Photosensitive glass, preparation method thereof, reinforced photosensitive glass and application

By adjusting the raw material composition of the photosensitive glass, the problems of Ag2O decomposition on precious metal containers are solved, and glass stability and optical signal shielding effect are achieved after melting and radiation treatment.

CN118993537AActive Publication Date: 2024-11-22CHONGQING AUREAVIA HI TECH GLASS CO LTD

Patent Information

Application Number
CN202411102134.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

There are stability problems in the melting process of photosensitive glass containing Ag2O. The silver atom Ag0 produced by decomposition of Ag2O will cause losses and damage to precious metal containers. At the same time, the optical transmittance is significantly reduced after UV exposure, affecting the shielding effect of the optical signal.

Method used

By controlling the raw material composition of the photosensitive glass, it includes 50 wt% to 60 wt% silica sand, 15 wt% to 22 wt% lithium carbonate, 6 wt% to 10 wt% aluminum hydroxide, 3 wt% to 6 wt% potassium nitrate, 3 wt% to 5 wt% zirconia, 0.3% to 0.6% silver nitrate, 0.05% to 0.10% cerium oxide and pentavalent antimony salt ensure stability of the glass components and form a low transmittance exposure after radiation and heat treatment. area.

Benefits of technology

It realizes the stability of the glass component during the melting process, avoids the erosion and damage of Ag0 to the precious metal container, and realizes effective shielding of optical signals in the visible light and near-infrared wavelength ranges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993537A_ABST
    Figure CN118993537A_ABST
Patent Text Reader

Abstract

According to the photosensitive glass, the preparation method thereof, the reinforced photosensitive glass and the application, by controlling the raw material composition of the photosensitive glass, the stability of glass components in the melting process of the photosensitive glass containing Ag2O can be ensured, and the problem that a precious metal container is damaged and damaged by silver atoms Ag0 generated by decomposition of Ag2O is solved; and moreover, when the photosensitive glass is obtained after radiation treatment and heat treatment, the optical transmittance of an exposure area in a visible light and near-infrared wavelength range is extremely low, and optical signals can be shielded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of glass technology, and in particular to a photosensitive glass and a preparation method thereof, strengthened photosensitive glass and uses thereof. Background Art

[0002] Photosensitive glass can respond to external light stimulation. Under certain lighting conditions, the glass structure and phase will change, showing different mechanical and optical properties. Photosensitive glass containing Ag is the most common type of photosensitive glass, and Ag is usually combined with Ce ions and Sb ions. During the melting process, Sb 3+ Can transfer electrons to Ce 4+ Restore it to Ce 3+ , in further UV exposure Ce 3+ Can transfer electrons to Ag + Restore it to Ag 0 , Ag 0 As the growth center of colloidal Ag crystals, subsequent heat treatment can lead to the precipitation and growth of Ag colloids. Due to the close lattice constants, Ag colloidal crystals can induce the precipitation of lithium metasilicate crystals. Based on the above reaction chain principle, Corning and Schott have developed Fotoform / Fotoceram and Foturan products respectively. Through subsequent etching of glass, micro-area mechanical processing of glass can be achieved for MEMS, TGV and microfluidic glass chips, etc.

[0003] There are many problems in the melting process of photosensitive glass containing Ag. For example, using corundum and quartz containers will have a great impact on the final glass components during the high-temperature melting process, and the melting container is also easy to break; while using precious metal containers (especially platinum, rhodium and other metal containers), Ag in the glass component will corrode the container, and long-term melting will cause serious loss and damage to the container (melting containers include crucibles, kilns, channels, etc.). Therefore, ensuring the stability of melting, maintaining the stability of glass components, and reducing and avoiding damage to the container during the melting process are technical problems that need to be solved urgently.

[0004] The application of this system of photosensitive glass is mainly concentrated in glass micromachining, and its application in optics has not yet been reported. In fact, in the UV exposure area, the optical transmittance of the photosensitive glass will be significantly reduced with the precipitation of colloidal Ag crystals and lithium silicate crystals. This feature makes Ag photosensitive microcrystalline glass applicable to the shielding of optical signals. Through UV exposure combined with the process of masking specific areas, the shielding of optical signals in a certain wavelength range in specific areas can be achieved.

[0005] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0006] The purpose of the present application is to provide a photosensitive glass, which can not only ensure the stability of the glass components during the melting process of the photosensitive glass containing Ag2O, but also solve the problem of silver atoms Ag generated by the decomposition of Ag2O. 0 It can not only solve the problem of loss and damage of precious metal containers, but also ensure that when photosensitive glass is obtained after radiation treatment and heat treatment, the optical transmittance of the exposed area in the visible light and near-infrared wavelength range is extremely low, thereby shielding optical signals.

[0007] In order to achieve the above objectives, this application provides the following technical solutions:

[0008] In a first aspect, a photosensitive glass is provided, which comprises the following components, calculated by the mass percentage of each raw material component in the photosensitive glass: 50wt% to 60wt% of silica sand, 15wt% to 22wt% of lithium carbonate, 6wt% to 10wt% of aluminum hydroxide, 3wt% to 6wt% of potassium nitrate, 3wt% to 6wt% of sodium nitrate, 3wt% to 5wt% of zirconium oxide, 0.3wt% to 0.6wt% of silver nitrate, 0.05wt% to 0.10wt% of cerium oxide, and pentavalent antimony salt; wherein, calculated as sodium antimonate, the mass percentage of the pentavalent antimony salt in the composition of the photosensitive glass is 0.3wt% to 0.8wt%.

[0009] As an optional implementation scheme, the composition of the photosensitive glass includes the following components according to the mass percentage of each raw material component in the photosensitive glass:

[0010] The content of silica sand is 53wt% to 59wt%, preferably 54.00wt% to 58.96wt%, and / or

[0011] The content of lithium carbonate is 17wt% to 20wt%, preferably 17.43wt% to 19.94wt%, and / or,

[0012] The content of aluminum hydroxide is 8wt% to 10wt%, preferably 8.22wt% to 9.97wt%, and / or

[0013] The content of potassium nitrate is 4wt% to 6wt%, preferably 4.07wt% to 5.97wt%, and / or,

[0014] The content of sodium nitrate is 3.5wt% to 5.5wt%, preferably 3.77wt% to 5.45wt%, and / or

[0015] The content of zirconium oxide is 3.33wt% to 5wt%, preferably 3.33wt% to 4.96wt%, and / or

[0016] The content of silver nitrate is 0.3wt% to 0.5wt%, preferably 0.32wt% to 0.49wt%, and / or

[0017] The content of cerium oxide is 0.05wt% to 0.09wt%, preferably 0.06wt% to 0.09wt%, and / or

[0018] The content of the pentavalent antimony salt is 0.3 wt % to 0.7 wt %, and preferably the content of the pentavalent antimony salt is 0.3 wt % to 0.5 wt %.

[0019] As an optional embodiment, the pentavalent antimony salt includes at least one of NaSbO3, KSbO3, NH4SbO3 and hydrates thereof.

[0020] As an optional embodiment, the thickness of the photosensitive glass is 0.4-2.0 mm.

[0021] As an optional embodiment, the photosensitive glass includes an exposure area and a non-exposure area. When the thickness of the photosensitive glass is 0.40mm~1.00mm, the transmittance T1 of the exposure area of ​​the photosensitive glass at a wavelength of 850nm is 0.00%~5.00%, and preferably the transmittance T1 is 0.00%~3%, and / or, when the thickness of the photosensitive glass is 0.40mm~1.00mm, the transmittance T2 of the exposure area of ​​the photosensitive glass at a wavelength of 550nm is 0.00%~5.00%, and preferably the transmittance T2 is 0.00%~2%, and / or, when the thickness of the photosensitive glass is 0.40mm~1.00mm, the transmittance T3 of the non-exposure area of ​​the photosensitive glass at a wavelength of 850nm is greater than 90%, and / or, when the thickness of the photosensitive glass is 0.40mm~1.00mm, the transmittance T4 of the non-exposure area of ​​the photosensitive glass at a wavelength of 550nm is greater than 90%.

[0022] In a second aspect, a method for preparing the photosensitive glass as described above is provided, comprising:

[0023] The raw material components are configured, then mixed and melted in a noble metal container, then formed, and then annealed to obtain a substrate glass;

[0024] The substrate glass comprises a first region and a second region, the first region is subjected to masking treatment, and the second region is not subjected to masking treatment, so as to obtain the masked substrate glass;

[0025] After the masked substrate glass is subjected to radiation treatment and heat treatment, a photosensitive glass having a non-exposed area and an exposed area is obtained; wherein the non-exposed area corresponds to the first area, and the exposed area corresponds to the second area.

[0026] As an optional embodiment, the noble metal container is a container made of at least one metal selected from the group consisting of gold, platinum and rhodium.

[0027] As an optional implementation scheme, the melting temperature is 1400° C. to 1650° C., and the melting time is 6 h to 48 h.

[0028] As an optional implementation scheme, the annealing temperature is 400° C. to 500° C., and the annealing time is 8 h to 24 h.

[0029] As an optional embodiment, the masking process includes masking using a masking ink and / or a mask plate.

[0030] As an optional embodiment, the radiation treatment comprises ultraviolet irradiation treatment.

