Reduced graphene oxide aerogel with bionic Brini-gang structure, elastomer as well as preparation method and application of reduced graphene oxide aerogel and elastomer
The preparation of bionic Bligan structure reduction graphene oxide aerogel through bidirectional cryo-directional assembly and spiral stacking assembly methods, solving the problem of insufficient application of Bligan structure integration into graphene aerogel, and achieving high-performance bionic Bligan The preparation of structural graphene-based conductive elastomers is suitable for a variety of functional applications.
Patent Information
- Application Number
- CN202411219571.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
The existing technology has not yet explored the functional application of bionic Bligan structures into graphene aerogels, especially inadequate research on the coupling of mechanical properties, electrical properties and electrical properties, and the integration of Bligan structures into new materials Technical difficulties and uncertainties.
Bionic Bligan structure reduction graphene oxide aerogel was prepared by bidirectional cryodirectional assembly growth and spiral stacking assembly to form a thin layer of graphene oxide frozen body with orientation, and a bionic Bligan structure was obtained through crosslinking and reduction processes. Reducing graphene oxide aerogel, further polymerizing PDMS in situ in the conductive frame, and preparing a stretchable, fatigue-resistant, self-monitoring bionic Bligan structure graphene-based conductive elastomer.
The preparation of bionic Bligan structural reduction graphene oxide aerogel has excellent mechanical properties and electrical conductivity. It is suitable for wearable devices and flexible electronic devices and other fields. It has the characteristics of stretchability, fatigue resistance and self-monitoring. .
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of micro- and nano-scale composite materials, in particular to bionic Brigon structure reduced graphene oxide aerogel, elastomer and preparation method and application thereof. Background Art
[0002] The magical nature has shaped many biomaterials with fine multi-level structures and excellent mechanical properties, which provide rich inspiration for the design and development of new materials for mankind. Bouligand structure, also known as spiral plywood structure, is commonly found in biomaterials such as fish scales, lobster shells and wood. This structure is composed of nanofibers that are unidirectionally aggregated into layers and then spirally stacked. Its unique structure has attracted widespread attention in recent years. The Bouligand structure can absorb energy, transmit stress and effectively inhibit the propagation of cracks by twisting and redirecting nanofibers when subjected to external loads. This mechanical mechanism provides biological tissues with excellent properties, including toughness, fracture resistance and impact resistance.
[0003] At present, the preparation methods of bionic Brigon structure materials mainly include arrangement lamination method, brushing method, 3D printing method and electrospinning method. Researchers integrate bionic Brigon structure into the design of new materials in order to achieve enhanced mechanical properties. Yu et al. developed a ceramic-polymer composite material with gradient-Brigon structure by combining 3D printing technology and melt infiltration technology, which significantly improved the peak load force and total energy absorption of the composite material under impact. Inspired by the Brigon structure of lobster abdomen, Zhao et al. designed and prepared a polyvinyl alcohol nanofiber hydrogel with bionic Brigon structure, which showed excellent fatigue resistance and impact resistance. Yu et al. successfully prepared a lightweight and high-strength bionic discontinuous Brigon structure composite film by brushing a mixed solution of xonotlite nanofibers and sodium alginate, thereby achieving synergistic toughening through discontinuous fiber bridging and induced crack deflection.
[0004] In addition to exploring the application of the Brigon structure in mechanical properties, further developing its functional applications is also critical. Hamad et al. prepared an elastic nanocomposite material with a Brigon structure. When stretched by external force, the material will cause the internal nanocrystals to rearrange, resulting in a birefringence effect, resulting in obvious color changes, showing the application prospects of optical color rendering. Ding et al. developed a ceramic thermal insulation aerogel with Brigon structural characteristics. Studies have shown that the material not only has ultra-high tensile strength, but also exhibits excellent thermal stability and fatigue resistance, effectively overcoming the problem of poor mechanical stability of thermal insulation aerogels under thermal shock conditions.
[0005] The above-mentioned enumeration of prior arts is intended to illustrate that the methods of integrating the Brigon structure into new materials and the types of new materials integrated are different, which will affect the formation of the Brigon structure and the performance of the new materials with the Brigon structure obtained after formation. Therefore, there are great technical difficulties and uncertainties in integrating the Brigon structure into new materials.
