Phosphogypsum-based cement
By increasing the amount of phosphogypsum in phosphogypsum cement and combining the formula of silicate cement clinker, slag and limestone, the problem of low resource utilization rate of phosphogypsum is solved, and efficient phosphogypsum utilization and cement production cost is achieved. , meets the mechanical strength and stability requirements of engineering requirements.
Patent Information
- Application Number
- CN202411099933.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The low resource utilization rate of phosphogypsum has led to its accumulation of land and pollution of the environment. The existing reuse methods have not been widely promoted.
Using phosphogypsum-based cement formula, including silicate cement clinker, slag, phosphogypsum and limestone, phosphogypsum cement with high strength and water resistance is formed through high-temperature calcination and hydration reactions, increasing the amount of phosphogypsum to improve resource utilization .
It realizes efficient utilization of phosphogypsum, reduces cement production costs, improves the mechanical strength, stability and plasticity of phosphogypsum cement, complies with national standards, and is suitable for various engineering needs.
Smart Images

Figure BDA0004989099280000061 
Figure BDA0004989099280000081 
Figure BDA0004989099280000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of cement, in particular to phosphogypsum-based cement. Background Art
[0002] Phosphogypsum is an industrial byproduct of phosphoric acid produced by wet process in phosphorus chemical enterprises. Each ton of phosphoric acid will produce 5 tons of phosphogypsum. With the rapid development of my country's phosphating industry, the annual byproduct of phosphogypsum has exceeded 40 million tons. The accumulated phosphogypsum exceeds 200 million tons. Due to various reasons, the resource utilization rate of phosphogypsum in my country is currently insufficient. The remaining part is treated as solid waste by accumulation or landfill. The accumulation of phosphogypsum not only occupies a large amount of land, but also causes serious pollution to the surrounding environment. It is urgent to accelerate the resource utilization of phosphogypsum.
[0003] At present, the recycling of phosphogypsum is to calcine phosphogypsum at high temperature to remove all crystal water to obtain anhydrous gypsum, and then add various sulfates to the anhydrous gypsum as accelerators to prepare anhydrous gypsum cement with good water resistance. The treated anhydrous gypsum is compounded with cement, lime, fly ash and other materials to prepare cementitious materials with higher strength and significantly improve the water resistance of cementitious materials. The application of phosphogypsum in building materials mainly includes the following aspects:
[0004] (1) After being processed, it can be used as a retarder to replace natural gypsum in cement manufacturing.
[0005] (2) Calcination dehydration or pressure steam dehydration to obtain β-type or α-type hemihydrate gypsum building gypsum is used to prepare gypsum mortar, gypsum board, gypsum molds, etc.
[0006] (3) After calcination at above 800°C, the anhydrous gypsum is used to prepare anhydrous gypsum cement.
[0007] (4) By compounding with cement, lime, slag or fly ash, it can prepare high-strength and water-resistant cementitious materials for use in gypsum mortar, soil solidification and other fields.
[0008] It can be used as raw material to produce sulphoaluminate cement or phosphogypsum to produce sulphuric acid cement.
[0009] Although there are many ways to utilize phosphogypsum, due to various factors, the above recycling methods have not been widely promoted and applied. Except for some areas lacking natural gypsum, the utilization rate of phosphogypsum as a byproduct of most phosphorus chemical companies is very low. Summary of the invention
[0010] The purpose of the present invention is to provide a phosphogypsum-based cement, which has good workability, strong plasticity, and good weather resistance. The phosphogypsum in the phosphogypsum cement is large in amount, and a large amount of phosphogypsum produced by phosphorus chemical enterprises can be consumed, thereby saving resources and reducing the production cost of cement.
[0011] The present invention solves the technical problem by adopting the following technical solutions.
[0012] On the one hand, an embodiment of the present invention provides a phosphogypsum-based cement, which includes the following raw materials by weight percentage: 2-5% of Portland cement clinker, 21-51% of slag, 35-65% of phosphogypsum and 10% of limestone.
[0013] In this formula, the dosage of phosphogypsum is 35-65%, and that of silicate cement clinker is 2-5%. It can be seen that the dosage of phosphogypsum is significantly greater than that of silicate cement clinker, and a large amount of phosphogypsum, a by-product of phosphorus chemical enterprises, can be consumed, and the strength of the obtained phosphogypsum cement also meets national standards.