[0031] As an optional embodiment, the wavelength of the ultraviolet irradiation treatment is 300nm-320nm, and the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 ~360mw / cm 2 The UV irradiation treatment time is 5min to 60min.

[0032] As an optional embodiment, the heat treatment includes a nucleation treatment and a crystallization treatment.

[0033] As an optional embodiment, the heating rate of the nucleation treatment is 1°C / min to 10°C / min; and / or,

[0034] The temperature of the nucleation treatment is 430°C to 540°C; and / or,

[0035] The time of the nucleation treatment is 30 minutes to 360 minutes, and / or,

[0036] The heating rate of the crystallization treatment is 1°C / min to 10°C / min; and / or,

[0037] The temperature of the crystallization treatment is 540°C to 800°C; and / or,

[0038] The crystallization treatment time is 30min to 480min.

[0039] As an optional embodiment, the thickness of the substrate glass is 0.4-2.0 mm.

[0040] In a third aspect, a strengthened photosensitive glass is provided, characterized in that the glass has a thickness of t, comprises a strengthening layer and a tensile stress layer, the strengthening layer extends from the surface of the strengthened photosensitive glass toward the inside, and the thickness of the strengthening layer is 0 to 0.22t.

[0041] The center of the tensile stress layer and / or the strengthened photosensitive glass comprises the following components, calculated as a percentage by mass of oxides:

[0042] SiO2: 65% to 74.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.90% to 12.00%, Na2O: 1.00% to 3.00%, K2O: 1.50% to 3.80%, ZrO2: 3.5% to 6.50%, Ag2O: 0.20% to 0.50%, CeO2: 0.07% to 0.13% and Sb2O3: 0.2% to 0.50%;

[0043] The strengthening layer, expressed in terms of oxide mass percentage, comprises the following components:

[0044] SiO2: 65% to 74.00%, Al2O3: 5.00% to 10.00%, Na2O: 4.00% to 16.00%, K2O: 2.0% to 5.0%, ZrO2: 3.5% to 6.50%, Ag2O: 0.20% to 0.50%, CeO2: 0.07% to 0.13% and Sb2O3: 0.2% to 0.50%; the content of Li2O in the strengthening layer is lower than the content of Li2O in the center of the tensile stress layer and / or the strengthened photosensitive glass;

[0045] Among them, Na2O is obtained from sodium nitrate, K2O is obtained from potassium nitrate, Ag2O is obtained from silver nitrate, and Sb2O3 is obtained from pentavalent antimony salt;

[0046] The tempered photosensitive glass includes a non-exposed area and an exposed area.

[0047] As an optional embodiment, t is 0.4-2.0 mm.

[0048] As an optional implementation scheme, the single-bar static pressure strength of the tempered photosensitive glass is above 200N, preferably 200N to 500N, and more preferably 200N to 490N.

[0049] In a fourth aspect, a cover glass is provided, which is made of the photosensitive glass of any embodiment of the first aspect, the photosensitive glass prepared by the method for preparing the photosensitive glass provided in any embodiment of the second aspect, or the strengthened photosensitive glass of any embodiment of the third aspect.

[0050] In a fifth aspect, an electronic device is provided, comprising the photosensitive glass of any embodiment of the first aspect, the photosensitive glass prepared by the method for preparing photosensitive glass provided in any embodiment of the second aspect, or the strengthened photosensitive glass of any embodiment of the third aspect.

[0051] As an optional embodiment, the electronic device includes a shell having a top and a bottom, and the bottom shell includes photosensitive glass such as the photosensitive glass of any embodiment of the first aspect or photosensitive glass prepared by the method for preparing photosensitive glass provided in any embodiment of the second aspect, or the strengthened photosensitive glass of the third aspect.

[0052] As an optional embodiment, the electronic device also includes a camera assembly, and the housing of the electronic device includes a camera protection cover, which is disposed on the camera assembly, and the camera protection cover includes photosensitive glass as described in any embodiment of the first aspect or photosensitive glass prepared by the method for preparing photosensitive glass provided in any embodiment of the second aspect, or the strengthened photosensitive glass of the third aspect.

[0053] In the sixth aspect, the use of the photosensitive glass according to any embodiment of the first aspect, the photosensitive glass prepared by the method for preparing the photosensitive glass provided by any embodiment of the second aspect, or the tempered photosensitive glass according to any embodiment of the third aspect for use in components in mobile phones, smart watches, wearable devices, camera modules or vehicles is provided.

[0054] One or more of the above technical solutions provided by the present application have the following advantages compared with the prior art:

[0055] By controlling the raw material composition of photosensitive glass, it is possible to ensure the stability of the glass composition during the melting process of photosensitive glass containing Ag2O, and solve the problem of silver atoms Ag generated by the decomposition of Ag2O. 0 It can not only solve the problem of loss and damage of precious metal containers, but also ensure that when photosensitive glass is obtained after radiation treatment and heat treatment, the optical transmittance of the exposed area in the visible light and near-infrared wavelength range is extremely low, thereby shielding optical signals. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0057] Figure 1 A schematic diagram of the structure of a substrate glass after being masked with masking ink provided in an embodiment of the present application.

[0058] Figure 2 A schematic diagram of the structure of the photosensitive glass provided in the embodiment of the present application.

[0059] Figure 3 The electronic device provided for the implementation manner of the present application is a structural schematic diagram of a mobile phone.

[0060] Figure 4 This is a schematic diagram of the structure of a smart watch in which the electronic device mentioned in the implementation manner of the present application is a smart watch.

[0061] Figure 5 These are photographs of the inside of the crucible after melting of Examples 9 to 10 and Comparative Examples 1 to 2 of the present application; wherein a. a photograph of the bottom of the crucible of Comparative Example 1, b. a photograph of the bottom of the crucible of Comparative Example 2, c. a photograph of the bottom of the crucible of Example 9, d. a photograph of the bottom of the crucible of Example 10.

[0062] Figure 6 This is a physical picture of the shielding of the exposure area of ​​Examples 9 to 10 of the present application and Comparative Examples 1 to 3 within the visible light range. The bright light spots in Comparative Examples 1-3 pass through red light.

[0063] Figure numerals: 11 - light-transmitting area; 12 - light-shielding area; 21 - exposure area; 22 - non-exposure area; 31 - camera protection cover; 32 - camera assembly; 33 - back cover; 41 - shell at the bottom of the smart watch. DETAILED DESCRIPTION

[0064] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0065] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all refer to including or not including (or may have or may not have). "And / or" as referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.

[0066] Explanation of terms and test methods:

[0067] In the present application, the main surface refers to the surface with the largest surface area, such as the upper surface or the lower surface of a horizontally placed substrate glass.

[0068] In the present application, when light of a certain wavelength is irradiated onto the main surface of the photosensitive glass, the light will be reflected, absorbed and transmitted, wherein the ratio of the intensity of the transmitted part to the intensity of the incident light is the transmittance.

[0069] In this application, the thickness of the glass is measured by a micrometer.

[0070] In the present application, the size specifications of the glass sheets are tested using a two-dimensional measuring machine (instrument model: MiyuMY~YXCL~4030).

[0071] Main surface Ag / Ag2O concentration test

[0072] The surface Ag / Ag2O concentration of the photosensitive glass in this application was measured by X-ray fluorescence spectrometer (XRF), and the test equipment used was Thermo Scientific ARL TM PERFORM'X. The target material is Rh (rhodium), the light tube voltage is 40KW, the current is 60mA, the collimator is 0.15, the crystal is LiF200, the detector is FPC, the test range is 29mm circle, and the analysis software is UniQuant non-standard analysis. XRF testing uses non-standard testing, and the concentration of elements or their oxides with atomic numbers 6 and below in the glass is not tested. For example, SiO2, Al2O3, Na2O, K2O, etc. can be accurately tested, while Li2O, B2O3, etc. cannot be accurately tested. That is, in this application, when the surface Ag / Ag2O concentration is tested by XRF, the total mass of the surface elements or their oxides does not include the mass of the elements or their oxides with atomic numbers 6 and below in the glass.

[0073] In the present application, an ultraviolet-visible spectrophotometer is used to test the transmittance of the exposed area and the non-exposed area of ​​the glass to be tested. The ultraviolet-visible spectrophotometer used in the test of the present application is Shimadzu UV-2000 ultraviolet-visible spectrophotometer.

[0074] The specific method for testing the exposure area of ​​the glass to be tested is: first use a fixture that is consistent with the shape and size of the glass to be tested, and the same area corresponding to the exposure area of ​​the glass to be tested is a hollow area and the non-exposure area corresponding to the glass to be tested is an opaque area, and the connection position between the hollow area and the opaque area is an opaque fixture as a blank sample for test calibration, and then cut the exposure area of ​​the glass to be tested into samples that coincide with the shape of the hollow area of ​​the fixture and put them into the hollow area of ​​the aforementioned fixture for testing to obtain the transmittance. Use an ultraviolet-visible spectrophotometer to test the transmittance of the exposure area of ​​5 pieces of glass to be tested in the same batch to light of different wavelengths, and then take the average value, which is recorded as the transmittance result of the exposure area of ​​the glass to be tested under the wavelength of light.