[0006] In addition, the functional application exploration of the Brigon structure in other aspects, such as electrical properties, mechanical properties and electrical properties coupling, has not been fully studied. Graphene aerogel is recognized to have great practical potential due to its light weight, high porosity, large specific surface area and excellent conductivity, and is often used as a conductive skeleton inside elastic conductors. However, there is no prior art that integrates the Brigon structure into graphene aerogel that has been disclosed, and the functional application of the Brigon structure after integrating it into graphene aerogel also needs to be explored. Summary of the invention
[0007] In view of this, the technical problem to be solved by the present invention is to provide a biomimetic Brigon structure reduced graphene oxide aerogel, an elastomer and a preparation method and application thereof. The preparation method provided by the present invention can prepare a biomimetic Brigon structure reduced graphene oxide aerogel, and then prepare a stretchable, fatigue-resistant, self-monitoring biomimetic Brigon structure reduced graphene oxide-based conductive elastomer. Another purpose of the present invention is to explore the structure and interface of the material constructed by the method. The purpose of the present invention is also to explore the mechanical properties of the material constructed by the method.
[0008] The present invention provides a method for preparing a bionic Brigon structure reduced graphene oxide aerogel, comprising the following steps:
[0009] S1) performing bidirectional freezing directional assembly growth on the graphene oxide suspension to obtain an oriented graphene oxide frozen body thin layer; the bidirectional freezing directional assembly growth comprises: taking the graphene suspension as a plane, performing bidirectional freezing directional assembly growth in two mutually perpendicular directions, namely, a y direction parallel to the plane and a z direction perpendicular to the plane;
[0010] S2) The oriented graphene oxide frozen body thin layer obtained in step S1) is made into a reduced graphene oxide aerogel film, and then the reduced graphene oxide aerogel film is assembled by spiral stacking to obtain a biomimetic Brigon structure reduced graphene oxide aerogel.
[0011] The present invention first performs bidirectional freezing and directional assembly growth on a graphene oxide suspension. The present invention uses the graphene oxide suspension as a plane, and simultaneously performs bidirectional freezing and directional assembly growth on the graphene oxide suspension in two mutually perpendicular directions, namely, the y direction parallel to the plane and the z direction perpendicular to the plane. Specifically, the present invention places the graphene oxide suspension on a medium, immerses one end of the medium in a cold source, and causes the graphene oxide suspension to generate a y-direction temperature gradient parallel to the surface of the medium and a z-direction temperature gradient perpendicular to the surface of the medium. The graphene suspension is used as a plane, and the plane is parallel to the surface of the medium, so that the two mutually perpendicular temperature gradients induce ice crystals in the graphene suspension to grow in a directional manner in the yz direction at the same time. More specifically, the present invention places the graphene oxide suspension on a medium, and cools the medium by a cold source. After the cold source is conducted in the medium for 5 to 10 cm, the graphene oxide suspension is simultaneously subjected to bidirectional freezing and directional assembly growth by the temperature gradient generated on the medium in the above two directions. The temperature of the bidirectional freezing directional assembly growth of the present invention is below 0°C, preferably -200°C~0°C, and more preferably -100°C~0°C. The thermal conductivity of the medium of the present invention is 10 W / (m•K)~30 W / (m•K), and specifically the medium includes 304 stainless steel, copper or aluminum. The concentration of the graphene oxide suspension of the present invention is 5 mg / mL~20 mg / mL, preferably 5 mg / mL, 10 mg / mL or 20 mg / mL.
[0012] In certain embodiments of the present invention, the present invention prepares a uniformly dispersed graphene oxide suspension of a certain concentration by the Hummers method. In some embodiments of the present invention, graphite sheets, sodium nitrate and concentrated sulfuric acid are mixed and stirred for 0.4 to 0.6 h, and then potassium permanganate is slowly added within 40 min and stirred into a paste, and stirring is continued for 20 h to 25 h. The reactant turns purple and the viscosity gradually increases. The electric stirring is stopped, and the mixture is placed for 6 to 7 days, and then water and hydrogen peroxide are added and stirred for 2 to 3 days. The obtained product is centrifuged and washed, and then dialyzed for 6 to 7 days, and the water is changed 2 to 3 times a day to obtain a graphene oxide suspension.
