Active carbon based on Yili weakly viscous bituminous coal and preparation method thereof
By adding biomass and asphalt to the preparation process of Yili weak-visible bituminous coal activated carbon, the carbonization process is optimized, and the problems of insufficient mechanical strength and uneven pore size distribution are solved, and the adsorption performance and durability of activated carbon are improved.
Patent Information
- Application Number
- CN202411129162.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The mechanical strength of Yili weak viscous bituminous coal activated carbon is insufficient and the pore size distribution is uneven, resulting in low adsorption efficiency and durability.
After crushing and grinding, biomass and asphalt are added as binders. The carbonization process is optimized to improve pore structure and mechanical strength through extrusion molding and high-temperature carbonization activation.
It significantly improves the mechanical strength and adsorption properties of activated carbon, improves the pore size distribution, and enhances its durability and economic benefits.
Smart Images

Figure CN118993069A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of activated carbon, and in particular to activated carbon based on Yili weakly sticky bituminous coal and a preparation method thereof. Background Art
[0003] The main type of coal in the Yili region of Xinjiang is weakly sticky bituminous coal, which is better than the bituminous coal in the mainland. This type of coal has the characteristics of high calorific value, low ash content, extremely low sulfur content, and its moisture content is below 5%. Based on these excellent characteristics, Xinjiang Yili coal can be prepared into high-performance, high-value-added activated carbon products.
[0004] Due to its porosity and high adsorption properties, activated carbon is widely used in environmental governance and industrial refining. By utilizing deep processing of coal to prepare activated carbon, the application areas of coal products can be expanded, and cleaner and more efficient resource development can be achieved, which can not only have a positive impact on the environment, but also improve economic benefits.
[0005] According to the previous investigation on Ili coal, the carbonization process and structural characteristics of weakly sticky bituminous coal were analyzed. The results showed that due to the relatively low volatile matter of weakly sticky bituminous coal raw materials, it exhibited high density and large molecular cohesion in the carbonization product, was not easy to soften and plasticize, and the structure was more likely to disintegrate during the carbonization process. In addition, the generated pores were not fully developed and the pore size was not uniform, resulting in a small specific surface area of weakly sticky bituminous coal activated carbon, which was insufficient to form a strong network structure with excellent mechanical properties. It is particularly noteworthy that a large number of incomplete micropores and tiny cracks were observed in Ili weakly sticky bituminous coal, and these defects will undoubtedly further reduce the mechanical strength of the material and have an adverse effect on subsequent operations and processing. Summary of the invention
[0006] In view of the problems existing in the prior art, such as uneven pore structure and poor mechanical strength, in order to develop high-quality, high-performance activated carbon, the present invention proposes an activated carbon based on Yili weakly sticky bituminous coal and a preparation method thereof, which effectively improves the internal structure, significantly improves the mechanical strength of the activated carbon, and improves its adsorption efficiency and durability, in order to achieve the conversion of this type of coal into high value-added products.
[0007] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing activated carbon based on Yili weakly sticky bituminous coal, comprising the following steps:
[0008] Step 1, crushing and grinding the blocky Yili weakly sticky bituminous coal to obtain coal powder;
[0009] Step 2, fully kneading the coal powder, the binder and the water in a dosage ratio of 1000g:200g~400g:100mL~300mL to obtain a composition, wherein the binder is one or more of biomass, asphalt, phenolic resin and caustic soda;
[0010] Step 3, extruding the composition to obtain a columnar activated carbon precursor;
[0011] Step 4, high-temperature carbonization of the columnar activated carbon precursor, with a heating rate of 3°C / min to 5°C / min, a carbonization temperature of 500°C to 600°C, and a residence time of 45min to 70min to obtain a carbonized product;
[0012] Step 5. Activate the carbonized product at high temperature in a water vapor atmosphere at a heating rate of 3°C / min to 5°C / min, an activation temperature of 830°C to 930°C, and a residence time of 50min to 120min to obtain an activated carbon product.
[0013] Based on the above technical solution, the present invention can also be improved as follows.
[0014] Furthermore, in Step 1, the particle size of the lumpy Yili weakly sticky bituminous coal is 1 mm to 10 mm, and the particle size of more than 90% of the coal powder is 150 mesh to 250 mesh.