[0075] In addition, the transmittance of the non-exposed area of ​​5 pieces of tested glass in the same batch to light of different wavelengths was tested using an ultraviolet-visible spectrophotometer. The average value of the transmittance of the non-exposed area of ​​the 5 pieces of tested glass under light of different wavelengths was taken and recorded as the transmittance result of the non-exposed area of ​​the tested glass under the light of the wavelength.

[0076] In this application, the test of single-rod static pressure strength can be: place the glass sample to be tested on the bottom ring of the tensile testing machine (LT-850A), start the test software, and set the moving speed of the extrusion rod (rod diameter 8mm, pressure head arc radius 10mm) to 50mm / min, click to start the test, the extrusion rod will apply force to the center of the glass sample to be tested at the set moving speed until the glass sample cracks and breaks. The test software will automatically read the force (N) when the glass sample breaks as the test result. Take 10 glass samples in the same state for testing, and take the average value of the test results as the single-rod static pressure strength of the glass sample to be tested.

[0077] In the present application, the wavelength range of visible light and near infrared light refers to 400 nm to 1000 nm.

[0078] In this application, the glass component contains Ag2O, which undergoes the following reversible reaction during the melting process:

[0079]

[0080] The decomposition of silver atoms Ag 0 Therefore, in order to prevent the Ag2O from decomposing and producing 0 The precious metal container of the mixed melting raw materials is corroded and damaged. In this application, various raw material components other than Ag2O that can provide oxygen atmosphere are used for melting to inhibit the conversion of Ag2O into Ag. 0; The raw material components that can preferably provide an oxygen atmosphere include nitrates and / or pentavalent antimony salts, etc. Specifically, nitrates are used as raw material components, including NaNO3, KNO3, AgNO3, etc. Nitrates will decompose to produce O2 during the melting process. The specific reaction is as follows, and then providing an oxidizing atmosphere can inhibit the decomposition of Ag2O.

[0081]

[0082] In addition, pentavalent antimony salts including NaSbO3, KSbO3, NH4SbO3 and their hydrates can also decompose to produce oxygen atmosphere during the melting process, thereby inhibiting the conversion of Ag2O to Ag 0 ; Taking NaSbO3 as an example, the specific reaction is as follows:

[0083] 2NaSbO3→Na2O+Sb2O3+O2↑

[0084] In addition, Sb 5+ Sb produced by the decomposition of antimony salts during the melting process 3+ Can act as a reducing agent to convert Ce into 4 + Restore to Ce 3+ , maintain Ce 3+ The effective content of Ce; and then in the later exposure area of ​​the photosensitive glass under radiation conditions such as ultraviolet irradiation, 3+ Ag + Reduction to Ag 0 , Ag 0 As a growth center, the Ag 0 Cluster nuclei induce the precipitation of lithium metasilicate crystals.

[0085] The present invention controls the composition of the photosensitive glass to ensure that the photosensitive glass containing Ag2O remains stable during the melting process and does not contain Ag. 0 Produce and then solve the Ag generated by the decomposition of Ag2O 0 It can not only solve the problem of corrosion and damage to the molten precious metal container, but also ensure that after radiation treatment and heat treatment, the exposed area of ​​the photosensitive glass forms an opaque area, thereby shielding the optical signal in the visible light and near-infrared wavelength range.

[0086] In some embodiments of the present application, a photosensitive glass is provided, which comprises the following components, calculated by the mass percentage of each raw material component in the photosensitive glass: 50wt% to 60wt% of silica sand, 15wt% to 22wt% of lithium carbonate, 6wt% to 10wt% of aluminum hydroxide, 3wt% to 6wt% of potassium nitrate, 3wt% to 6wt% of sodium nitrate, 3wt% to 5wt% of zirconium oxide, 0.3wt% to 0.6wt% of silver nitrate, 0.05wt% to 0.10wt% of cerium oxide, and pentavalent antimony salt; wherein, calculated as sodium antimonate, the mass percentage of the pentavalent antimony salt in the composition of the photosensitive glass is 0.3wt% to 0.8wt%.

[0087] The type of crystals precipitated from the photosensitive glass during the crystallization process is mainly lithium metasilicate (Li2SiO3), and the precipitation of Li2SiO3 is beneficial to reducing the optical transmittance of the exposure area of ​​the photosensitive glass, and is beneficial to the shielding of optical signals by the photosensitive glass in the visible light and near-infrared wavelength range. In the present application, SiO2 is a glass-forming oxide, which serves as the network skeleton of the glass and is derived from silica sand. In some embodiments of the present application, according to the mass percentage of each component of the raw material in the photosensitive glass, the content of silica sand is 53wt% to 60wt%, preferably 53wt% to 59wt%, and more preferably 54.00wt% to 58.96wt%.

[0088] In some embodiments of the present application, according to the mass percentage of each raw material component in the photosensitive glass, the content of silica sand can be 53wt%, 53.5wt%, 54wt%, 54.5wt%, 55wt%, 55.5wt%, 56wt%, 56.5wt%, 57wt%, 57.5wt%, 58wt%, 58.5wt%, 58.96wt%, 59wt% or 60wt%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0089] In some embodiments of the present application, according to the mass percentage of each component of the raw material in the photosensitive glass, the mass percentage of lithium carbonate is 15wt% to 22wt%, preferably 15wt% to 20wt%, and more preferably 17wt% to 20wt%. In some embodiments of the present application, according to the mass percentage of each component of the raw material in the photosensitive glass, the content of lithium carbonate can be 15wt%, 16wt%, 17wt%, 17.43wt%, 17.5wt%, 18wt%, 18.5wt%, 19wt%, 19.5wt%, 19.94wt%, 20wt%, 21wt% or 22wt%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0090] In the present application, Al2O3, as a glass network intermediate, enters the glass network structure as [AlO4] tetrahedron, and alumina can increase the stability of the photosensitive glass, which is derived from aluminum hydroxide. In some embodiments of the present application, according to the mass percentage of each component of the raw material in the photosensitive glass, the content of aluminum hydroxide is 6wt% to 10wt%, preferably 8wt% to 10wt%, and more preferably 8.22wt% to 9.97wt%. In some embodiments of the present application, according to the mass percentage of each component of the raw material in the photosensitive glass, the content of aluminum hydroxide can be 6wt%, 7wt%, 8wt%, 8.22wt%, 8.5wt%, 8.7wt%, 9wt%, 9.2wt%, 9.5wt%, 9.7wt%, 9.97wt% or 10wt%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0091] In the present application, zirconium oxide (ZrO2) can improve the chemical stability of the photosensitive glass, but ZrO2 has a high melting point. When the amount added is too high, the melting temperature of the photosensitive glass will be increased. In some embodiments of the present application, according to the mass percentage of each component of the raw material in the photosensitive glass, the content of zirconium oxide is 3wt% to 5wt%, preferably 3.33wt% to 5wt%, and more preferably 3.33wt% to 4.96wt%. In some embodiments of the present application, according to the mass percentage of each component of the raw material in the photosensitive glass, the content of zirconium oxide can be 3.0wt%, 3.2wt%, 3.33wt%, 3.5wt%, 3.7wt%, 4.0wt%, 4.2wt%, 4.5wt%, 4.8wt%, 4.96wt% or 5.0wt%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0092] In this application, Na2O and K2O are glass network exogenous bodies and fluxes that can lower the melting point of glass. + , K + Existing situation, Na + , K + It will preferentially enter the aluminum-silicon-oxygen network to compensate for the electricity price, and to a certain extent maintain the lithium content in the lithium-rich area, making the Si / Li ratio in the lithium-rich area closer to the chemical ratio of Li2SiO3. Thus, the crystalline phase precipitated from the photosensitive glass containing Na2O and K2O is lithium metasilicate; and Na2O comes from sodium nitrate, and K2O comes from potassium nitrate. In this application, nitrates such as sodium nitrate, potassium nitrate and / or silver nitrate are combined with antimonates for better clarification effect, which in turn affects the transmittance and other properties of the finished product. Carbonates cannot achieve the transmittance effect of the finished product involved in this application.

[0093] In some embodiments of the present application, according to the mass percentage of each raw material component in the photosensitive glass, the content of sodium nitrate is 3.0-6.0wt%, preferably 3.5-5.5wt%, and more preferably 3.77wt%-5.45wt%. In some embodiments of the present application, according to the mass percentage of each raw material component in the photosensitive glass, the content of sodium nitrate can be 3.0wt%, 3.5wt%, 3.77wt%, 4.0wt%, 4.2wt%, 4.5wt%, 4.8wt%, 5wt%, 5.3wt%, 5.45wt% or 5.5wt%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0094] In some embodiments of the present application, according to the mass percentage of each raw material component in the photosensitive glass, the content of potassium nitrate is 3wt% to 6wt%, preferably 4wt% to 6wt%, and more preferably 4.07wt% to 5.97wt%. In some embodiments of the present application, according to the mass percentage of each raw material component in the photosensitive glass, the content of potassium nitrate can be 3.0wt%, 4.0wt%, 4.07wt%, 4.2wt%, 4.5wt%, 4.7wt%, 5.0wt%, 5.2wt%, 5.5wt%, 5.8wt%, 5.97wt% or 6.0wt%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0095] In some embodiments of the present application, according to the mass percentage of each raw material component in the photosensitive glass, the content of silver nitrate is 0.3wt% to 0.6wt%, preferably 0.30wt% to 0.5wt%, and more preferably 0.32wt% to 0.49wt%. In some embodiments of the present application, according to the mass percentage of each raw material component in the photosensitive glass, the content of silver nitrate can be 0.30wt%, 0.32wt%, 0.35wt%, 0.37wt%, 0.40wt%, 0.43wt%, 0.45wt%, 0.49wt%, 0.50wt% or 0.60wt%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0096] Cerium oxide (CeO2) is a photosensitizer. In the UV exposure process, it is Ag + Provide electrons. In some embodiments of the present application, according to the mass percentage of each raw material component in the photosensitive glass, the content of cerium oxide is 0.05wt% to 0.10wt%, preferably 0.05wt% to 0.09wt%, and more preferably 0.06wt% to 0.09wt%. In some embodiments of the present application, according to the mass percentage of each raw material component in the photosensitive glass, the content of cerium oxide can be 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt% or 0.10wt%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0097] In some embodiments of the present application, in order to ensure that Sb 5+The amount is sufficient. In the present application, calculated as sodium antimonate, according to the mass percentage of each raw material component in the photosensitive glass, the content of pentavalent antimony salt is 0.3wt% to 0.8wt%, preferably 0.31wt% to 0.5wt%, and more preferably 0.31wt% to 0.49wt%.