[0013] In certain embodiments of the present invention, the present invention utilizes a scraping method, that is, a coating film preparation device is used to coat the graphene oxide suspension on a bidirectional freezing mold, and liquid nitrogen is used as a cold source to cool the bidirectional freezing mold, so that the graphene oxide suspension is bidirectionally frozen and oriented to assemble and grow in the above two directions on the bidirectional freezing mold at the same time, thereby obtaining an oriented graphene oxide frozen body thin layer. The specification of the coating film preparation device of the present invention is one of 200 μm, 300 μm or 400 μm, and the optimal is 400 μm. The bidirectional freezing mold of the present invention includes a heat-conducting metal bridge platform for coating the graphene oxide suspension and support legs arranged at both ends of the platform; the platform and the support legs together constitute a support platform structure, which can be more specifically a gate-shaped structure. The platform and the support legs of the present invention can be integrally formed or separately formed; the platform and the support legs are both used to transfer temperature, specifically, the support legs at one end are connected to a cold source, and the temperature of the cold source is transferred to the platform through the support legs, so that the platform generates a temperature gradient in the yz direction; the present invention has no special restrictions on the angle at which the platform and the support legs intersect, as long as they can play a supporting role, for example, they can intersect at 60°~120°, preferably 90° orthogonal; no matter how much the angle at which the platform and the support legs intersect, as long as one end of the support legs of the bidirectional freezing mold is placed in the cold source, the platform can generate a temperature gradient in the yz direction, thereby inducing ice crystals in the graphene suspension to grow in a directional manner along the yz direction at the same time. In one embodiment of the present invention, the bidirectional freezing mold of the present invention is a metal bridge made of stainless steel, and the shape is a right-angled arch. During bidirectional freezing, one end of the metal bridge is immersed in the cold source, thereby generating temperature gradients in two directions horizontal to the metal bridge and vertical to the metal bridge.
[0014] After obtaining an oriented frozen graphene oxide thin layer, the obtained oriented frozen graphene oxide thin layer is made into a reduced graphene oxide aerogel film, and then the reduced graphene oxide aerogel film is spirally stacked and assembled to obtain a biomimetic Brigon structure reduced graphene oxide aerogel.
[0015] The present invention prepares the oriented graphene oxide frozen body thin layer into a reduced graphene oxide aerogel film, comprising the following steps: firstly, the oriented graphene oxide frozen body thin layer is cross-linked under the action of a cross-linking agent to obtain a graphene oxide hydrogel; the cross-linking agent is a metal ion solution, specifically a metal ion organic solution, more specifically a metal ion ethanol solution; the concentration of the cross-linking agent is 5 mg / mL to 15 mg / mL, preferably 10 mg / mL. In certain embodiments of the present invention, the cross-linking agent of the present invention is selected from one or more of an ethanol solution of calcium chloride and an ethanol solution of ferric chloride.
[0016] After obtaining the graphene oxide hydrogel, the present invention reduces the obtained graphene oxide hydrogel to obtain reduced graphene oxide hydrogel; the reduction temperature is 80 ℃ ~ 100 ℃, and the optimal is 95 ℃; the reduction time is 1 h ~ 24 h, and the optimal is 3 h. The reduction of the present invention is carried out under the action of a reducing agent, and the reducing agent is selected from at least one of ascorbic acid, hydrazine hydrate, ethylene glycol, and sodium hypochlorite; the concentration of the reducing agent is 1 mg / mL ~ 40 mg / mL, preferably 10 mg / mL. In some embodiments of the present invention, the reducing agent is selected from an ascorbic acid aqueous solution with a concentration of 1 mg / mL ~ 40 mg / mL, and most preferably 10 mg / mL.
[0017] After obtaining the reduced graphene oxide hydrogel, the reduced graphene oxide hydrogel is dried, specifically, the reduced graphene oxide hydrogel is washed and then dried to obtain a reduced graphene oxide aerogel film; the number of washings is 2 to 4 times; the drying temperature is 35°C to 45°C. In one embodiment of the present invention, the reduced graphene oxide hydrogel is washed 3 times with a 50% ethanol aqueous solution and then dried at 40°C to obtain a reduced graphene oxide aerogel film.
[0018] After the reduced graphene oxide aerogel film is obtained, the reduced graphene oxide aerogel film is spirally stacked and assembled to obtain a biomimetic Brigon structure reduced graphene oxide aerogel. The present invention assembles an oriented reduced graphene oxide aerogel by spiral stacking, specifically, a plurality of reduced graphene oxide aerogel films are spirally stacked and assembled under the action of an adhesive according to an interlayer deflection angle of any angle between 15° and 90°, more specifically, a plurality of reduced graphene oxide aerogel films are spirally stacked and assembled under the action of an adhesive according to an interlayer deflection angle of 30°, 45°, 60° or 90°, to obtain a biomimetic Brigon structure reduced graphene oxide aerogel; the interlayer deflection angle refers to: when the current layer of spiral stacking assembly is performed, the film of the previous layer of spiral stacking assembly is used as a reference, and the deflection angle formed by the film of the current layer of spiral stacking assembly and the film, and the interlayer deflection angles of each adjacent layer can be the same or different; the number of layers of the spiral stacking assembly is more than 2 layers, preferably 2 to 16 layers. In some embodiments of the present invention, ethanol as an adhesive is evenly sprayed on the first reduced graphene oxide aerogel film with an atomizer, and then the second reduced graphene oxide aerogel film is rotated and placed according to the above-mentioned interlayer deflection angle, and ethanol as an adhesive is evenly sprayed on the second reduced graphene oxide aerogel film with an atomizer, and the spiral stacking assembly is continued in this way to obtain a bionic Brigon structure reduced graphene oxide aerogel.