[0014] Among them, Portland cement clinker is made of limestone and clay as the main raw materials, which are crushed, batched, and ground into raw materials, and then calcined in cement kilns. Portland cement clinker contains four oxides, CaO, SiO2, Fe2O3, and Al2O3, which account for 95% of the clinker, and the other 5% are other oxides, such as MgO, SO3, etc., and the above four oxides do not exist as individual oxides, but as a variety of mineral aggregates generated by the reaction of two or more oxides.
[0015] The glass in the granulated slag powder is an active component. The finely ground slag powder depolymerizes and dissolves under alkaline conditions, and a hydration reaction occurs to form a stable hydration product. When phosphogypsum is hydrated, it recrystallizes into dihydrate gypsum. The large-scale generation and growth of dihydrate gypsum crystal nuclei, as well as the contact and intergrowth between crystals, form a slurry crystal structure network in the gypsum slurry. Limestone and silicate cement are strong alkaline substances that can provide an alkaline environment for the dissolution and hydration of slag powder.
[0016] In some embodiments of the present invention, the following raw materials are included by weight percentage: 4% silicate cement clinker, 41% slag, 45% phosphogypsum and 10% limestone. Under this ratio, the standard consistency water consumption of phosphogypsum cement is 31.40%, the initial setting and final setting time are suitable, and the flexural and compressive strengths are high, which meets the use standards of cement. That is to say, under the premise of ensuring that the comprehensive performance of phosphogypsum cement meets the use standards, a large amount of phosphogypsum (55%) can be added to maximize the utilization of phosphogypsum and quickly consume phosphogypsum.
[0017] In some embodiments of the present invention, the original phosphogypsum obtained by the wet production of phosphoric acid by the phosphogypsum chemical enterprise is obtained after pre-treatment by methods such as water washing, limestone neutralization, and high-temperature calcination. The chemical formula of the original phosphogypsum is Ca2SO4·2H2O, which itself does not have gelling properties. It is dehydrated to become hemihydrate gypsum. After the hemihydrate gypsum is hydrated and dissolved in the liquid phase. It is recrystallized into dihydrate gypsum, and a large number of dihydrate gypsum crystal nuclei are generated and grown, and the crystals are in contact and intergrowth, forming a slurry crystal structure network in the gypsum slurry, thereby becoming a strong artificial stone.
[0018] In some embodiments of the present invention, the water content of the original phosphogypsum is 12-15%.
[0019] In some embodiments of the present invention, the chemical composition of the phosphogypsum is loss 11.91%, SiO2 3.21%, Al2O3 1.09%, Fe2O3 0.31%, CaO 34.52%, MgO 0.06%, SO3 47.30%, P2O5 1.1%, F - 0.2%. The density of the phosphogypsum is 2350kg / m 3 , with a specific surface area of 81m 2 / g, the dihydrate gypsum in phosphogypsum is completely crystallized, and the grain size is approximately between 20-50μm.
[0020] In some embodiments of the present invention, the Blaine specific surface area of the limestone is 500-520m 2 / kg.
[0021] Compared with the prior art, the embodiments of the present invention have at least the following advantages or beneficial effects:
[0022] The phosphogypsum-based cement in the present application has a large amount of phosphogypsum added to the raw materials while ensuring excellent mechanical strength. It can not only consume a large amount of phosphogypsum produced by phosphorus chemical industry and solve the problem of phosphogypsum accumulation, but also greatly reduce the production cost of phosphogypsum cement, with good economic and environmental benefits.
[0023] Secondly, compared with traditional silicate cement, the phosphogypsum of this application adds a large amount of phosphogypsum, which has little effect on the mechanical strength of phosphogypsum cement such as compression and flexural strength, meets the corresponding national standards, and can better meet various engineering needs. Secondly, the stability of the phosphogypsum-based cement in this application is good. Under different use environments, the performance of the phosphogypsum-based cement changes little, and it can be used for a long time in different environments. It also has good workability. During the construction process, the phosphogypsum-based cement is easy to mix, transport and pour, which improves the construction efficiency. It also has strong plasticity and can adapt to various complex construction environments and design requirements. It has good water resistance and can maintain stable performance in a humid environment. It has good weather resistance and can be used for a long time in different climates without being easily damaged. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0025] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other. The present invention will be described in detail below with reference to specific embodiments.
[0026] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0027] Example 1
[0028] Prepare the raw materials of phosphogypsum-based cement according to the following raw material ratio:
[0029] 2% Portland cement clinker, 43% slag, 45% phosphogypsum and 10% limestone.