[0098] In some embodiments of the present application, the content of pentavalent antimony salt can be 0.30wt%, 0.31wt%, 0.33wt%, 0.35wt%, 0.38wt%, 0.40wt%, 0.43wt%, 0.45wt%, 0.48wt%, 0.49wt% or 0.50wt% based on the mass percentage of each component of the raw material in the photosensitive glass, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0099] It should be noted that pentavalent antimony salts include but are not limited to sodium antimonate, potassium antimonate, ammonium antimonate and / or hydrates thereof. In the present application, different types of pentavalent antimony salts are converted to sodium antimonate.

[0100] In some embodiments of the present application, the pentavalent antimony salt includes at least one of NaSbO3, KSbO3, NH4SbO3 and hydrates thereof.

[0101] In the present application, the photosensitive glass includes an exposed area and a non-exposed area, the exposed area has a low transmittance in the visible light and near-infrared wavelength range, and the non-exposed area has a high transmittance in the visible light and near-infrared wavelength range. In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40 mm to 1.00 mm, the transmittance T1 of the exposed area of ​​the photosensitive glass at a wavelength of 850 nm is 0.00% to 5.00%, and preferably the transmittance T1 is 0.00% to 3%. In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40 mm to 1.00 mm, the transmittance T1 of the exposure area of ​​the photosensitive glass at a wavelength of 850 nm can be 0.00%, 0.22%, 0.50%, 0.88%, 0.96%, 1.00%, 1.27%, 1.55%, 1.59%, 1.64%, 2.00%, 2.30%, 2.51%, 3.00%, 3.50%, 4.00%, 4.50%, 4.80% or 5.00%; or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0102] In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40 mm to 1.00 mm, the transmittance T2 of the exposure area of ​​the photosensitive glass at a wavelength of 550 nm is 0.00% to 5.00%, and the transmittance T2 is preferably 0.00% to 2%. In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40 mm to 1.00 mm, the transmittance T2 of the exposure area of ​​the photosensitive glass at a wavelength of 550 nm can be 0.00%, 0.20%, 0.50%, 0.70%, 0.90%, 1.00%, 1.35%, 1.50%, 1.70%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, 4.20%, 4.50%, 4.90% or 5.00%; or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.

[0103] In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40 mm to 1.00 mm, the transmittance T3 of the non-exposed area of ​​the photosensitive glass at a wavelength of 850 nm is above 90%. In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40 mm to 1.00 mm, the transmittance T3 of the non-exposed area of ​​the photosensitive glass at a wavelength of 850 nm can be 90.00%, 90.50%, 91.00%, 91.69%, 91.92%, 92.03%, 92.21%, 93.00%, 93.50%, 94.00%, 94.80% or 95.00%; or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the implementation scheme, any of the above ranges can be combined with any other ranges.

[0104] In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T4 of the non-exposed area of ​​the photosensitive glass at a wavelength of 550 nm is above 90%. In some embodiments of the present application, when the thickness of the photosensitive glass is 0.40-1.00 mm, the transmittance T4 of the non-exposed area of ​​the photosensitive glass at a wavelength of 550 nm can be 90.00%, 90.74%, 91.05%, 91.60%, 92.03%, 92.50%, 93.00%, 93.50%, 94.00%, 94.80% or 95.00%; or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the implementation scheme, any of the above ranges can be combined with any other ranges.

[0105] In some embodiments of the present application, a method for preparing the above-mentioned photosensitive glass is provided, which comprises:

[0106] The raw material components are configured, then mixed and melted in a noble metal container, then formed, and then annealed to obtain a substrate glass;

[0107] The substrate glass comprises a first region and a second region, the first region is subjected to masking treatment, and the second region is not subjected to masking treatment, so as to obtain the masked substrate glass;

[0108] After the masked substrate glass is subjected to radiation treatment and heat treatment, a photosensitive glass having a non-exposed area and an exposed area is obtained; wherein the non-exposed area corresponds to the first area, and the exposed area corresponds to the second area.

[0109] In the present application, the container includes but is not limited to crucibles, crucibles, kilns, channels, etc., wherein the precious metal container means that at least the part in contact with the raw material is made of precious metal, wherein the precious metal includes but is not limited to gold, platinum, rhodium, etc. In some embodiments of the present application, the precious metal container is a container made of at least one metal including gold, platinum, and rhodium.

[0110] In the present application, the substrate glass may be prepared by a molding method in the prior art, and the present application has no restrictions on this. For example, the molding method of the substrate glass may include but is not limited to float, overflow, pulling, rolling or casting processes.

[0111] Exemplarily, the ingredients are prepared according to the specified raw materials and the corresponding weight proportions. After the raw materials are evenly mixed, they are put into the precious metal container in sections and continuously for melting. The feeding method can be adjusted according to the different precious metal containers. After the glass is melted, it is formed into glass bricks, and then the glass bricks are transferred to the annealing furnace for annealing. After the annealing is completed, the base glass is obtained by naturally cooling to room temperature.

[0112] In some embodiments of the present application, the composition of the substrate glass of the present application is the same or substantially the same as the composition of the photosensitive glass; the specific composition is as above.

[0113] In some embodiments of the present application, the melting temperature is 1400°C to 1650°C, and the melting time is 6h to 48h. In some embodiments of the present application, the melting temperature can be 1400°C, 1475°C, 1500°C, 1525°C, 1550°C, 1575°C, 1600°C, 1625°C or 1650°C, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.

[0114] In some embodiments of the present application, the melting time may be any of 6h, 9h, 12h, 15h, 18h, 21h, 24h, 27h, 30h, 33h, 36h, 39h, 42h, 45h, and 48h, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that, in a specific embodiment, any of the above ranges may be combined with any other ranges, as long as the photosensitive glass with the desired performance of the present application can be obtained.

[0115] In some embodiments of the present application, the annealing temperature is 400°C to 500°C, and the annealing time is 8h to 24h. In some embodiments of the present application, the annealing temperature is 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C or 500°C, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0116] In some embodiments of the present application, the annealing time can be 5h, 6h, 7h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h or 24h, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0117] In some embodiments of the present application, the masking process includes masking using masking ink and / or a mask plate.

[0118] For example, the schematic diagram of the structure of the substrate glass after masking with masking ink is as follows: Figure 1 The composite circular hole has a light-transmitting area 11 of the inner diameter and a light-shielding area 12 outside the inner diameter; the structural schematic diagram of the corresponding photosensitive glass is as shown in Figure 2 The position corresponding to the light-transmitting area 11 forms an exposure area 21, and the position corresponding to the light-shielding area 12 forms a non-exposure area 22.

[0119] In some embodiments of the present application, the radiation treatment comprises ultraviolet irradiation treatment.

[0120] In some embodiments of the present application, the wavelength of the ultraviolet irradiation treatment is 300nm to 320nm, and the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 ~360mw / cm 2 The UV irradiation treatment time is 5min to 60min.

[0121] In some embodiments of the present application, the wavelength of the ultraviolet irradiation treatment is 300nm, 302nm, 305nm, 308nm, 310nm, 312nm, 315nm, 317nm or 320nm, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 、40mw / cm 2 、60mw / cm 2 、80mw / cm 2 、100mw / cm 2 、120mw / cm 2 、140mw / cm 2 、160mw / cm 2 、180mw / cm 2 、200mw / cm 2 、210mw / cm 2 、220mw / cm 2 、230mw / cm 2 、240mw / cm 2 、250mw / cm 2 、260mw / cm 2 、270mw / cm 2 、280mw / cm 2 、290mw / cm 2 、300mw / cm 2 、310mw / cm 2 、320mw / cm 2 、330mw / cm 2 、340mw / cm 2 、350mw / cm 2 or 360mw / cm 2 , or a value within the numerical range formed by any two of the above specific values ​​as endpoints. In some embodiments of the present application, the time of ultraviolet irradiation treatment is 5min, 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min or 60min, or a value within the numerical range formed by any two of the above specific values ​​as endpoints; as long as the photosensitive glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the photosensitive glass with the required performance of the present application can be obtained.

