High-refractive-index polymer material containing sulfur and selenium elements and preparation method of high-refractive-index polymer material

By introducing selenium elements and thiols into the polymer, the S-C-S structure is formed, which solves the problem that the properties of existing high-refractive index materials are difficult to take into account, and polymer preparation with high refractive index, low birefractive and good mechanical properties is achieved. It is suitable for Optical and optoelectronics fields.

CN118994580AActive Publication Date: 2024-11-22JILIN UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411245602.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

While increasing the refractive index, existing high-index polymer materials often lead to a decrease in other optical and mechanical properties, and the preparation process is complicated, making it difficult to take into account the advantages of the comprehensive properties.

Method used

During the process of preparing polydithioacetals by condensation of thiol and aldehyde monomers, selenium is introduced to form an S-C-S structure, which increases the content of high polarization atoms, avoids the color deepening caused by the formation of polysulfide bonds, and in acid The reaction was carried out under catalysis to obtain a polymer with high refractive index, low birefractive index and good mechanical properties.

Benefits of technology

It has achieved the preparation of high refractive index polymers under mild conditions, with high ABB number, low birefractive index, high transmittance and good mechanical properties, and meets the application needs of the optical and optoelectronics fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994580A_ABST
    Figure CN118994580A_ABST
Patent Text Reader

Abstract

The invention discloses a high-refractive-index polymer material containing sulfur and selenium elements and a preparation method of the high-refractive-index polymer material, and belongs to the technical field of preparation of high-refractive-index polymer materials. According to the invention, the selenium-containing mercaptan monomer with high refractive index and the aldehyde monomer are utilized to prepare the polydithioacetal with high refractive index containing sulfur and selenium elements under the catalysis of the acid, the reaction conditions are mild, the preparation process is simple, and by utilizing the respective advantages of the two elements, the preparation method is simple, and the preparation cost is low. The high refractive index polymer has high Abbe number, low birefringence, high transmittance and good mechanical properties at the same time. Through the structural design, the refractive index of the polymer is further improved, the problem that the high refractive index and other optical and mechanical properties are difficult to consider is solved to a certain extent, the use requirement of the polymer as an optical material is met, and the polymer has potential application value in the fields of optics and photoelectronics. High-refractive-index polydithioacetal containing sulfur and selenium elements and a low-refractive-index material are stacked layer by layer in a spin coating mode to form a one-dimensional photonic crystal, and the one-dimensional photonic crystal can be used as a distributed Bragg reflector.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-refractive index polymer material preparation, and in particular relates to a high-refractive index polymer material containing sulfur and selenium elements and a preparation method thereof. Background Art

[0002] The development of the optical and optoelectronic fields is inseparable from the continuous research and development of high-performance high-refractive index polymer materials. Optical materials with high refractive index, low dispersion, high transparency, high thermal stability and good processability can meet the application requirements in cutting-edge fields such as photonic crystals, photoresists, and microlens arrays. However, high refractive index and other optical and mechanical properties are often not taken into account at the same time. It is of great significance to prepare high-refractive index polymer materials with excellent comprehensive properties through structural design.

[0003] From the current development of high refractive index polymer materials, the preparation of sulfur-containing high refractive index polymer materials is relatively extensive. The polarizability of sulfur atoms and sulfur-containing groups is relatively high. The introduction of sulfur atoms into the chain structure has little effect on the color and can provide good impact resistance. The refractive index of traditional sulfur-containing polymers is usually around 1.75. To further increase the refractive index, it is necessary to introduce specific polarizable hydrogen bonds or use methods such as inverse vulcanization and vapor deposition to introduce polysulfide bonds. These methods have a relatively complicated preparation process and will result in an increase in the density of the material or a darker color, and other properties will also deteriorate.

[0004] Selenium, which is in the same family as sulfur, has a larger ratio of polarizability to van der Waals volume, and makes a significant contribution to improving the refractive index. At the same time, selenium can increase the Abbe number of polymers, and the more flexible selenoether bonds are expected to give the material the advantage of low birefringence. Currently, the refractive index of selenium-containing polymers is relatively high, but due to structural limitations, other properties cannot break through inherent limitations, and there are often problems such as too low Abbe number, dark color, and poor thermal stability.