[0030] The phosphogypsum-based cement is prepared as follows: various raw materials are mixed and stirred evenly at normal temperature and pressure.
[0031] Among them, in this implementation, the silicate cement clinker used is the P·152.5 silicate cement produced by Wuhan Huaxin Cement Company, and the slag used is the finished slag powder produced by Wuhan Huaxin Cement Company.
[0032] The original phosphogypsum is produced by Hubei Huangmailing Phosphorus Chemical Industry Group. Its chemical composition is loss 11.91%, SiO2 3.21%, Al2O3 1.09%, Fe2O3 0.31%, CaO 34.52%, MgO 0.06%, SO3 47.30%, P2O 51.1%, F -The original phosphogypsum has a water content of 12-15%, is a powdery solid, and has a light gray or dark gray appearance. The original phosphogypsum is calcined at 600° C. to obtain the phosphogypsum of this embodiment.
[0033] The limestone used was produced by Wuhan Huaxin Cement Company. It was first crushed by a jaw crusher to a size of 500mm×500mm, and then ground to a Brinell specific surface area of 512m 2 / kg for standby use. The chemical composition of each raw material is shown in Table 1.
[0034] Table 1 Composition of each raw material
[0035]
[0036] Example 2
[0037] Prepare the raw materials of phosphogypsum-based cement according to the following raw material ratio:
[0038] 3% Portland cement clinker, 42% slag, 45% phosphogypsum and 10% limestone.
[0039] The phosphogypsum-based cement was prepared according to the method of Example 1, and the raw materials used were the same as those in Example 1.
[0040] Example 3
[0041] Prepare the raw materials of phosphogypsum-based cement according to the following raw material ratio:
[0042] Portland cement clinker 4%, slag 41%, phosphogypsum 45% and limestone 10%.
[0043] The phosphogypsum-based cement was prepared according to the method of Example 1, and the raw materials used were the same as those in Example 1.
[0044] Example 4
[0045] Prepare the raw materials of phosphogypsum-based cement according to the following raw material ratio:
[0046] 5% Portland cement clinker, 40% slag, 45% phosphogypsum and 10% limestone.
[0047] The phosphogypsum-based cement was prepared according to the method of Example 1, and the raw materials used were the same as those in Example 1.
[0048] Example 5
[0049] Prepare the raw materials of phosphogypsum-based cement according to the following raw material ratio:
[0050] Portland cement clinker 4%, slag 51%, phosphogypsum 35% and limestone 10%.
[0051] The phosphogypsum-based cement was prepared according to the method of Example 1, and the raw materials used were the same as those in Example 1.
[0052] Example 6
[0053] Prepare the raw materials of phosphogypsum-based cement according to the following raw material ratio:
[0054] Portland cement clinker 4%, slag 41%, phosphogypsum 45% and limestone 10%.
[0055] The phosphogypsum-based cement was prepared according to the method of Example 1, and the raw materials used were the same as those in Example 1.
[0056] Example 7
[0057] Prepare the raw materials of phosphogypsum-based cement according to the following raw material ratio:
[0058] Portland cement clinker 4%, slag 31%, phosphogypsum 55% and limestone 10%.
[0059] The phosphogypsum-based cement was prepared according to the method of Example 1, and the raw materials used were the same as those in Example 1.
[0060] Example 8
[0061] Prepare the raw materials of phosphogypsum-based cement according to the following raw material ratio:
[0062] Portland cement clinker 4%, slag 21%, phosphogypsum 65% and limestone 10%.
[0063] The phosphogypsum-based cement was prepared according to the method of Example 1, and the raw materials used were the same as those in Example 1.
[0064] Comparative Example 1
[0065] The phosphogypsum cement prepared by the raw materials and preparation method of Example 2 in patent CN116675448A was used as a sample, wherein the proportion of each raw material was: 77.5% clinker, 8% limestone, 4% slag, 6.5% phosphogypsum, and 4% coal-fired furnace slag.
[0066] Comparative Example 2
[0067] The silicate cement was purchased directly from the market. Its manufacturer was P·152.5 silicate cement from Wuhan Huaxin Cement Company.
[0068] Experimental example
[0069] The cements of Examples 1-8 and Comparative Examples 1-2 were used as research objects. Water and each cement were added to a mixer and then mixed evenly before forming. According to the measurement method and sample requirements in the national standard GBT1346-2011, the setting time, standard consistency water consumption, and flexural and compressive strengths of the above samples were measured. The measurement results are shown in Table 1.