[0015] Furthermore, in Step 1, a crusher is used for the crushing process, and a ball mill is used for the grinding process.
[0016] Furthermore, after the lump Ili weakly sticky bituminous coal is broken, it is first dried at a temperature of 30°C to 80°C for 12h to 48h, and then ground.
[0017] Furthermore, the Step 2 binder is a mixture of biomass and asphalt, and the mass ratio of biomass to asphalt is 0.05 to 0.5:1.
[0018] Furthermore, the biomass is one or more of starch, cellulose, and lignin.
[0019] Furthermore, in Step 3, a hydraulic press is used for extrusion molding, the extrusion pressure is 5 MPa to 20 MPa, and the outer diameter of the columnar activated carbon precursor is 3 mm to 6 mm.
[0020] Furthermore, in Step 5, the water vapor atmosphere is generated by evaporation of liquid water, and the water flow rate is 6 mL / min to 12 mL / min.
[0021] Based on the above technical solution, the present invention also provides an activated carbon prepared by the preparation method.
[0022] Furthermore, it has at least one of the following characteristics:
[0023] The specific surface area of activated carbon is 600m 2 / g~900m 2 / g;
[0024] The iodine adsorption value of activated carbon is 750mg / g~950mg / g;
[0025] The strength of activated carbon is 85% to 99%;
[0026] The average pore size of activated carbon is 3nm to 20nm;
[0027] The micropore volume of activated carbon is 0.2 cm 3 / g~0.3cm 3 / g;
[0028] The mesopore volume of activated carbon is 0.7 cm 3 / g~0.9cm 3 / g.
[0029] The beneficial effects of the present invention are:
[0030] The present invention adds an appropriate amount of asphalt during the preparation of activated carbon, which can effectively improve the problems of insufficient mechanical strength and uneven pore size distribution in the preparation of activated carbon from Yili weakly sticky bituminous coal, as follows:
[0031] 1) Asphalt has a bonding effect, which can improve the plasticity of weakly sticky bituminous coal raw materials during the carbonization process and is conducive to the formation of a more developed pore structure;
[0032] 2) Asphalt contains rich aromatic components, which can increase the number of micropores and mesopores of activated carbon by cross-linking and reorganization at high temperature;
[0033] 3) Adding asphalt will increase the volatile content of weakly sticky bituminous coal, which helps to generate more pores during pyrolysis;
[0034] 4) The microdispersion of asphalt in the coal matrix can inhibit excessive agglomeration and control the pore size distribution to a certain extent;
[0035] 5) Asphaltene can cover the surface of coal-based micropores and improve the mechanical strength of activated carbon;
[0036] 6) Adding asphalt will increase the yield of weakly sticky bituminous coal, which can make up for the disadvantage of low yield of weakly sticky bituminous coal to a certain extent;
[0037] 7) Sulfur and nitrogen compounds contained in asphalt can also increase active sites and improve some adsorption properties;
[0038] In addition, biomass such as starch, lignin, and cellulose are added to the activated carbon binder of the present invention, and the specific effects are as follows:
[0039] 1) Increase porosity and specific surface area. Biomass such as starch, cellulose, and lignin can be pyrolyzed during the heating and carbonization process to generate pores, which increase the porosity and specific surface area of activated carbon;
[0040] 2) Improve the pore structure. The addition of biomass components can inhibit the excessive increase of the pore structure of activated carbon at high temperature, and fine-tune the pore structure to make its pore distribution more reasonable;
[0041] Finally, the present invention effectively improves the mechanical strength and adsorption performance of the activated carbon product by setting a suitable heating rate, and setting a suitable carbonization and activation retention temperature and retention time;
[0042] In addition, the preparation method is simple to operate, low in cost, and has high industrial application value. The raw material used for the activated carbon of the present invention is weakly sticky bituminous coal mined locally in Yili, which is not only of great significance to the research and development of coal resources in Xinjiang, but also provides an effective strategy for the efficient utilization of Xinjiang coal mine resources, thereby maintaining a higher economic yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 The DTG curve and TG curve of Yili weakly viscous bituminous coal;
[0044] Figure 2 This is a physical picture of the activated carbon prepared in Example 1 of the present invention;
[0045] Figure 3 This is a scanning electron microscope image of the activated carbon prepared in Example 1 of the present invention;
[0046] Figure 4 This is the XRD pattern of the activated carbon prepared in Example 1 of the present invention;
[0047] Figure 5 This is the XPS graph of the activated carbon prepared in Example 1 of the present invention;
[0048] Figure 6 This is the EDS image of the activated carbon prepared in Example 1 of the present invention;
[0049] Figure 7 The isothermal adsorption-desorption curve and pore size distribution diagram of the activated carbon prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0050] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0051] The method for testing the performance of the activated carbon products obtained in Example 1, Comparative Example 1 and Comparative Example 2 is as follows:
[0052] Pore diameter, specific surface area, and pore volume: The pore diameter and pore volume of the shaped activated carbon were tested using a physical adsorption instrument (Michiko Baier, Japan), and the specific surface area was calculated according to the BET theory;
[0053] Iodine adsorption value: GB / T 7702.7;
[0054] Strength: GB / T 7702.3;
[0055] Microporosity: GB / T 7702.20.