[0122] In some embodiments of the present application, the heat treatment includes a nucleation treatment and a crystallization treatment, which are common processes in the art.

[0123] In some embodiments of the present application, the heating rate of the nucleation treatment is 1°C / min to 10°C / min. In some embodiments of the present application, the time of the nucleation treatment may be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the temperature of the nucleation treatment may be 430°C to 500°C. In some embodiments of the present application, the temperature of the nucleation treatment may be 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C or 500°C, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the time of the nucleation treatment is 30min to 360min. In some embodiments of the present application, the time of the nucleation treatment can be 30 min, 45 min, 50 min, 55 min, 60 min, 90 min, 100 min, 120 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 220 min, 240 min, 280 min, 300 min, 320 min, 340 min or 360 min, or a value within the numerical range formed by any two of the above specific values ​​as endpoints.

[0124] In the present application, the crystallization treatment includes a one-step crystallization treatment and a multi-step crystallization treatment. In some embodiments of the present application, the heating rate of the crystallization treatment is 1°C / min to 10°C / min. In some embodiments of the present application, the time of the crystallization treatment can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints.

[0125] In some embodiments of the present application, the temperature of the one-step crystallization treatment may be 500°C to 800°C. In some embodiments of the present application, the temperature of the one-step crystallization treatment may be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 600°C, 650°C, 700°C, 750°C or 800°C, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the time of the one-step crystallization treatment is 30min to 480min. In some embodiments of the present application, the time for the crystallization treatment can be 30 min, 45 min, 50 min, 55 min, 60 min, 90 min, 100 min, 120 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 220 min, 240 min, 280 min, 300 min, 340 min, 380 min, 400 min, 430 min, 450 min or 480 min, or a value within the numerical range formed by any two of the above specific values ​​as endpoints.

[0126] In some embodiments of the present application, the multi-step crystallization process includes a two-step crystallization process. In some embodiments of the present application, the temperature of the first crystallization process in the two-step crystallization process is 500° C. to 560° C., and the temperature of the second crystallization process is 560° C. to 800° C. It is understood that the temperature of the second crystallization process is higher than the temperature of the first crystallization process.

[0127] In some embodiments of the present application, the temperature of the first crystallization process in the two-step crystallization process may be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C or 560°C, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the temperature of the second crystallization process in the two-step crystallization process may be 560°C, 570°C, 580°C, 600°C, 650°C, 700°C, 750°C or 800°C, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints.

[0128] In some embodiments of the present application, the time of the first crystallization treatment in the two-step crystallization treatment is 30 min to 240 min, and the time of the second crystallization treatment is 30 min to 240 min. In some embodiments of the present application, the time of the first crystallization treatment in the two-step crystallization treatment can be 30 min, 45 min, 50 min, 55 min, 60 min, 90 min, 100 min, 120 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 220 min or 240 min, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the time of the second crystallization treatment in the two-step crystallization treatment can be 30 min, 45 min, 50 min, 55 min, 60 min, 90 min, 100 min, 120 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 220 min or 240 min, or a value within the numerical range formed by any two of the above specific values ​​as endpoints.

[0129] Before and / or after the heat treatment, those skilled in the art may also perform other conventional steps to obtain a photosensitive glass sample that meets the required specifications or requirements, such as shaping, cutting (such as cutting with a multi-wire cutting machine), CNC machining (computer numerical control, i.e., CNC machine tools), thinning, or polishing. The size of the photosensitive glass is not limited in the present application, for example, it may be 50 mm×50 mm×1.0 mm, 300 mm×120 mm×0.7 mm, etc.

[0130] In some embodiments of the present application, the thickness of the substrate glass and / or photosensitive glass of the present application is not particularly limited, for example, it can be 0.4 to 2.0 mm. In some embodiments of the present application, the thickness of the photosensitive glass of the present application can be 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm or 2.0 mm, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0131] In some embodiments of the present application, a strengthened photosensitive glass is provided, having a thickness of t, and comprising a strengthening layer and a tensile stress layer. The strengthening layer extends from the surface of the strengthened photosensitive glass toward the inside, and the thickness of the strengthening layer is 0 to 0.22t.

[0132] The center of the tensile stress layer and / or the strengthened photosensitive glass comprises the following components, calculated as a percentage by mass of oxides:

[0133] SiO2: 65% to 74.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.90% to 12.00%, Na2O: 1.00% to 3.00%, K2O: 1.50% to 3.80%, ZrO2: 3.5% to 6.50%, Ag2O: 0.20% to 0.50%, CeO2: 0.07% to 0.13% and Sb2O3: 0.2% to 0.50%;

[0134] The strengthening layer, expressed in terms of oxide mass percentage, comprises the following components:

[0135] SiO2: 65% to 74.00%, Al2O3: 5.00% to 10.00%, Na2O: 4.00% to 16.00%, K2O: 2.0% to 5.0%, ZrO2: 3.5% to 6.50%, Ag2O: 0.20% to 0.50%, CeO2: 0.07% to 0.13% and Sb2O3: 0.2% to 0.50%; the content of Li2O in the strengthening layer is lower than the content of Li2O in the center of the tensile stress layer and / or the strengthened photosensitive glass;

[0136] Among them, Na2O is obtained from sodium nitrate, K2O is obtained from potassium nitrate, Ag2O is obtained from silver nitrate, and Sb2O3 is obtained from pentavalent antimony salt;

[0137] The tempered photosensitive glass includes a non-exposed area and an exposed area.

[0138] In some embodiments of the present application, a strengthened photosensitive glass is provided, and the thickness is t. The strengthened photosensitive glass is obtained by chemically strengthening the photosensitive glass of any of the above embodiments.

[0139] In some embodiments of the present application, the strengthened photosensitive glass comprises a strengthening layer and a tensile stress layer, and the strengthening layer comprises the following components in terms of mass percentage of oxides:

[0140] SiO2: 65% to 74.00%, Al2O3: 5.00% to 10.00%, Na2O: 4.00% to 16.00%, K2O: 2.0% to 5.0%, ZrO2: 3.5% to 6.50%, Ag2O: 0.20% to 0.50%, CeO2: 0.07% to 0.13% and Sb2O3: 0.2% to 0.50%; the content of Li2O in the strengthening layer is lower than the content of Li2O in the center of the tensile stress layer and / or the strengthened photosensitive glass;

[0141] Among them, Na2O is obtained from sodium nitrate, K2O is obtained from potassium nitrate, Ag2O is obtained from silver nitrate, and Sb2O3 is obtained from pentavalent antimony salt;

[0142] The center of the tensile stress layer and / or the strengthened photosensitive glass comprises the following components, calculated as a percentage by mass of oxides:

[0143] SiO2: 65% ~ 74.00%, Al2O3: 5.00% ~ 10.00%, Li2O: 7.90% ~ 12.00%, Na2O: 1.00% ~ 3.00%, K2O: 1.50% ~ 3.80%, ZrO2: 3.5% ~ 6.50%, Ag2O: 0.20% ~ 0.50%, CeO2: 0.07% ~ 0.13% and Sb2O3: 0.2% ~ 0.50%.

[0144] In the present application, SiO2 is a glass-forming oxide, which forms an irregular continuous network with the structural unit of silicon-oxygen tetrahedron, and is the skeleton of the glass. In some embodiments of the present application, the content of SiO2 in the strengthening layer or tensile stress layer or the center of the strengthened photosensitive glass is 65.00% to 74.00%, preferably 66.00% to 73.20%, based on the mass percentage of the oxide.

[0145] In some embodiments of the present application, the content of SiO2 in the strengthening layer or tensile stress layer or the center of the strengthened photosensitive glass can be 65.00%, 66.00%, 67.00%, 68.00%, 69.00%, 70.00%, 71.00%, 72.00%, 73.00% or 74.00%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0146] In this application, Al2O3 is a glass network intermediate, and enters the glass network structure as [AlO4] tetrahedron. The increase of Al2O3 can improve the T g Temperature, thermal stability is enhanced, and it is beneficial to inhibit the phase separation during the heat treatment of glass, but too much will increase the melting temperature of the glass. In some embodiments of the present application, the content of Al2O3 in the strengthening layer or tensile stress layer or center of the strengthened photosensitive glass is 5.00% to 10.00%, preferably 5.10% to 9.70%, and more preferably 5.20% to 9.40%, calculated by mass percentage of oxides.

[0147] In some embodiments of the present application, the content of Al2O3 in the strengthening layer or tensile stress layer or the center of the strengthened photosensitive glass can be 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 7.25%, 5.83%, 8.76%, 7.62%, 7.89%, 6.47% or 8.96%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0148] In some embodiments of the present application, the content of Li2O in the strengthening layer of the strengthened photosensitive glass is 7.90% to 12.00% in terms of the mass percentage of the oxide.

[0149] In some embodiments of the present application, the content of Li2O in the tensile stress layer or the center of the strengthened photosensitive glass can be 7.90%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 10.50%, 11.00%, 11.50% or 12.00%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints, in terms of the mass percentage of the oxide. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0150] In some embodiments of the present application, the content of Li2O in the strengthening layer is lower than the content of Li2O in the center of the tensile stress layer and / or the strengthened photosensitive glass, measured in terms of mass percentage of oxide.