[0019] The present invention provides a biomimetic Brigon structure reduced graphene oxide aerogel obtained by the preparation method described in any of the above technical solutions. The preparation method of the present invention obtains a graphene oxide frozen body thin layer with an oriented structure through a unique bidirectional freezing directional assembly growth method, and then replaces the anisotropic thin layer usually constructed by fibers with the reduced graphene oxide nanosheet thin layer assembly with an oriented structure, and prepares a biomimetic Brigon structure reduced graphene oxide aerogel through spiral stacking. The biomimetic Brigon structure reduced graphene oxide aerogel is a reduced graphene oxide aerogel conductive frame with a biomimetic Brigon structure, and by in-situ polymerization of PDMS (polydimethylsiloxane) in the reduced graphene oxide aerogel conductive frame, a stretchable, fatigue-resistant, self-monitoring biomimetic Brigon structure graphene-based conductive elastomer can be further developed.
[0020] The invention provides a bionic Brigon structure reduced graphene oxide elastomer, comprising a frame and PDMS filled in the frame; the frame is obtained from the bionic Brigon structure reduced graphene oxide aerogel obtained by the preparation method described in any one of the above technical solutions; the PDMS is obtained from a PDMS prepolymer and a cross-linking agent.
[0021] The present invention also provides a preparation method of the above-mentioned biomimetic Brigon structure reduced graphene oxide elastomer, comprising: filling PDMS prepolymer and a cross-linking agent into a biomimetic Brigon structure reduced graphene oxide aerogel for curing to obtain a biomimetic Brigon structure reduced graphene oxide elastomer; the biomimetic Brigon structure reduced graphene oxide aerogel is a biomimetic Brigon structure reduced graphene oxide aerogel obtained by the preparation method described in any of the above technical solutions. Specifically, the biomimetic Brigon structure reduced graphene oxide aerogel is immersed in a mixed solution of the PDMS prepolymer and the cross-linking agent for vacuum treatment, and a vacuum-assisted infusion method is used to ensure that the mixed solution of the PDMS prepolymer and the cross-linking agent completely enters the biomimetic Brigon structure reduced graphene oxide aerogel, and curing is performed to obtain a biomimetic Brigon structure reduced graphene oxide elastomer; the mass ratio of the PDMS prepolymer and the cross-linking agent in the present invention is (1~10):(1~10), and the optimal ratio is 1:1. The vacuum treatment time of the present invention is 25 min to 35 min, preferably 30 min. The curing temperature of the present invention is 90 ℃ to 100 ℃, preferably 95 ℃; the curing time is 5 h to 7 h, preferably 6 h. The PDMS prepolymer of the present invention is selected from one or more of Dow Corning 184, Blue Tile Stone WS-1940 or Xinwei 909, preferably Dow Corning 184.
[0022] The present invention also provides the use of the above-mentioned bionic Brigon structure reduced graphene oxide elastomer or the bionic Brigon structure reduced graphene oxide elastomer obtained by the above-mentioned preparation method in the fields of wearable devices, health detection or flexible electronic devices.
[0023] The present invention provides a biomimetic Burygang structure reduced graphene oxide aerogel, an elastomer, and a preparation method and application thereof. The preparation method of the biomimetic Burygang structure reduced graphene oxide aerogel provided by the present invention constructs a reduced graphene oxide nanosheet thin layer assembly with a biomimetic Burygang oriented structure by a scraping and bidirectional freezing method, replaces the anisotropic thin layer usually constructed by fibers with the reduced graphene oxide nanosheet thin layer assembly, and prepares a reduced graphene oxide aerogel conductive frame with a biomimetic Burygang structure by spiral stacking, so that in the subsequent preparation method of the biomimetic Burygang structure reduced graphene oxide elastomer, PDMS is in situ polymerized in the reduced graphene oxide aerogel conductive frame to obtain a biomimetic Burygang structure reduced graphene oxide-based conductive elastomer. For the preparation method of the elastomer, it is a new type of "scraping freezing-spiral stacking-in situ polymerization" combined technology, and the obtained biomimetic Burygang structure reduced graphene oxide-based conductive elastomer has the characteristics of stretchability, fatigue resistance, and self-monitoring. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A schematic diagram of the self-made bidirectional freezing mold of the present invention;
[0025] Figure 2 A scanning electron microscope image of the reduced graphene oxide aerogel film prepared in Example 1 of the present invention;
[0026] Figure 3 An optical microscope image of the reduced graphene oxide aerogel film prepared in Example 1 of the present invention;
[0027] Figure 4 The CT slice image of the bionic Brigon structure reduced graphene oxide aerogel obtained by rotating 45° stacking;
[0028] Figure 5 The CT three-dimensional image of the bionic Brigon structure reduced graphene oxide aerogel obtained by rotating 45°;
[0029] Figure 6 is a cross-sectional view of the reduced graphene oxide elastomer prepared in Example 1 of the present invention;