[0056] Figure 1 The DTG curve and TG curve of Yili weakly sticky bituminous coal show that the temperature before 200℃ is the stage of water evaporation and weight loss, and the temperature between 200℃ and 420℃ is the stage of coal sample oxidation and weight gain. In this stage, the coal is mainly chemically adsorbed, and the CH in the pores of the coal sample is completely oxidized at 250℃. 4 , CO 2 、N 2 The degassing reaction, taking into account the results of differential thermal-thermogravimetric analysis, the carbon activation temperature range is determined to be 400℃~950℃. According to empirical data, the carbonization time of Yili weakly sticky bituminous coal should not be too long, and 45min~70min is more appropriate. Example 1 Figure 2 , Figure 3 , Figure 4 As shown, a method for preparing activated carbon based on Yili weakly sticky bituminous coal comprises the following steps:
[0057] Step 1, put the blocky Yili weakly sticky bituminous coal into a crusher for crushing, take it out and dry it at 60°C for 24 hours, the obtained granular coal particle size is 1mm to 10mm, then add the granular coal into a ball mill for grinding to obtain coal powder, and more than 90% of the coal powder can pass through 200 mesh;
[0058] Step 2, take 1000g coal powder, 265g binder, and 200mL water, mix them thoroughly, take them out, and obtain a composition, wherein the binder is a mixture of 200g asphalt, 55g starch, and 10g cellulose;
[0059] Step 3, placing the composition in a hydraulic press with a pressure of 10 MPa, taking it out to obtain a 4 mm columnar activated carbon precursor;
[0060] Step 4, high-temperature carbonization of the columnar activated carbon precursor, controlling the heating rate to be 3°C / min, the temperature is raised to 500°C to 600°C, such as 530°C, 580°C, the carbonization time is 45min to 70min, such as 50min, 60min, and the activated carbon carbonized product is obtained;
[0061] Step 5. Activate the carbonized product at high temperature under a water vapor atmosphere, control the heating rate to 3°C / min, raise the temperature to 830°C~930°C, such as 880°C, 920°C, retain for 60 minutes, generate water vapor from water, and introduce water at a flow rate of 8.000mL / min. Take it out to obtain an activated carbon product.
[0062] pass Figure 3 From the SEM image, we can see that the activated carbon product is nanoparticles with a diameter of about 200nm, and is relatively evenly dispersed. It is mainly composed of mesopores and micropores, the pore size distribution is relatively concentrated, and there are relatively few macropores. Mesopores and micropores are also distributed and inlaid in the macropores, which greatly increases the specific surface area and adsorption performance of the activated carbon sample.
[0063] Figure 4 This is the XRD diagram of the activated carbon product obtained. By comparing the characteristic peaks in the figure, it can be seen that the activated carbon sample has an irregular carbon crystal structure. At the same time, it is found that it has two obvious broad diffraction peaks at 2θ=23° and 2θ=43°, representing the (002) plane and (100) plane of the graphite crystal type, respectively. This shows that the activated carbon sample contains microcrystals with a chaotic layer graphite structure, and this microcrystal structure is irregular, which enhances the activity of the surface atoms of the lump coal and forms a relatively developed pore structure, which is beneficial to the enhancement of the adsorption performance of the lump coal. In addition, a relatively obvious narrow diffraction peak appears at 2θ=32°, which corresponds to graphite crystalline carbon material, indicating that the material has good crystallinity.