[0151] In some embodiments of the present application, the content of Na2O in the tensile stress layer or the center of the strengthened photosensitive glass is 1.00% to 3.00%, preferably 1.00% to 2.80%, by mass percentage of oxide. In some embodiments of the present application, the content of Na2O in the tensile stress layer or the center of the strengthened photosensitive glass can be 1.00%, 1.10%, 1.20%, 1.30%, 1.40%, 1.50%, 1.60%, 1.70%, 1.80%, 1.90%, 2.00%, 2.10%, 2.20%, 2.30%, 2.40%, 2.50%, 2.60%, 2.70%, 2.80%, 2.90% or 3.00%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0152] In some embodiments of the present application, the content of Na2O in the strengthening layer of the strengthened photosensitive glass is 4.00% to 16.00%, preferably 4.00% to 15%, calculated as a percentage by mass of the oxide. In some embodiments of the present application, the content of Na2O in the strengthening layer of the strengthened photosensitive glass can be 4.00%, 4.50%, 4.80%, 5.00%, 5.40%, 5.80%, 6.60%, 6.90%, 7.00%, 7.20%, 7.80%, 8.00%, 8.50%, 8.90%, 9.00%, 9.50%, %, 11.00%, 11.50%, 12.00%, 12.50%, 12.90%, 13.00%, 13.50%, 14.00%, 14.50%, 15.00%, 15.60%, 15.90% or 16.00%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that, in embodiments, any of the above ranges can be combined with any other ranges.

[0153] In some embodiments of the present application, the content of K2O in the tensile stress layer or the center of the strengthened photosensitive glass is 1.50% to 3.80%, preferably 1.80% to 3.50%, by mass percentage of oxide. In some embodiments of the present application, the content of K2O in the tensile stress layer or the center of the strengthened photosensitive glass can be 1.50%, 1.80%, 2.00%, 2.30%, 2.40%, 2.80%, 3.00%, 3.30%, 3.40%, 3.50%, 3.60%, 3.70% or 3.80%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0154] In some embodiments of the present application, the content of K2O in the strengthening layer of the strengthened photosensitive glass is 2.00% to 5.00%, preferably 2.20% to 4.90%, calculated as a percentage by mass of the oxide. In some embodiments of the present application, the content of K2O in the strengthening layer of the strengthened photosensitive glass is 2.00%, 2.50%, 2.80%, 3.00%, 3.40%, 3.80%, 4.00%, 4.30%, 4.80% or 5.00%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0155] In some embodiments of the present application, the content of ZrO2 in the strengthening layer or tensile stress layer or the center of the strengthened photosensitive glass is 3.50% to 6.50%, preferably 3.80% to 6.40%, by mass percentage of oxide. In some embodiments of the present application, the content of ZrO2 in the strengthening layer or tensile stress layer or the center of the strengthened photosensitive glass is 3.50%, 3.80%, 4.00%, 4.30%, 4.80%, 5.00%, 5.30%, 5.70%, 5.80%, 5.90%, 6.00%, 6.20% or 6.50%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0156] In some embodiments of the present application, the content of Ag2O in the strengthening layer or tensile stress layer or the center of the strengthened photosensitive glass is 0.20% to 0.50%, preferably 0.20% to 0.49%, by mass percentage of oxide. In some embodiments of the present application, the content of Ag2O in the strengthening layer or tensile stress layer or the center of the strengthened photosensitive glass is 0.20%, 0.22%, 0.24%, 0.26%, 0.28%, 0.30%, 0.32%, 0.34%, 0.36%, 0.38%, 0.40%, 0.42%, 0.44%, 0.46%, 0.48% or 0.50%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0157] In some embodiments of the present application, the mass percentage of CeO2 in the strengthening layer or the tensile stress layer or the center of the strengthened photosensitive glass is 0.07% to 0.13%, preferably 0.08% to 0.12%, calculated as the mass percentage of the oxide.

[0158] In some embodiments of the present application, the content of CeO2 in the strengthening layer or tensile stress layer or the center of the strengthened photosensitive glass can be 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, or 0.13%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints, in terms of the mass percentage of the oxide. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0159] In this application, Sb2O3 is a weak reducing agent and also acts as a clarifier. 3+ During the glass melting process, Ce 4+Oxidation-reduction reaction occurs to maintain Ce 3+ In some embodiments of the present application, the mass percentage of Sb2O3 in the strengthening layer or tensile stress layer or the center of the strengthened photosensitive glass is 0.20% to 0.50%, preferably 0.22% to 0.49%, calculated as the mass percentage of oxides.

[0160] In some embodiments of the present application, the content of Sb2O3 in the strengthening layer or tensile stress layer or the center of the strengthened photosensitive glass can be 0.20%, 0.22%, 0.25%, 0.28%, 0.30%, 0.34%, 0.37%, 0.39%, 0.40%, 0.42%, 0.45%, 0.47%, 0.49% or 0.50%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0161] In the present application, chemical strengthening can be performed by a conventionally known method; for example, chemical strengthening includes single-step chemical strengthening or multi-step chemical strengthening.

[0162] In some embodiments of the present application, single-step chemical strengthening uses a salt bath containing NaNO3; preferably, the content of NaNO3 in the salt bath is 30wt% to 100wt%; preferably, single-step chemical strengthening uses a mixed salt bath containing NaNO3 and KNO3, and preferably the content of KNO3 in the mixed salt bath is greater than or equal to 80wt% and less than 100wt%, and the content of NaNO3 is greater than 0 and less than or equal to 20wt%.

[0163] In some embodiments of the present application, the temperature of the single-step chemical strengthening is 380° C. to 480° C.; preferably, the ion exchange time of the single-step chemical strengthening is 5 h to 20 h.

[0164] In some embodiments of the present application, multi-step chemical strengthening includes two-step chemical strengthening, wherein the first step of chemical strengthening uses a salt bath containing NaNO3, preferably with a NaNO3 content of 30wt% to 100wt%; the second step of chemical strengthening uses a salt bath containing KNO3, preferably with a KNO3 content of 60wt% to 100wt%.

[0165] In some embodiments of the present application, the temperature of the first step chemical strengthening is 380°C to 480°C, and the time of the first step chemical strengthening is preferably 3h to 20h; and / or, the temperature of the second step chemical strengthening is 380°C to 480°C, and the time of the second step chemical strengthening is preferably 5min to 30min.

[0166] In some embodiments of the present application, the photosensitive glass may be subjected to other conventional processing before chemical strengthening to obtain a photosensitive glass sample that meets the required specifications or requirements, wherein the processing includes one or more of CNC processing, grinding and polishing, cleaning, 3D hot bending, and scanning. It should be noted that the size of the strengthened photosensitive glass sample is not limited in the present application, for example, it can be 50mm×50mm×1.0mm, 300mm×120mm×0.7mm, etc.

[0167] In some embodiments of the present application, the strengthened photosensitive glass may be flat or curved.

[0168] In some embodiments of the present application, the thickness t of the tempered photosensitive glass of the present application is not particularly limited, for example, it can be 0.4 to 2.0 mm. In some embodiments of the present application, the thickness t of the tempered photosensitive glass can be 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm or 2.0 mm, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0169] In some embodiments of the present application, the surface CS of the non-exposed area of ​​the strengthened photosensitive glass is above 300 MPa, preferably above 350 MPa, and more preferably 350 MPa to 600 MPa. In some embodiments of the present application, the surface CS of the non-exposed area of ​​the strengthened photosensitive glass can be 350 MPa, 351 MPa, 395 MPa, 438 MPa, 385 MPa, 391 MPa, 398 MPa, 402 MPa, 422 MPa, 450 MPa, 480 MPa, 500 MPa, 530 MPa, 550 MPa, 580 MPa or 600 MPa, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints; as long as the photosensitive glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges.

[0170] In some embodiments of the present application, the static pressure strength of a single rod of the strengthened photosensitive glass is above 200N, preferably 200N to 500N, and more preferably 200N to 490N. In some embodiments of the present application, the static pressure strength of a single rod of the strengthened curved photosensitive glass in the present application may be 200N, 250N, 294N, 361N, 392N, 301N, 314N, 375N, 376N, 390N, 400N, 450N, 480N or 500N, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints; as long as the photosensitive glass with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges may be combined with any other ranges.

[0171] The photosensitive glass and / or strengthened photosensitive glass provided in the present application can be used in electronic devices, including but not limited to mobile phones, tablet computers, handheld game consoles, portable digital devices (such as digital cameras), smart homes, smart wearables (such as smart bracelets, smart watches, smart glasses), and can also be used in vehicles, aircraft or aircraft, and can also be used in any glass device that requires photosensitive glass. For example, it can be used in the back cover glass of mobile phones, the shell glass of smart watches, etc.; for example, it can be used in the windshield of vehicles, aircraft or aircraft, such as the front windshield or side windshield.

[0172] For example, the photosensitive glass and / or strengthened photosensitive glass provided in the present application can be used to manufacture cover glass, and the cover glass can be a back cover or camera protection cover of an electronic device such as a mobile phone. For example, the photosensitive glass and / or strengthened photosensitive glass with excellent performance provided in the present application can be used in electronic devices. In some embodiments of the present application, an electronic device is provided, which can be a mobile phone (such as Figure 3 As shown, the photosensitive glass and / or the strengthened photosensitive glass can be used as the back cover of a mobile phone), a tablet computer, a smart wearable device (such as Figure 4 As shown, photosensitive glass and / or strengthened photosensitive glass can be used as the shell at the bottom of a smart watch) and other electronic products.