[0030] Figure 7 This is a tensile mechanical properties diagram of the reduced graphene oxide elastomer prepared in Example 1 of the present invention;
[0031] Figure 8A schematic diagram of the self-made one-way freezing mold of the present invention;
[0032] Fig. 9 This is a scanning electron microscope image of the reduced graphene oxide aerogel film obtained by the unidirectional freezing method;
[0033] Fig.10 This is an optical microscope image of reduced graphene oxide aerogel film obtained by unidirectional freezing method;
[0034] Fig.11 This is a scanning electron microscope image of the reduced graphene oxide aerogel film prepared in Example 2 of the present invention;
[0035] Fig.12 This is a cross-sectional view of the reduced graphene oxide elastomer prepared in Example 2 of the present invention;
[0036] Fig.13 This is a scanning electron microscope image of the reduced graphene oxide aerogel film prepared in Example 3 of the present invention;
[0037] Fig.14 This is a cross-sectional view of the reduced graphene oxide elastomer prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0038] The present invention discloses a bionic Brigon structure reduced graphene oxide aerogel, an elastomer, and a preparation method and application thereof. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters for implementation. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0039] The overall technical solution adopted by the present invention comprises the following steps:
[0040] (1) Prepare a uniformly dispersed graphene oxide suspension of a certain concentration by the Hummers method.
[0041] (2) The graphene oxide solution was evenly coated on a homemade bidirectional freezing mold by a scraping method, and liquid nitrogen was slowly added to cool it down to promote the directional growth of ice crystals, thereby obtaining an oriented graphene oxide frozen thin layer.
[0042] (3) Immerse the thin layer of frozen graphene oxide in a metal ion ethanol solution for cross-linking to obtain graphene oxide hydrogel.
[0043] (4) The graphene oxide hydrogel is reduced to reduced graphene oxide hydrogel by a hydrothermal reduction method.
[0044] (5) The reduced graphene oxide hydrogel is washed and then dried on a hot plate to obtain a reduced graphene oxide aerogel film.
[0045] (6) The oriented reduced graphene oxide aerogel films were spirally stacked to obtain the Brillouin reduced graphene oxide aerogel.
[0046] (7) PDMS was poured into the reduced graphene oxide aerogel frame by vacuum-assisted infusion method, and the bionic Brigon structure reduced graphene oxide elastomer was obtained after high-temperature curing.
[0047] All the raw materials in the following examples are not particularly limited in their sources and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0048] The present invention will be further described below in conjunction with embodiments:
[0049] Example 1
[0050] Preparation of conductive elastic materials based on reduced graphene oxide with biomimetic Brigon structure:
[0051] Hummers method for preparing graphene oxide suspension: weigh 5.00 g of graphite flakes and 3.75 g of sodium nitrate in a 1 L beaker, slowly add 160 mL of concentrated sulfuric acid while mechanically stirring, stir and react for 0.5 h, then slowly add 20 g of potassium permanganate within 40 min and stir into a paste. Continue stirring for 20 h, the reactant turns purple and the viscosity gradually increases, stop the electric stirring, leave it for 7 days, and stir the reactant manually several times during this period. Slowly add 500 mL of deionized water while stirring with a glass rod, then gradually add 30 mL of 30 wt% H2O2 aqueous solution, and stir vigorously for 3 days. Wash the graphene oxide by centrifugation, dialyze for 7 days, and change the water 2-3 times a day.
[0052] Preparation of oriented reduced graphene oxide aerogel films with a thickness of 170 μm: Figure 1 As shown, Figure 1The figure is a schematic diagram of the self-made bidirectional freezing mold of the present invention. A cut aluminum foil is laid flat on the self-made bidirectional freezing mold. 3 mL of graphene oxide solution is dripped at one end with a plastic dropper. The solution is slowly and evenly coated on the aluminum foil with a coating preparation device with a specification of 400 μm. Liquid nitrogen is slowly added to cool down to promote the directional growth of ice crystals to obtain an oriented graphene oxide frozen body thin layer. It is immediately immersed in a square dish containing 10 mg / mL calcium chloride-ethanol solution and cross-linked in a refrigerator at -20°C for 1 h to obtain a calcium-cross-linked graphene oxide hydrogel. The graphene oxide hydrogel is fished out and immersed in a square dish containing 10 mg / mL ascorbic acid solution. After hydrothermal reduction in a 95°C oven for 3 h, it is washed three times with 50 vol% ethanol aqueous solution and dried on a 40°C hot stage to obtain an oriented reduced graphene oxide aerogel film. See Figure 2~Figure 3 , Figure 2 is a scanning electron microscope image of the reduced graphene oxide aerogel film prepared in Example 1 of the present invention, Figure 3 This is an optical microscope image of the reduced graphene oxide aerogel film prepared in Example 1 of the present invention. Figure 2~Figure 3 As shown, the structure of the aerogel is oriented.