[0005] Therefore, it is urgent to design a novel high refractive index polymer material, which can be prepared under mild conditions and simple steps, and has ultra-high refractive index and good optical and mechanical properties. In the present invention, sulfur and selenium, two high polarizability elements, are introduced into the polymer system together, and their respective advantages are utilized to maintain a balance between other properties while improving the refractive index. In the process of preparing polydithioacetal by condensation of mercaptan and aldehyde monomers, H2O with low refractive index is removed, and SCS structure is formed, the content of high polarizability atoms is further increased, and the color deepening caused by the formation of polysulfide bonds is avoided. This structural design provides a new idea for the development of high refractive index high-performance polymer optical materials, and has application potential in the fields of optics and optoelectronics. Summary of the invention

[0006] The purpose of the present invention is to provide a high refractive index polymer material containing sulfur and selenium elements and a preparation method thereof. The present invention uses high refractive index selenium-containing thiol monomers and aldehyde monomers to prepare high refractive index polydithioacetal containing sulfur and selenium elements under the catalysis of acid, and its refractive index value is 1.7995-1.8569 at 473nm. The method has mild reaction conditions and a simple preparation process. By utilizing the respective advantages of the two elements, the high refractive index polymer has high Abbe number, low birefringence, high transmittance and good mechanical properties. Through structural design, while further improving the refractive index of the polymer, the problem of high refractive index and other optical and mechanical properties being difficult to take into account is solved to a certain extent, and the use requirements of the polymer as an optical material are met, and the polymer has potential application value in the fields of optics and optoelectronics.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] A method for preparing a high refractive index polymer material containing sulfur and selenium elements, the steps of which are as follows:

[0009] A selenium-containing thiol compound and an aldehyde-containing aromatic compound in a molar ratio of thiol to aldehyde of 1:0.25-4 are weighed and dissolved in an organic solvent, and then an acid catalyst in an amount of 0.10-0.45 parts by weight of the aldehyde-containing aromatic compound is added, and the temperature is raised to a certain temperature under stirring to carry out a condensation reaction; after the reaction is completed, the reaction mixture is dripped into an anti-precipitant for precipitation, and the precipitate is collected and vacuum dried at 50-80° C. to a constant weight to obtain the high refractive index polymer material, which is a polydithioacetal polymer containing sulfur and selenium elements, and has the following general structural formula:

[0010]

[0011] Wherein, n is an integer representing the degree of polymerization, and 2≤n≤400, R1 is a selenoether group, and R2 is one or more of an aromatic ring and an aromatic derivative ring.

[0012] Preferably, the R1 is one or more of the following substituents:

[0013]

[0014] Preferably, R2 is one or more of the following substituents:

[0015]

[0016] Preferably, the selenethiolate compound in the above method is one or a mixture of bis(2-mercaptoethyl)selenoether (A), bis(2-mercaptopropyl)selenoether (B), 4,4'-dimercaptodiphenylselenoether (C), 4,4'-dimercaptodiphenyl diselenide (D), 5,5'-seleniumbis(thiophene-2-thiol) (E), 4,4'-dimercaptodinaphthylselenoether (F), 4,4'-dimercaptodiphenylselenoether (G); the aldehyde-containing aromatic The aromatic compound is one or a mixture of benzaldehyde (H), 1-naphthaldehyde (I), 2-naphthaldehyde (J), 9-anthraldehyde (K), p-hydroxybenzaldehyde (L), 3-methoxy-4-hydroxybenzaldehyde (M), biphenyl-3-carboxaldehyde (N), benzothiazole-2-carboxaldehyde (O), benzothiophene-4-carboxaldehyde (P), 9-fluorenecarboxaldehyde (Q), diphenylamino-4-benzaldehyde (R), and 3,5'-dibromobenzaldehyde (S).

[0017]

[0018] Preferably, the organic solvent is one or a mixture of dichloromethane, tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

[0019] Preferably, the concentration of the selenethiolate compound in the organic solvent is 1.2-1.8 mol / L.

[0020] Preferably, the acid catalyst is one or a mixture of p-toluenesulfonic acid, trifluoroacetic acid, zirconium tetrachloride, and hydrochloric acid (12 mol / L).

[0021] Preferably, the reaction temperature is 40 to 100° C., and the reaction time is 1 to 24 hours.