[0173] In some embodiments of the present application, the electronic device includes a smart wearable device worn on the body, which includes a housing having a top and a bottom, and the housing at the bottom includes the photosensitive glass and / or strengthened photosensitive glass described above in the present application. The bottom is designed to contact the user's skin when worn.

[0174] In some embodiments of the present application, Figure 3As shown, the electronic device also includes a camera assembly 32 located inside the housing, and the housing may include a camera protection cover 31, the camera protection cover 31 is covered on the camera assembly 32 to protect the camera assembly 32, and the camera protection cover 31 adopts the aforementioned photosensitive glass and / or strengthened photosensitive glass. In some embodiments of the present application, the camera protection cover 31 may be partially made of the aforementioned photosensitive glass, or may be made of the aforementioned photosensitive glass in its entirety. In some embodiments of the present application, the setting position of the camera protection cover 31 is determined according to the setting position of the camera assembly 32, and may be located on the front side of the electronic device, or may be located on the rear side of the electronic device. In some embodiments of the present application, the camera protection cover 31 may be a separate structure from the back cover 33. In other embodiments of the present application, the camera protection cover 31 may also be an integrated structure with the back cover 33.

[0175] The technical solution of the present application is further described in detail below in conjunction with the embodiments. The embodiments of the present application described in detail below are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.

[0176] Example 1

[0177] (1) The raw materials were prepared according to the proportions of the components in Table 1. The total mass of the prepared raw materials was 2000 g. 10 g of clarifier sodium chloride (NaCl) was added to the prepared raw materials, and then mixed in a V-type mixer for 30 minutes to obtain a uniform raw material mixture.

[0178] The raw material mixture is transferred to a platinum crucible at 1500℃ for melting, and the melt is stirred with a platinum stirring rod for 10 hours, and then pulled into shape and continuously drawn into glass bricks of the required specifications. The glass bricks are quickly placed in an annealing furnace at 500℃ for 10 hours, and then naturally cooled to room temperature to obtain the base glass bricks.

[0179] The substrate glass bricks are cut, CNC processed (the CNC equipment model used in this application is: RCG500S), and polished in sequence to obtain substrate glass with a size of 50mm×50mm×1.0mm.

[0180] (2) ultrasonically cleaning the substrate glass obtained above for 10 minutes and then drying it in a drying oven;

[0181] After cleaning, the substrate glass is coated with masking ink in a local area, such as Figure 1 As shown, the black area is the masked area; then, the irradiation treatment was carried out under parallel ultraviolet light with a wavelength of 310nm (UVHX800*850 drawer type) for a total of 25min, and the intensity of the ultraviolet irradiation treatment was 120mw / cm2 ;

[0182] The UV-irradiated glass was heat-treated according to the heat treatment process in Table 1 to obtain photosensitive glass; the heat treatment included nucleation treatment and crystallization treatment; the heating rates of nucleation treatment and crystallization treatment were both 10°C / min; the photosensitive glass was subjected to cold processing such as laser cutting, splitting, polishing, chamfering, etc., to obtain photosensitive glass with a size of φ30*1.0mm, such as Figure 2 shown.

[0183] Embodiment 2 to Embodiment 8

[0184] The steps are respectively carried out with reference to Example 1, except that the raw material composition ratio, heat treatment process parameters and the like of Examples 1 to 8.

[0185] Relevant performance tests were performed on Examples 1 to 8, and the results are shown in Table 1.

[0186] Table 1

[0187]

[0188]

[0189] The photosensitive glasses of Examples 1, 3 and 6 were subjected to chemical strengthening treatment, wherein the chemical strengthening treatment was carried out in sequence by chemical strengthening in a 100wt% NaNO3 salt bath at 460°C for 18h and chemical strengthening in a 100wt% KNO3 salt bath at 440°C for 20min to obtain strengthened photosensitive glasses.

[0190] The mass percentages of the raw materials of the photosensitive glass of Examples 1, 3 and 6 converted into oxides are shown in Table 2 below; the surface CS and horizontal bar static pressure strength of the non-exposed area of ​​the strengthened photosensitive glass were tested, and the results are shown in Table 3.

[0191] Table 2

[0192]

[0193]

[0194] Table 3

[0195] Example 1 Example 3 Example 6 Non-exposure area CS / Mpa 372 398 426 Single rod static pressure strength / N 302 365 388

[0196] Examples 9 to 10 and Comparative Examples 1 to 3

[0197] The same method is carried out with reference to Example 1, except that the raw material compositions of Examples 9 to 10 and Comparative Examples 1 to 3 are different as shown in Table 4.

[0198] Among them, Examples 9 to 10 and Comparative Examples 1 to 3 are all calculated in terms of molar percentage of oxides, and the same oxide is provided by different raw materials. Taking the Sb2O3 column as an example, in Examples 9-10 and Comparative Examples 1-3, the content of Sb2O3 is 0.37 in terms of molar percentage of oxides, the difference being that Example 9 uses sodium antimonate as a raw material to provide Sb2O3, Example 10 uses ammonium antimonate as a raw material to provide Sb2O3, and Comparative Examples 1-3 use antimony oxide (Sb2O3) as a raw material to provide Sb2O3. Thus; in addition, the molar percentage of the oxides in Examples 9 to 10 is converted into the mass ratio of the raw material components: 57.96wt% of silica sand, 18.34wt% of lithium carbonate, 8.89wt% of aluminum hydroxide, 5.30wt% of potassium nitrate, 5.05wt% of sodium nitrate, 3.62wt% of zirconium oxide, 0.43wt% of silver nitrate, 0.07wt% of cerium oxide, and pentavalent antimony salt; wherein, calculated as sodium antimonate, the content of pentavalent antimony salt is 0.34wt%; which is within the mass ratio range of the present application.

[0199] The Ag / Ag2O concentration (the result is converted into the mass ratio of Ag2O) of the main surface of the photosensitive glass prepared in Examples 9 to 10 and Comparative Examples 1 to 3 and the transmittance T3 (850nm) of the exposed area thereof were tested; in addition, the shielding diagram of the exposed area of ​​the photosensitive glass prepared in Examples 9 to 10 and Comparative Examples 1 to 3 in the visible light range was obtained as shown in FIG. Figure 6 The results are shown in Table 5.

[0200] Table 4

[0201]

[0202]

[0203] Table 5

[0204]

[0205] The bottom photos of the crucibles after melting in Examples 9-10 and Comparative Examples 1-2 are as follows: Figure 5 As shown, a. a photograph of the bottom of the crucible of Comparative Example 1, b. a photograph of the bottom of the crucible of Comparative Example 2, c. a photograph of the bottom of the crucible of Example 9, d. a photograph of the bottom of the crucible of Example 10.

[0206] Figure 6 This is a physical picture of the shielding of the exposure area of ​​Examples 9 to 10 of the present application and Comparative Examples 1 to 3 within the visible light range. The bright light spots in Comparative Examples 1-3 pass through red light.

[0207] According to the above Table 1 and Figure 5 ,as well as Figure 6It can be seen that the photosensitive glass prepared in the present application can ensure the stability of the glass components of the Ag-containing photosensitive glass during the melting process, without Ag precipitation to corrode the precious metal container; and the exposure area of ​​the prepared photosensitive glass can shield optical signals within the visible light and near-infrared wavelength range.

[0208] According to the above Table 4 and Figure 5 It can be seen that, under the same molar ratio of oxides, the photosensitive glass prepared without nitrate raw materials will cause serious corrosion to the platinum crucible; while adding some nitrate raw materials can reduce the corrosion, but as long as silver oxide is directly used in the raw materials, it will cause certain corrosion to the platinum crucible. In addition, when the raw materials of the present application use sodium nitrate, potassium nitrate, silver nitrate and sodium antimonate at the same time, it can be guaranteed that the platinum crucible will not be corroded.

[0209] According to Table 5 above, there is no Ag in Examples 9-10 during the raw material melting and molding process. + The loss of Comparative Examples 1-3 is Ag + This is because in Examples 9-10, sodium nitrate, potassium nitrate, silver nitrate and antimonate (sodium antimonate or ammonium antimonate) are used as raw material components to prepare the photosensitive glass, and there is no Ag in the melting process. + The content of Ag2O in the final product is almost the same as that in the initial composition; however, in Comparative Examples 1-3, some Ag + The Ag2O content in the final product is much lower than the Ag2O content in the initial composition. At the same time, the exposure area of ​​the photosensitive glass prepared in Examples 9-10 has good shielding performance in the visible light region, while the exposure area of ​​the photosensitive glass prepared in Comparative Examples 1-3 has red light transmission in the visible light region. In addition, the exposure area of ​​the photosensitive glass prepared in Examples 9-10 has a low transmittance at 850nm, which has good shielding performance.