[0064] Figure 5 The XPS diagram of the activated carbon product is shown in Figure 2. Figure 5 It can be seen that activated carbon is mainly composed of C and O elements, which is consistent with the XRD results. In addition, Ca and S elements can also be found in the spectrum, indicating the presence of inorganic salts in the raw coal.
[0065] Figure 6 The EDS (energy spectrum) diagram of the activated carbon product is obtained. The element types and contents in the activated carbon product are analyzed by X-ray energy spectrum technology, such as Figure 6 As shown, characteristic peaks of C, O, Mg, Al, S, Ca and Fe elements can be seen, among which the C peak is narrower and has a higher peak intensity. The material is mainly composed of C and O, but also contains a small amount of impurities such as Mg, Al, S, Ca and Fe elements.
[0066] Figure 7 Isothermal adsorption-desorption curve and pore size distribution of activated carbon products. The specific surface area of activated carbon products is 727.75m 2 / g, the average pore diameter is 5.464nm, which belongs to the mesopore range, and the micropore volume is 0.2685cm 3 / g, and the mesopore volume is 0.818cm 3 / g, mesopores account for 75% of the total pore volume, and the total pore volume is 1.0865cm 3 / g, the mesopores mainly play the role of channels in the adsorption process, which can improve the mass transfer rate and adsorption efficiency of the adsorbate on the activated carbon.
[0067] The activated carbon product obtained in Example 1 meets the requirements of the national standard GB / T7701 for columnar activated carbon, with a strength of 93.2%, an iodine adsorption value of 910 mg / g, a carbon yield of 32%, and a BET specific surface area of 727.75 m 2 / g, the average pore diameter is 5.464nm, which belongs to the mesoporous range, and the micropore volume is 0.2685cm 3 / g, and the mesopore volume is 0.818cm 3 / g, mesopores account for 75% of the total pore volume, and the carbon tetrachloride adsorption rate is 56.9%.
[0068] Example 2
[0069] A method for preparing activated carbon based on Yili weakly sticky bituminous coal comprises the following steps:
[0070] Step 1, put the blocky Yili weakly sticky bituminous coal into a crusher for crushing, take it out and dry it at 60°C for 24 hours, the obtained granular coal particle size is 1mm to 10mm, then add the granular coal into a ball mill for grinding to obtain coal powder, and more than 90% of the coal powder can pass through 200 mesh;
[0071] Step 2, take 1000g coal powder, 280g binder, and 200mL water, mix them thoroughly, take them out, and obtain a composition, wherein the binder is a mixture of 250g asphalt, 20g phenolic resin and 10g cellulose;
[0072] Step 3, placing the composition in a hydraulic press with a pressure of 10 MPa, taking it out to obtain a 4 mm columnar activated carbon precursor;
[0073] Step 4, high-temperature carbonization of the columnar activated carbon precursor, controlling the heating rate to be 3°C / min, the temperature is raised to 500°C to 600°C, such as 530°C, 580°C, the carbonization time is 45min to 70min, such as 50min, 60min, and the activated carbon carbonized product is obtained;
[0074] Step 5. Activate the carbonized product at high temperature under a water vapor atmosphere, control the heating rate to 3°C / min, raise the temperature to 830°C~930°C, such as 880°C, 920°C, retain for 60 minutes, generate water vapor from water, and introduce water at a flow rate of 8.000mL / min. Take it out to obtain an activated carbon product.
[0075] The tested activated carbon product strength is 94.5%, the iodine adsorption value is 843 mg / g, the specific surface area is 678.2 m2 / g, and the carbon tetrachloride adsorption rate is 51.2%.