[0022] Preferably, the anti-precipitant is one of methanol, ethanol, ether, n-hexane, ethyl acetate or a mixture of any volume ratio of the above; the volume ratio of the reaction mixture to the anti-precipitant is 1:8-15. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is an infrared spectrum of the high refractive index polydithioacetal containing sulfur and selenium elements prepared in Example 1;

[0024] Figure 2 The fitting curve of the refractive index values ​​of the high-refractive-index polydithioacetal containing sulfur and selenium elements prepared in Example 2 at different wavelengths;

[0025] Figure 3 The UV-visible spectra of the high-refractive-index polydithioacetals containing sulfur and selenium elements prepared in Examples 1 to 5;

[0026] Figure 4 is a differential scanning calorimetry curve of the high refractive index polydithioacetal containing sulfur and selenium elements prepared in Example 5;

[0027] Figure 1 In the infrared spectrum of the polymer shown, -1 The infrared characteristic peak of S-CH-S appeared nearby, indicating the successful preparation of polydithioacetal polymer.

[0028] Table 1 shows the optical and mechanical properties of the high refractive index polydithioacetal containing sulfur and selenium elements prepared in Examples 1-5.

[0029] DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0031] Example 1

[0032] 4742.4 mg of 4,4'-dithiodiphenyl selenide, 1135.9 mg of 1-naphthaldehyde and 1135.9 mg of 2-naphthaldehyde were weighed and dissolved in 10 mL of 1,4'-dioxane, 900 mg of trifluoroacetic acid was added, and the mixture was heated to 60°C under stirring for 4 hours. After the reaction, the reaction mixture was dripped into 100 mL of ethyl acetate and cyclohexane in a volume ratio of 1:1 for precipitation, and the precipitate was collected by centrifugation and dried in a vacuum oven at 60°C to constant weight to obtain a high refractive index polymer material with a structural formula shown in PTA-1. The mass of the polymer PTA-1 obtained was 6102.3 mg. The number average molecular weight of PTA-1 was measured by gel permeation chromatography (GPC) to be 15400 g / mol.

[0033] like Figure 1 As shown, the infrared spectrum of PTA-1 is at 2390 cm -1 The infrared characteristic peak of S-CH-S appeared nearby, indicating the successful preparation of the polymer. Since the molar ratio of the selenium-containing thiol compound to the aldehyde-containing aromatic compound was 1.1:1, the thiol group was excessive, so the infrared peak of the thiol group existed at 2560cm-1, and PTA-1 was a high-fold polymer terminated with thiol groups.

[0034] 80 mg of PTA-1 was dissolved in 1 mL of 1,4-dioxane. After it was completely dissolved, 100 μL of the solution was applied to a glass substrate, and the solvent was evaporated at 60 °C. Then, the refractive index was tested by a prism coupling instrument. The results showed that the refractive index of the polymer PTA-1 was 1.8343 at 473 nm and the film thickness was 11.5 μm. Due to the atoms and groups with small molecular dispersion such as sulfur, selenium and naphthyl contained in the polymer chain structure, the polymer does not have abnormal dispersion in the visible light region, so PTA-1 has both a high refractive index and a high Abbe number of 18. The properties of PTA-1 are shown in Table 1.

[0035]

[0036] Example 2

[0037] Weigh 2980.7 mg of 4,4'-dimercapto-dinaphthyl selenide, 410 mg of biphenyl-3-carboxaldehyde, 243.3 mg of benzothiazole-2-carboxaldehyde and 1025 mg of diphenylamino-4-benzaldehyde, dissolve in 5 mL of N,N-dimethylacetamide, add 419.6 mg of p-toluenesulfonic acid, heat to 70°C under stirring, and react for 2.5 hours; after the reaction, drop the reaction mixture into 60 mL of methanol for precipitation, collect the precipitate by centrifugation, put it into a 60°C vacuum oven and dry it to constant weight to obtain a high refractive index polymer material, the structural formula of which is shown in PTA-2, and the mass of the polymer PTA-2 finally obtained is 3960.2 mg. The number average molecular weight of PTA-2 measured by gel permeation chromatography (GPC) is 26400 g / mol.

[0038] 80 mg of PTA-2 was dissolved in 1 mL of N,N-dimethylacetamide. After it was completely dissolved, 100 μL of the solution was applied to a glass substrate, and the solvent was evaporated at 80 °C. Then, the refractive index was tested by a prism coupling instrument. The refractive index fitting curves of PTA-2 at different wavelengths are shown in Figure 2. Figure 2 The results show that the refractive index of polymer PTA-2 is 1.8216 at 473nm and the film thickness is 10.2μm. The properties of PTA-2 are shown in Table 1.