[0210] The above are only specific embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A photosensitive glass, characterized in that: According to the mass percentage of each raw material component in the photosensitive glass, the photosensitive glass comprises the following components: 50wt% to 60wt% of silica sand, 15wt% to 22wt% of lithium carbonate, 6wt% to 10wt% of aluminum hydroxide, 3wt% to 6wt% of potassium nitrate, 3wt% to 6wt% of sodium nitrate, 3wt% to 5wt% of zirconium oxide, 0.3wt% to 0.6wt% of silver nitrate, 0.05wt% to 0.10wt% of cerium oxide, and pentavalent antimony salt; wherein, calculated as sodium antimonate, the mass percentage of the pentavalent antimony salt in the composition of the photosensitive glass is 0.3wt% to 0.8wt%.

2. The photosensitive glass according to claim 1, characterized in that: According to the mass percentage of each raw material component in the photosensitive glass, the composition of the photosensitive glass includes the following components: The content of the silica sand is 53wt% to 59wt%, preferably 54.00wt% to 58.96wt%, and / or, The content of lithium carbonate is 17wt% to 20wt%, preferably 17.43wt% to 19.94wt%, and / or, The content of the aluminum hydroxide is 8wt% to 10wt%, preferably 8.22wt% to 9.97wt%, and / or, The content of potassium nitrate is 4wt% to 6wt%, preferably 4.07wt% to 5.97wt%, and / or, The content of sodium nitrate is 3.5wt% to 5.5wt%, preferably 3.77wt% to 5.45wt%, and / or, The content of zirconium oxide is 3wt% to 5wt%, preferably 3.33wt% to 4.96wt%, and / or, The content of the silver nitrate is 0.3wt% to 0.5wt%, preferably 0.32wt% to 0.49wt%, and / or, The content of cerium oxide is 0.05wt% to 0.10wt%, preferably 0.06wt% to 0.09wt%, and / or, The content of the pentavalent antimony salt is 0.3 wt % to 0.7 wt %, and preferably the content of the pentavalent antimony salt is 0.3 wt % to 0.5 wt %.

3. The photosensitive glass according to claim 1 or 2, characterized in that: The pentavalent antimony salt includes at least one of NaSbO3, KSbO3, NH4SbO3 and hydrates thereof.

4. The photosensitive glass according to any one of claims 1 to 3, characterized in that: The thickness of the photosensitive glass is 0.4-1.0 mm.

5. The photosensitive glass according to any one of claims 1 to 4, characterized in that: The photosensitive glass includes an exposure area and a non-exposure area; When the thickness of the photosensitive glass is 0.40 mm to 1.00 mm, the transmittance T1 of the exposure area of ​​the photosensitive glass at a wavelength of 850 nm is 0.00% to 5.00%, preferably the transmittance T1 is 0.00% to 3%, and / or; When the thickness of the photosensitive glass is 0.40 mm to 1.00 mm, the transmittance T2 of the exposure area of ​​the photosensitive glass at a wavelength of 550 nm is 0.00% to 5.00%, preferably 0.00% to 2%; and / or, When the thickness of the photosensitive glass is 0.40 mm to 1.00 mm, the transmittance T3 of the non-exposed area of ​​the photosensitive glass at a wavelength of 850 nm is above 90%; and / or, When the thickness of the photosensitive glass is 0.40 mm to 1.00 mm, the transmittance T4 of the non-exposed area of ​​the photosensitive glass at a wavelength of 550 nm is above 90%.

6. A method for preparing the photosensitive glass according to any one of claims 1 to 5, characterized in that: include: The raw material components are configured, then mixed and melted in a noble metal container, then formed, and then annealed to obtain a substrate glass; The substrate glass comprises a first region and a second region, the first region is subjected to masking treatment, and the second region is not subjected to masking treatment, so as to obtain a masked substrate glass; After the masked substrate glass is subjected to radiation treatment and heat treatment, a photosensitive glass having a non-exposed area and an exposed area is obtained; wherein the non-exposed area corresponds to the first area, and the exposed area corresponds to the second area.

7. The preparation method according to claim 6, characterized in that: The noble metal container is a container made of at least one metal selected from the group consisting of gold, platinum and rhodium.

8. The preparation method according to claim 6 or 7, characterized in that: The melting temperature is 1400° C. to 1650° C., and the melting time is 6 h to 48 h; and / or the annealing temperature is 400° C. to 500° C., and the annealing time is 8 h to 24 h.

9. The preparation method according to any one of claims 6 to 8, characterized in that The radiation treatment method includes ultraviolet irradiation treatment.

10. The preparation method according to claim 9, characterized in that: The wavelength of the ultraviolet irradiation treatment is 300nm-320nm, and the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 ~360mw / cm 2 The ultraviolet irradiation treatment time is 5min to 60min.

11. The preparation method according to any one of claims 6 to 10, characterized in that: The heat treatment includes a nucleation treatment and a crystallization treatment.

12. The preparation method according to claim 11, characterized in that: The heating rate of the nucleation treatment is 1°C / min to 10°C / min; and / or, The temperature of the nucleation treatment is 430° C. to 540° C.; and / or, The time of the nucleation treatment is 30 minutes to 360 minutes, and / or, The heating rate of the crystallization treatment is 1°C / min to 10°C / min; and / or, The temperature of the crystallization treatment is 540° C. to 800° C.; and / or, The crystallization treatment time is 30 min to 240 min.

13. A tempered photosensitive glass, characterized in that: The thickness is t, and it includes a strengthening layer and a tensile stress layer, wherein the strengthening layer extends from the surface of the strengthened photosensitive glass toward the inside, and the thickness of the strengthening layer is 0 to 0.22t; The center of the tensile stress layer and / or the strengthened photosensitive glass comprises the following components in terms of mass percentage of oxides: SiO2: 65% to 74.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.90% to 12.00%, Na2O: 1.00% to 3.00%, K2O: 1.50% to 3.80%, ZrO2: 3.5% to 6.50%, Ag2O: 0.20% to 0.50%, CeO2: 0.07% to 0.13% and Sb2O3: 0.2% to 0.50%; The strengthening layer comprises the following components in terms of oxide mass percentage: SiO2: 65% to 74.00%, Al2O3: 5.00% to 10.00%, Na2O: 4.00% to 16.00%, K2O: 2.0% to 5.0%, ZrO2: 3.5% to 6.50%, Ag2O: 0.20% to 0.50%, CeO2: 0.07% to 0.13% and Sb2O3: 0.2% to 0.50%; the content of Li2O in the strengthening layer is lower than the content of Li2O in the center of the tensile stress layer and / or the strengthened photosensitive glass; Among them, Na2O is obtained from sodium nitrate, K2O is obtained from potassium nitrate, Ag2O is obtained from silver nitrate, and Sb2O3 is obtained from pentavalent antimony salt; The strengthened photosensitive glass includes a non-exposed area and an exposed area.

14. The tempered photosensitive glass according to claim 13, characterized in that: The horizontal bar static pressure strength of the tempered photosensitive glass is above 200N, preferably 200N to 500N, and more preferably 200N to 490N.

15. A cover glass, characterized in that: The cover glass is made of the photosensitive glass according to any one of claims 1 to 5, the photosensitive glass prepared by the preparation method according to any one of claims 6 to 12, or the strengthened photosensitive glass according to any one of claims 13-14.

16. An electronic device, characterized in that: The electronic device comprises the photosensitive glass according to any one of claims 1 to 5, the photosensitive glass prepared by the preparation method according to any one of claims 6 to 12, or the strengthened photosensitive glass according to any one of claims 13 to 14.

17. The electronic device according to claim 16, characterized in that: The electronic device comprises a housing having a top and a bottom, wherein the housing at the bottom comprises the photosensitive glass according to any one of claims 1 to 5, the photosensitive glass prepared by the preparation method according to any one of claims 6 to 12, or the strengthened photosensitive glass according to any one of claims 13 to 14.

18. The electronic device according to claim 16, characterized in that: The electronic device also includes a camera assembly, the housing of the electronic device includes a camera protection cover, the camera protection cover is covered on the camera assembly, and the camera protection cover includes the photosensitive glass as described in any one of claims 1-5, the photosensitive glass prepared by the preparation method as described in any one of claims 6-12, or the strengthened photosensitive glass as described in any one of claims 13-14.

19. Use of the photosensitive glass according to any one of claims 1 to 5, the photosensitive glass prepared by the preparation method according to any one of claims 6 to 12, or the strengthened photosensitive glass according to any one of claims 13 to 14 in preparing parts for mobile phones, smart watches, wearable devices, camera modules, and vehicles.

Citation Information

Patent Citations

  • Continuous production of photo-sensitive glass bodies

    CN106167346A

  • Glass cover plate, preparation method thereof and touch screen

    CN109896729A

  • Lithium-aluminum silicon-series glass material allowing photolithography, and preparation method and application thereof

    CN110937805A

  • Glass ceramic and glass ceramic product

    CN118388139A

  • Photosensitive glass material, photosensitive microcrystalline glass and photosensitive microcrystalline glass product

    CN118420224A

Cited By

  • Photosensitive microcrystalline glass, preparation method thereof and chemically strengthened photosensitive microcrystalline glass

    CN122212483A

  • Photosensitive glass, preparation method thereof, reinforced photosensitive glass and application

    CN122380651A

  • Photosensitive glass and preparation method therefor, reinforced photosensitive glass, and use

    WO2026037299A1