[0076] Example 3
[0077] A method for preparing activated carbon based on Yili weakly sticky bituminous coal comprises the following steps:
[0078] Step 1, put the blocky Yili weakly sticky bituminous coal into a crusher for crushing, take it out and dry it at 60°C for 24 hours, the obtained granular coal particle size is 1mm to 10mm, then add the granular coal into a ball mill for grinding to obtain coal powder, and more than 90% of the coal powder can pass through 200 mesh;
[0079] Step 2, take 1000g coal powder, 320g binder, and 200mL water, mix them thoroughly, take them out, and obtain a composition, wherein the binder is a mixture of 200g asphalt, 60g starch, 20g phenolic resin, 30g caustic soda and 10g cellulose;
[0080] Step 3, placing the composition in a hydraulic press with a pressure of 10 MPa, taking it out to obtain a 4 mm columnar activated carbon precursor;
[0081] Step 4, high-temperature carbonization of the columnar activated carbon precursor, controlling the heating rate to be 3°C / min, the temperature is raised to 500°C to 600°C, such as 530°C, 580°C, the carbonization time is 45min to 70min, such as 50min, 60min, and the activated carbon carbonized product is obtained;
[0082] Step 5. Activate the carbonized product at high temperature under a water vapor atmosphere, control the heating rate to 3°C / min, raise the temperature to 830°C~930°C, such as 880°C, 920°C, retain for 60 minutes, generate water vapor from water, and introduce water at a flow rate of 8.000mL / min. Take it out to obtain an activated carbon product.
[0083] The strength of the activated carbon product tested was 96.8%, the iodine adsorption value was 839 mg / g, and the specific surface area was 670.9 m 2 / g, carbon tetrachloride adsorption rate 55.2%.
[0084] Comparative Example 1
[0085] A method for preparing activated carbon based on Yili weakly sticky bituminous coal comprises the following steps:
[0086] Step 1, put the blocky Yili weakly sticky bituminous coal into a crusher for crushing, take it out and dry it at 60°C for 24 hours, the obtained granular coal has a particle size of 1mm to 10mm, and then add the granular coal into a ball mill for grinding to obtain coal powder, and more than 90% of the coal powder passes 200 mesh;
[0087] Step 2, take 1000g coal powder, 300g binder, and 200mL water, mix them thoroughly, take them out, and obtain a composition, wherein the binder is a mixture of 20g starch, 200g asphalt and 80g coal tar;
[0088] Step 3, placing the composition in a hydraulic press with a pressure of 10 MPa, taking it out to obtain a 4 mm columnar activated carbon precursor;
[0089] Step 4, high-temperature carbonization of the columnar activated carbon precursor, controlling the heating rate to be 3°C / min, the temperature is raised to 500°C to 600°C, such as 530°C, 580°C, the carbonization time is 45min to 70min, such as 50min, 60min, and the activated carbon carbonized product is obtained;
[0090] Step 5. Activate the carbonized product at high temperature under a water vapor atmosphere, control the heating rate to 3°C / min, raise the temperature to 830°C~930°C, such as 880°C, 920°C, retain for 120 minutes, water vapor is generated by the evaporation of liquid water, the flow rate of water is 8.000mL / min, take it out, and obtain the activated carbon product.
[0091] The tested strength of the activated carbon product was 9%. Since the activation retention time was 120 minutes, it was over-activated for this type of coal, causing its pore structure to continue to expand, eventually leading to structural collapse and a significant drop in strength.
[0092] Comparative Example 2
[0093] A method for preparing activated carbon based on Yili weakly sticky bituminous coal comprises the following steps:
[0094] Step 1, put the blocky Yili weakly sticky bituminous coal into a crusher for crushing, take it out and dry it at 60°C for 24 hours, the obtained granular coal has a particle size of 1mm to 10mm, and then add the granular coal into a ball mill for grinding to obtain coal powder, and more than 90% of the coal powder passes 200 mesh;
[0095] Step 2, take 1000g coal powder, 330g binder, and 200mL water, mix them thoroughly, take them out, and obtain a composition, wherein the binder is a mixture of 100g starch, 30g cellulose, and 200g tar;
[0096] Step 3, placing the composition in a hydraulic press with a pressure of 10 MPa, taking it out to obtain a 4 mm columnar activated carbon precursor;
[0097] Step 4, high-temperature carbonization of the columnar activated carbon precursor, controlling the heating rate to be 3°C / min, the temperature is raised to 500°C to 600°C, such as 530°C, 580°C, the carbonization time is 45min to 70min, such as 50min, 60min, and the activated carbon carbonized product is obtained;
[0098] Step 5. Activate the carbonized product at high temperature under a water vapor atmosphere, control the heating rate to 3°C / min, raise the temperature to 830°C~930°C, such as 880°C, 920°C, retain for 60 minutes, generate water vapor from water, and introduce water at a flow rate of 8.000mL / min. Take it out to obtain an activated carbon product.