[0039]

[0040] Example 3

[0041] 2980.2 mg of 4,4'-dithiodiphenyl diselenide, 241.8 mg of p-hydroxybenzaldehyde, 903.8 mg of 3-methoxy-4-hydroxybenzaldehyde and 321.2 mg of benzothiophene-4-carboxaldehyde were weighed and dissolved in 6 mL of a mixed solvent of N,N-dimethylformamide and N-methylpyrrolidone with a volume ratio of 1:1, 220 mg of 12 mol / L hydrochloric acid were added, and the mixture was heated to 80°C under stirring and reacted for 1 hour; after the reaction, the reaction mixture was dripped into 66 mL of ether for precipitation, the precipitate was collected by centrifugation, and dried in a vacuum oven at 60°C to constant weight to obtain a high refractive index polymer material, the structural formula of which is shown in PTA-3, and the mass of the polymer PTA-3 finally obtained was 3655.4 mg. The number average molecular weight of PTA-3 was measured by gel permeation chromatography (GPC) to be 19600 g / mol.

[0042] 80 mg of PTA-3 was dissolved in 1 mL of a mixed solvent (N,N-dimethylformamide: N-methylpyrrolidone, volume ratio 1:1). After complete dissolution, 100 μL of the solution was applied to a glass substrate, the solvent was evaporated at 85 °C, and then the refractive index was tested by a prism coupling instrument. The results showed that the refractive index of the polymer PTA-3 was 1.8408 at 473 nm and the film thickness was 15.4 μm. The chain structure of PTA-3 contains flexible selenium-selenium bonds, selenoether bonds and thioether bonds, which reduce the stacking and orientation of the polymer chain, so the polymer has a low birefringence of 0.0003. The properties of PTA-3 are shown in Table 1.

[0043]

[0044] Example 4

[0045] Weigh 171.1 mg of bis(2-mercaptoethyl)selenoether, 389.8 mg of bis(2-mercaptopropyl)selenoether, 1840.6 mg of 5,5'-selenobis(thiophene-2-thiol) and 751.7 mg of benzaldehyde, dissolve in 5 mL of dichloromethane, add 75.2 mg of zirconium tetrachloride, heat to 30°C under stirring, and react for 6 hours; after the reaction, drop the reaction mixture into 70 mL of ethanol for precipitation, collect the precipitate by centrifugation, put it into a 60°C vacuum oven and dry it to constant weight to obtain a high refractive index polymer material, the structural formula is shown in PTA-4, and the mass of the polymer PTA-4 is 2803.1 mg. The number average molecular weight of PTA-4 measured by gel permeation chromatography (GPC) is 14600 g / mol.

[0046] 80 mg of PTA-4 was dissolved in 1 mL of dichloromethane. After complete dissolution, 100 μL of the solution was applied to a glass substrate, the solvent was evaporated at 25 °C, and then the refractive index was tested by a prism coupling instrument. The results showed that the refractive index of polymer PTA-4 was 1.7995 at 473 nm and the film thickness was 12.6 μm. The flexible alkyl chain, selenoether bond and thioether bond in the chain structure of PTA-4 accounted for a high proportion, which inhibited the interchain stacking and increased the transmittance of the material in the visible light region. The transmittance of the 12.6 μm film at 500 nm reached 95.5%. The properties of PTA-4 are shown in Table 1.

[0047]

[0048] Example 5

[0049] Weigh 4965.9 mg of 4,4'-dimercaptodiphenyl selenoether, 1196.2 mg of 9-anthracenealdehyde, 901.2 mg of 9-fluorene carboxaldehyde and 306.2 mg of 3,5'-dibromobenzaldehyde, dissolve in 8 mL of tetrahydrofuran, add 721.1 mg of trifluoroacetic acid, heat to 55 ° C under stirring, and react for 4 hours; after the reaction, drop the reaction mixture into 80 mL of methanol for precipitation, collect the precipitate by centrifugation, put it into a 60 ° C vacuum oven and dry it to constant weight to obtain a high refractive index polymer material, the structural formula is shown in PTA-5, and the mass of the polymer PTA-5 finally obtained is 6374.6 mg. The number average molecular weight of PTA-5 measured by gel permeation chromatography (GPC) is 23700 g / mol.

[0050] 80 mg of PTA-5 was dissolved in 1 mL of tetrahydrofuran. After it was completely dissolved, 100 μL of the solution was applied to a glass substrate, and the solvent was evaporated at 40°C. Then, the refractive index of the polymer PTA-5 was tested by a prism coupling instrument. The results showed that the refractive index of the polymer PTA-5 was 1.8569 at 473 nm and the film thickness was 13.1 μm. The differential scanning calorimetry curve of PTA-5 is shown in Figure 2. Figure 4 As shown in Table 1, due to the rigid polymer chain structure, PTA-5 has a high glass transition temperature of 87.7°C and good thermal stability. The properties of PTA-5 are shown in Table 1.