[0070] Table 1 Performance test of Examples 1-8 and Comparative Examples 1-2
[0071]
[0072]
[0073] By comparing Examples 1-4, it can be concluded that the setting time of phosphogypsum-based cement is longer and the water consumption of standard consistency is larger. When the content of phosphogypsum and limestone is fixed, as the content of Portland cement clinker increases and the content of slag decreases, the initial setting and final setting time of cement are roughly linearly shortened, while the water consumption of standard consistency of cement increases slightly. Through the analysis of experimental data, the comprehensive performance of phosphogypsum-based cement is optimal when 4% of Portland cement clinker is used as an activator.
[0074] Comparative Examples 5-8 show that as the amount of phosphogypsum increases, the water consumption of the standard consistency of phosphogypsum-based cement also gradually increases. When the amount of phosphogypsum is 65%, the water consumption of the standard consistency reaches nearly 33%. At the same time, as the amount of phosphogypsum increases, the initial setting and final setting time of phosphogypsum-based cement also increase. Among them, the increase in the final setting time is greater. In summary, when the content of phosphogypsum is 55% and the content of silicate cement clinker is 4%, the flexural and compressive strengths of phosphogypsum-based cement meet the use standards.
[0075] In the cement of Comparative Example 1, the amount of phosphogypsum added is only 6.5%, and the amount of cement clinker added is 77.5%. Its essence is cement clinker, and phosphogypsum is added as a small amount of additive. In Examples 1-8, phosphogypsum is the main component, and silicate cement clinker is added as an activator, which serves to provide an alkaline environment for the hydration of raw materials in cement. Under alkaline conditions, slag can be activated to depolymerize and dissolve, and then react with phosphogypsum to form a stable hydration product. In Comparative Example 1, a small amount of phosphogypsum is added, and its role is to act as a setting regulator. During hydration, it can react with the aluminum phase or aluminum-iron phase in the cement clinker mineral to form a stable hydration product, calcium sulfonate. However, it is inevitable that the cement will set rapidly when the aluminum phase content in the cement clinker is high. That is to say, in the formula of Comparative Example 1, if too much phosphogypsum is added, the cement will set rapidly, which is not conducive to construction.
[0076] Compared with Comparative Example 1, the phosphogypsum-based cement of Examples 1-8 has properties that meet national standards by adjusting the ratio of phosphogypsum and silicate cement clinker. Although the strength of the obtained phosphogypsum cement is reduced, it still meets national standards. Moreover, this ratio can consume a large amount of phosphogypsum, has a high secondary utilization rate of resources, and significantly reduces the production cost of cement.
[0077] The embodiments described above are part of the embodiments of the present invention, rather than all of the embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A phosphogypsum-based cement, characterized in that: The following raw materials are included by weight percentage: Portland cement clinker 2-5%, slag 21-51%, phosphogypsum 35-65% and limestone 10%.
2. The phosphogypsum-based cement according to claim 1, characterized in that: The following raw materials are included by weight percentage: Portland cement clinker 4%, slag 41%, phosphogypsum 45% and limestone 10%.
3. The phosphogypsum-based cement according to claim 1, characterized in that: The following raw materials are included by weight percentage: Portland cement clinker 4%, slag 51%, phosphogypsum 35% and limestone 10%.
4. The phosphogypsum-based cement according to claim 1, characterized in that: The following raw materials are included by weight percentage: 5% Portland cement clinker, 40% slag, 45% phosphogypsum and 10% limestone.
5. The phosphogypsum-based cement according to claim 1, characterized in that: The phosphogypsum is obtained by treating the original phosphogypsum through one of the following methods: water washing, limestone neutralization, and high-temperature calcination.
6. The phosphogypsum-based cement according to claim 5, characterized in that: The water content of the original phosphogypsum is 12-15%.
7. The phosphogypsum-based cement according to claim 5, characterized in that: The chemical composition of the original phosphogypsum is loss 11.91%, SiO2 3.21%, Al2O3 1.09%, Fe2O3 0.31%, CaO34.52%, MgO 0.06%, SO347.30%, P2O5 1.1%, F - 0.2%.
8. The phosphogypsum-based cement according to claim 1, characterized in that: The Blaine specific surface area of the limestone is 500-520m 2 / kg.
Citation Information
Cited By
Cement production process capable of reducing carbon emission
CN119841563A
A cement production process for reducing carbon emissions
CN119841563B