[0053] Preparation of biomimetic Brigon structure reduced graphene oxide elastomer: spray ethanol as an adhesive evenly on a piece of oriented reduced graphene oxide aerogel film with an atomizer, rotate 45 degrees to place the second aerogel film, spray ethanol and then rotate 45 degrees to place the third aerogel film, and so on. After the spiral stacking is assembled, the biomimetic Brigon structure reduced graphene oxide aerogel preform is cut to obtain, such as Figure 4~Figure 5 As shown, Figure 4 This is a CT slice image of the bionic Brigon structure reduced graphene oxide aerogel obtained by rotating 45° stacking. Figure 5 The CT three-dimensional image of the biomimetic Brigon structure reduced graphene oxide aerogel obtained by rotating 45°. The assembled aerogel preform was vacuumed for 10 min to enhance the interlayer bonding tightness and dried on a 40 ℃ hot plate. PDMS was prepared in a centrifuge tube according to the mass ratio of Dow Corning 184 PDMS prepolymer and its matching crosslinker of 1:1. After mixing evenly, it was poured into a square dish containing reduced graphene oxide aerogel so that the aerogel was completely immersed in PDMS. Vacuuming for 30 min ensured that PDMS completely entered the aerogel frame. The impregnated reduced graphene oxide aerogel-PDMS complex was fished out, placed in a clean square dish, and cured in a 95 ℃ oven for 6 h to obtain a biomimetic Brigon structure reduced graphene oxide elastomer.
[0054] See also Figure 6 , Figure 6This is a cross-sectional view of the reduced graphene oxide elastomer prepared in Example 1 of the present invention. It can be seen that the arrangement direction of each layer of aerogel is different and spirally deflected, and PDMS is evenly filled in the reduced graphene oxide framework with almost no obvious stratification and gaps, indicating that PDMS has been successfully polymerized and tightly filled in the framework.
[0055] See also Figure 7 , Figure 7 This is a tensile mechanical properties diagram of the reduced graphene oxide elastomer prepared in Example 1 of the present invention, which shows that it has a certain elasticity. Among them, the lines of different colors only represent different test times, and the sample compositions are the same.
[0056] Comparative Example 1
[0057] The preparation of graphene oxide suspension is the same as in Example 1.
[0058] The graphene oxide suspension is subjected to unidirectional freezing and directional growth by a unidirectional freezing method. The unidirectional freezing and directional growth is as follows: a cold source is placed under the metal substrate to generate a temperature gradient in the z direction perpendicular to the substrate surface, inducing ice crystals to grow in a directional manner along the z direction, and preparing a reduced graphene oxide aerogel film. More specifically, the following is the process:
[0059] like Figure 8 As shown, Figure 8 The schematic diagram of the self-made unidirectional freezing mold of the present invention is as follows: a cut aluminum foil is laid flat on the unidirectional freezing mold (a stainless steel plate), 3 mL of graphene oxide suspension is dripped at one end with a plastic dropper, and the solution is slowly and evenly coated on the aluminum foil with a coating preparation device with a specification of 400 μm, and liquid nitrogen is slowly added under the stainless steel plate to cool down, so as to promote the directional growth of ice crystals upward, and obtain an oriented graphene oxide frozen body thin layer, which is immediately immersed in a square dish containing 10 mg / mL calcium chloride-ethanol solution, and cross-linked in a -20 ℃ refrigerator for 1 h to obtain graphene oxide hydrogel. The graphene oxide hydrogel is fished out, immersed in a square dish containing 10 mg / mL ascorbic acid solution, placed in a 95 ℃ oven for hydrothermal reduction for 3 h, washed three times with 50% ethanol aqueous solution, and dried on a 40 ℃ hot stage to obtain a reduced graphene oxide aerogel film with a honeycomb structure.
[0060] See also Figure 9~Figure 10 , Fig. 9 This is a scanning electron microscope image of reduced graphene oxide aerogel film obtained by unidirectional freezing method. Fig.10 This is an optical microscope image of a reduced graphene oxide aerogel film obtained using a unidirectional freezing method. Figure 9~Figure 10As shown, the structure of the aerogel is a porous honeycomb, which cannot replace the anisotropic thin layer spiral stacking usually constructed by fibers to prepare an aerogel conductive framework with a bionic Brigon structure.
