticity and has bending ability, as shown in Figure 5 As shown in (b) and (c).
[0052] Example 4
[0053] The original size of Ag2Te is 4mm×6mm×9mm. 0.6 S 0.4 The semiconductor sample was rolled to obtain a plate with a thickness of 0.9 mm. The plate was transferred to a quartz tube, sealed in an argon atmosphere, placed in a muffle furnace and heated to 400 °C for annealing for 30 minutes, and then cooled to room temperature in air. The plate was forged into a school emblem pattern using cold forging and a die, such as Figure 6 shown.
[0054] Example 5
[0055] Compared with Example 1, the difference is that the silver-sulfur-based material is Ag 1.6 Cu 0.4 S 0.4 Te 0.6 The single rolling deformation rate is 49%.
[0056] Example 6
[0057] Compared with Example 1, the difference is that the silver-sulfur-based material is Ag2S 0.5 Se 0.5 The single rolling deformation rate is 83%. After iterative annealing, the final deformation reaches 5650%.
[0058] Comparative Example 3
[0059] Compared with Example 5, the difference is that the silver-sulfur-based material is Ag 1.2 Cu 0.8 S 0.4 Te 0.6 ,like Fig. 9 As shown, the prepared material has voids and exhibits brittle fracture characteristics and has no plastic deformation capability.
[0060] Example 7
[0061] Compared with Example 1, the difference is that the silver-sulfur-based material is Ag2S 0.6 Te 0.4 The single rolling deformation rate is 140%. After iterative annealing, the final rolling deformation rate reaches 6767%.
[0062] Example 8
[0063] Compared with Example 1, the difference is that the silver-sulfur-based material is Ag2S 0.8 Te 0.2 The single rolling deformation rate is 153%. After iterative annealing, the final rolling deformation rate reaches 7067%.
[0064] Example 9
[0065] Compared with Example 1, the difference is that the cooling method is water cooling, the cooling rate is about 200K / min, and the single rolling deformation rate is 150%. After iterative annealing, the final rolling deformation rate reaches 6800%.
[0066] Example 10
[0067] Compared with Example 1, the difference is that the cooling method is furnace cooling, the cooling rate before 250°C is about 6K / min, and the single rolling deformation rate is 14%. Figure 7 (a) and Figure 7 As shown in (b), a monoclinic structure is formed at a lower cooling rate, and a certain amount of brittle second phase is generated in the organization.
[0068] Embodiment 11
[0069] Compared with Example 1, the difference is that the protective gas pressure is 0 MPa, the annealing temperature is 700° C., and the annealing time is 120 min. Figure 8 (a) and Figure 8 As shown in (b), a small amount of metallic Ag was found to be precipitated on the surface of the sample in the XRD and optical photographs. This was due to the high annealing temperature, long annealing time and lack of protective gas pressure, which led to the volatilization of a small amount of S and Te.
[0070] Comparative Example 4
[0071] Compared with Example 1, the difference is that the cooling method is slow cooling, and the slow cooling is achieved by program-controlled furnace cooling speed, and the controlled cooling speed is 0.4K / min. Fig.10 (a) and Fig.10 (b) XRD and SEM characterizations revealed that there was a large amount of brittle second phase structure in the sample, which caused microcracks and made cold processing impossible.
[0072] Comparative Example 5
[0073] The difference from Example 1 is that the silver-sulfur-based material is Ag2S 0.2 Te 0.8 , the deformation rate of a single cold working is 23%. Fig.11 As shown, the prepared silver-sulfur-based material developed cracks after a single cold working.
[0074] Comparative Example 6
[0075] The difference from Example 1 is that the annealing temperature is 250°C. Fig.12 As shown in Figure 2, the sample phase structure changes to a monoclinic structure, and brittle fracture occurs directly at room temperature. It cannot be cold processed by rolling or other methods, such as Fig.12 The secondary electrons and backscattering show that the low-temperature annealed sample has a large number of microcracks after polishing and suffers brittle fracture.
Claims
1. A method for achieving ultra-high plastic deformation of silver-sulfur-based plastic inorganic semiconductors, characterized in that: include: (1) Cold processing of silver-sulfur based materials; (2) annealing the cold-processed silver-sulfur-based material under an inert gas atmosphere or a vacuum environment; (3) Repeat (1)-(2) to achieve ultra-high deformation of silver-sulfur-based plastic inorganic semiconductor materials; The silver-sulfur-based material is Ag 2-x Cu x S 1-y M y , wherein M is Se and / or Te, x=0-0.5, y=0.2-0.
7.
2. The method for achieving ultra-high plastic deformation of silver-sulfur-based plastic inorganic semiconductor according to claim 1, characterized in that: The annealing temperature of step (2) is above the phase transition temperature and below 750° C., and the annealing time is above 5 min.
3. The method for achieving ultra-high plastic deformation of silver-sulfur-based plastic inorganic semiconductor according to claim 2, characterized in that: The annealing temperature of step (2) is 300-700°C.
4. The method for achieving ultra-high plastic deformation of silver-sulfur-based plastic inorganic semiconductor according to claim 3, characterized in that: The annealing temperature of step (2) is 350-500° C., and the annealing time is 5-120 min.
5. The method for achieving ultra-high plastic deformation of silver-sulfur-based plastic inorganic semiconductor according to claim 1, characterized in that: The elongation rate of step 1 is less than 50%, the rolling deformation rate is less than 200%, or the reduction of the drawing diameter is less than 50%.
6. The method for achieving ultra-high plastic deformation of silver-sulfur-based plastic inorganic semiconductor according to claim 1, characterized in that: Cooling methods after annealing include air cooling, water cooling and furnace cooling.
7. The method for achieving ultra-high plastic deformation of silver-sulfur-based plastic inorganic semiconductor according to claim 6, characterized in that: The cooling methods after annealing are air cooling and water cooling.
8. A silver-sulfur-based plastic inorganic semiconductor prepared by the method for achieving ultra-high plastic deformation of a silver-sulfur-based plastic inorganic semiconductor as described in any one of claims 1 to 7.
Citation Information
Patent Citations
Preparation method of silver-based chalcogenide Ag2X thermoelectric material
CN111252802A
Silver-based chalcogenide metal insulator phase change flexible semiconductor thermosensitive sensor and application technology
CN115096935A
Silver sulfide-based thermoelectric material and preparation method thereof
CN117177646A
Preparation of semiconductor films