[0099] The tested strength of the activated carbon product was 36%, and the iodine adsorption value was 763 mg / g. The strength dropped significantly without adding asphalt. In addition, due to the large amount of starch added, the starch produced larger pores during thermal decomposition and was easy to disintegrate, resulting in a decrease in the iodine adsorption value and a further decrease in strength.
[0100] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing activated carbon based on Yili weakly sticky bituminous coal, It is characterized in that The steps include: Step 1, crushing and grinding the blocky Yili weakly sticky bituminous coal to obtain coal powder; Step 2, fully kneading the coal powder, the binder and the water in a dosage ratio of 1000g:200g~400g:100mL~300mL to obtain a composition, wherein the binder is one or more of biomass, asphalt, phenolic resin and caustic soda; Step 3, extruding the composition to obtain a columnar activated carbon precursor; Step 4, high-temperature carbonization of the columnar activated carbon precursor, with a heating rate of 3°C / min to 5°C / min, a carbonization temperature of 500°C to 600°C, and a residence time of 45min to 70min to obtain a carbonized product; Step 5. Activate the carbonized product at high temperature in a water vapor atmosphere at a heating rate of 3°C / min to 5°C / min, an activation temperature of 830°C to 930°C, and a residence time of 50min to 120min to obtain an activated carbon product.
2. The method for preparing activated carbon based on Yili weakly sticky bituminous coal according to claim 1, It is characterized in that In Step 1, the particle size of the lumpy Yili weakly sticky bituminous coal is 1mm to 10mm, and the particle size of more than 90% of the coal powder is 150 mesh to 250 mesh.
3. A method for preparing activated carbon based on Yili weakly sticky bituminous coal according to claim 1 or 2, It is characterized in that In Step 1, a crusher is used for crushing, and a ball mill is used for grinding.
4. A method for preparing activated carbon based on Yili weakly sticky bituminous coal according to claim 1, 2 or 3, It is characterized in that After the lump Ili weakly sticky bituminous coal is broken, it is first dried at 30℃~80℃ for 12h~48h and then ground.
5. The method for preparing activated carbon based on Yili weakly sticky bituminous coal according to claim 1, It is characterized in that In Step 2, the binder is a mixture of biomass and asphalt, and the mass ratio of biomass to asphalt is 0.05 to 0.5:
1.
6. The method for preparing activated carbon based on Yili weakly sticky bituminous coal according to claim 5, It is characterized in that The biomass is one or more of starch, cellulose and lignin.
7. The method for preparing activated carbon based on Yili weakly sticky bituminous coal according to claim 1, It is characterized in that In Step 3, a hydraulic press is used for extrusion molding, the extrusion pressure is 5MPa to 20MPa, and the outer diameter of the columnar activated carbon precursor is 3mm to 6mm.
8. The method for preparing activated carbon based on Yili weakly sticky bituminous coal according to claim 1, It is characterized in that In Step 5, the water vapor atmosphere is generated by evaporation of liquid water, and the water flow rate is 6 mL / min to 12 mL / min.
9. An activated carbon, It is characterized in that The method is prepared according to any one of claims 1 to 8.
10. The activated carbon according to claim 9, It is characterized in that It has at least one of the following characteristics: The specific surface area of the activated carbon is 600m 2 / g~900m 2 / g; The iodine adsorption value of the activated carbon is 750 mg / g to 950 mg / g; The strength of the activated carbon is 85% to 99%; The average pore size of the activated carbon is 3nm to 20nm; The micropore volume of the activated carbon is 0.2 cm 3 / g~0.3cm 3 / g; The mesopore volume of the activated carbon is 0.7 cm 3 / g~0.9cm 3 / g.
Citation Information
Patent Citations
Columnar activated carbon based on coal pitch binders and preparation method of columnar activated carbon
CN102674341A
Biomass gasification residue formed activated carbon and preparation method thereof
CN109160512A
Active carbon
CN110078073A
Coal columnar activated carbon and preparation method thereof
CN110877909A
Method for preparing activated carbon by using novel adhesive
CN112010303A