[0061] Example 2
[0062] Preparation of bionic Brigon structure graphene-based conductive elastic materials:
[0063] The preparation of graphene oxide suspension is the same as in Example 1.
[0064] Preparation of oriented 120 μm thick reduced graphene oxide aerogel film: lay a cut aluminum foil on a homemade bidirectional freezing mold, drip 3 mL of graphene oxide solution at one end with a plastic dropper, and slowly and evenly coat the solution on the aluminum foil with a coating preparation device with a specification of 300 μm. Slowly add liquid nitrogen to cool down to promote the directional growth of ice crystals to obtain an oriented graphene oxide frozen body thin layer, which is immediately immersed in a square dish containing 10 mg / mL calcium chloride-ethanol solution and cross-linked in a -20 ℃ refrigerator for 1 h to obtain graphene oxide hydrogel. The graphene oxide hydrogel is fished out and immersed in a square dish containing 5 mg / mL ascorbic acid solution. After hydrothermal reduction in a 95 ℃ oven for 6 h, it is washed three times with 50% ethanol aqueous solution and dried on a 40 ℃ hot plate to obtain an oriented reduced graphene oxide aerogel film. See Fig.11 , Fig.11 This is a scanning electron microscope image of the reduced graphene oxide aerogel film prepared in Example 2 of the present invention. As shown in the figure, the aerogel has an oriented structure.
[0065] Preparation of biomimetic Brigon structure reduced graphene oxide elastomer: Use an atomizer to evenly spray ethanol as an adhesive on a piece of oriented graphene aerogel film, rotate 30° to place the second aerogel film, spray ethanol and then rotate 30° to place the third aerogel film, and so on. After spiral stacking and assembly, cut to obtain biomimetic Brigon structure graphene aerogel. Vacuum the assembled aerogel for 10 min to enhance the interlayer bonding tightness, and place it on a 40 ℃ hot table to dry. Prepare PDMS in a centrifuge tube according to the mass ratio of Dow Corning 184 PDMS prepolymer and its matching crosslinker of 1:2, pour it into a square dish containing reduced graphene oxide aerogel, so that the aerogel is completely immersed in PDMS, and vacuum for 30 min to ensure that PDMS completely enters the reduced graphene oxide aerogel frame. The impregnated reduced graphene oxide aerogel-PDMS composite was fished out, placed in a clean square dish, and cured in an oven at 95°C for 6 h to obtain a bionic Brigon structure reduced graphene oxide elastomer.
[0066] See also Fig.12 , Fig.12 This is a cross-sectional view of the reduced graphene oxide elastomer prepared in Example 2 of the present invention. It can be seen that PDMS is evenly filled in the graphene framework with almost no obvious stratification and gaps, indicating that PDMS has been successfully polymerized and tightly filled in the framework.
[0067] Example 3
[0068] Preparation of bionic Brigon structure graphene-based conductive elastic materials:
[0069] The preparation of graphene oxide suspension is the same as in Example 1.
[0070] Preparation of oriented 120 μm thick reduced graphene oxide aerogel film: lay a cut aluminum foil on a homemade bidirectional freezing mold, drip 3 mL of graphene oxide solution at one end with a plastic dropper, and slowly and evenly coat the solution on the aluminum foil with a coating preparation device with a specification of 300 μm. Slowly add liquid nitrogen to cool down to promote the directional growth of ice crystals to obtain an oriented graphene oxide frozen body thin layer, which is immediately immersed in a square dish containing 10 mg / mL ferric chloride-ethanol solution and cross-linked in a -20 ℃ refrigerator for 1 h to obtain graphene oxide hydrogel. The graphene oxide hydrogel is fished out and immersed in a square dish containing 10 mg / mL ascorbic acid solution. After hydrothermal reduction in a 95 ℃ oven for 1 h, it is washed three times with 50% ethanol aqueous solution and dried on a 40 ℃ hot plate to obtain an oriented reduced graphene oxide aerogel film. See Fig.13 , Fig.13 This is a scanning electron microscope image of the reduced graphene oxide aerogel film prepared in Example 3 of the present invention. As shown in the figure, the aerogel has a certain orientation.
[0071] Preparation of biomimetic Brigon structure reduced graphene oxide elastomer: Use an atomizer to evenly spray ethanol as an adhesive on a piece of oriented reduced graphene oxide aerogel film, rotate 60° to place the second aerogel film, spray ethanol and then rotate 60° to place the third aerogel film, and so on. After the spiral stacking is assembled, the biomimetic Brigon structure reduced graphene oxide aerogel is cut. The assembled aerogel is vacuumed for 10 min to enhance the interlayer bonding tightness and placed on a 40 ℃ hot table for drying. PDMS is prepared in a centrifuge tube according to a mass ratio of Dow Corning 184 PDMS prepolymer and its matching crosslinker of 1:1, and poured into a square dish containing reduced graphene oxide aerogel so that the aerogel is completely immersed in PDMS. Vacuum for 30 min to ensure that PDMS completely enters the aerogel frame. The impregnated reduced graphene oxide aerogel-PDMS composite was fished out, placed in a clean square dish, and cured in an oven at 95°C for 6 h to obtain a bionic Brigon structure reduced graphene oxide elastomer.
[0072] See also Fig.14 , Fig.14 This is a cross-sectional view of the reduced graphene oxide elastomer prepared in Example 3 of the present invention. It can be seen that PDMS is uniformly filled in the reduced graphene oxide framework, with almost no obvious stratification and gaps, indicating that PDMS has been successfully polymerized and tightly filled in the framework.
[0073] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a bionic Brigon structure reduced graphene oxide aerogel, characterized in that: The following steps are involved: S1) performing bidirectional freezing directional assembly growth on the graphene oxide suspension to obtain an oriented graphene oxide frozen body thin layer; the bidirectional freezing directional assembly growth comprises: taking the graphene suspension as a plane, performing bidirectional freezing directional assembly growth in two mutually perpendicular directions, namely, a y direction parallel to the plane and a z direction perpendicular to the plane; S2) The oriented graphene oxide frozen body thin layer obtained in step S1) is made into a reduced graphene oxide aerogel film, and then the reduced graphene oxide aerogel film is assembled by spiral stacking to obtain a biomimetic Brigon structure reduced graphene oxide aerogel.
2. The preparation method according to claim 1, characterized in that: In step S1), the temperature of the bidirectional freezing directional assembly growth is below 0°C.
3. The preparation method according to claim 1, characterized in that: In step S1), the concentration of the graphene oxide suspension is 5 mg / mL to 20 mg / mL.
4. The preparation method according to claim 1, characterized in that: In step S2), the inter-layer deflection angle of the spiral stacking assembly is any angle between 15° and 90°.
5. The preparation method according to claim 1, characterized in that: In step S2), the number of layers to be spirally stacked and assembled is 2 or more.
6. The preparation method according to claim 1, characterized in that: In step S2), the oriented graphene oxide frozen body thin layer is made into a reduced graphene oxide aerogel film, comprising the following steps: a) cross-linking the oriented graphene oxide frozen body thin layer under the action of a cross-linking agent to obtain a graphene oxide hydrogel; the cross-linking agent is selected from one or more of an ethanol solution of calcium chloride and an ethanol solution of ferric chloride; b) hydrothermally reducing the graphene oxide hydrogel obtained in step a) and then drying it to obtain a reduced graphene oxide aerogel film.
7. The bionic Brigon structure reduced graphene oxide aerogel obtained according to any one of the preparation methods described in claims 1 to 6.
8. A bionic Brigon structure reduced graphene oxide elastomer, characterized in that: comprising a frame and PDMS filled in the frame; The frame is obtained by reducing graphene oxide aerogel with a bionic Brigon structure obtained by the preparation method according to any one of claims 1 to 6.
9. A method for preparing a bionic Brigon structure reduced graphene oxide elastomer, characterized in that: include: The PDMS prepolymer and the cross-linking agent are filled into the biomimetic Brigon structure reduced graphene oxide aerogel for curing to obtain the biomimetic Brigon structure reduced graphene oxide elastomer; The bionic Brigon structure reduced graphene oxide aerogel is a bionic Brigon structure reduced graphene oxide aerogel obtained according to the preparation method according to any one of claims 1 to 6.
10. Application of the bionic Brigon structure reduced graphene oxide elastomer according to claim 8 or the bionic Brigon structure reduced graphene oxide elastomer obtained by the preparation method according to claim 9 in the fields of wearable devices, health detection or flexible electronic devices.
Citation Information
Patent Citations
High-temperature-resistant elastic graphene aerogel material and preparation method thereof
CN112536004A
Nuclear protection nanofiber aerogel with bionic structure and preparation method thereof
CN115478430A
Graphene aerogel with oriented ordered pore structure as well as preparation method and application of graphene aerogel
CN116059978A
Light tough fiber composite material imitating cavity ratchet scales and preparation method of light tough fiber composite material
CN118288629A
Cited By
High-throughput modeling and calculating method and system for metal-based composite material
CN120995785A
A high-throughput modeling and computing method and system for metal matrix composites