[0051]

[0052] As can be seen from the above embodiments, the present invention provides a method for preparing a high-refractive-index polydithioacetal containing sulfur and selenium elements. The preparation process of the present invention is simple and the reaction conditions are mild. It can be seen from experimental verification that the obtained polymer material has a high refractive index, a high Abbe number, a low birefringence, a high transmittance and good mechanical properties. The high-refractive-index polydithioacetal containing sulfur and selenium elements and the low-refractive-index material are stacked layer by layer by spin coating to form a one-dimensional photonic crystal, which is used as a distributed Bragg reflector; it can be miscible with a low-refractive-index monomer as a high-refractive-index photocurable adhesive, which is used in cutting-edge optical and optoelectronic fields such as lithography, holography, and optical waveguides.

[0053] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general method used herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A high refractive index polymer material containing sulfur and selenium elements, characterized in that: It is a polydithioacetal polymer containing sulfur and selenium elements, and its general structure is shown below: Wherein, n is an integer representing the degree of polymerization, and 2≤n≤400, R1 is a selenoether group, and R2 is one or more of an aromatic ring and an aromatic derivative ring.

2. The high refractive index polymer material containing sulfur and selenium elements as claimed in claim 1, characterized in that: R1 is one or more of the following substituents, 3. The high refractive index polymer material containing sulfur and selenium elements as claimed in claim 1, characterized in that: R2 is one or more of the following substituents, 4. The method for preparing a high refractive index polymer material containing sulfur and selenium elements as claimed in claim 1, 2 or 3, characterized in that: A selenium-containing thiol compound and an aldehyde-containing aromatic compound in a molar ratio of thiol to aldehyde of 1:0.25-4 are weighed and dissolved in an organic solvent, and then an acid catalyst in an amount of 0.10-0.45 parts by weight of the aldehyde-containing aromatic compound is added, and the temperature is raised to a certain temperature under stirring to carry out a condensation reaction; after the reaction is completed, the reaction mixture is dripped into a reverse precipitant for precipitation, and the precipitate is collected and vacuum dried at 50-80° C. to a constant weight to obtain the high refractive index polymer material.

5. The method for preparing a high refractive index polymer material containing sulfur and selenium elements as claimed in claim 4, characterized in that: The selenithiolate compound is one or a mixture of bis(2-mercaptoethyl)selenoether (A), bis(2-mercaptopropyl)selenoether (B), 4,4'-dimercaptodiphenylselenoether (C), 4,4'-dimercaptodiphenyl diselenide (D), 5,5'-selenobis(thiophene-2-thiol) (E), 4,4'-dimercaptodinaphthylselenoether (F), and 4,4'-dimercaptodiphenylselenoether (G); the aldehyde-containing aromatic compound is benzaldehyde ( H), 1-naphthaldehyde (I), 2-naphthaldehyde (J), 9-anthraldehyde (K), p-hydroxybenzaldehyde (L), 3-methoxy-4-hydroxybenzaldehyde (M), biphenyl-3-carboxaldehyde (N), benzothiazole-2-carboxaldehyde (O), benzothiophene-4-carboxaldehyde (P), 9-fluorenecarboxaldehyde (Q), diphenylamino-4-benzaldehyde (R), 3,5'-dibromobenzaldehyde (S) or a mixture thereof; the structural formulas thereof are shown below respectively, 6. The method for preparing a high refractive index polymer material containing sulfur and selenium elements as claimed in claim 4, characterized in that: The organic solvent is one or a mixture of dichloromethane, tetrahydrofuran, 1,4-dioxane, N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone.

7. The method for preparing a high refractive index polymer material containing sulfur and selenium elements as claimed in claim 4, characterized in that: The concentration of the selenethiolate compound in the organic solvent is 1.2-1.8 mol / L.

8. The method for preparing a high refractive index polymer material containing sulfur and selenium elements as claimed in claim 4, characterized in that: The acid catalyst is one or a mixture of p-toluenesulfonic acid, trifluoroacetic acid, zirconium tetrachloride and hydrochloric acid.

9. The method for preparing a high refractive index polymer material containing sulfur and selenium elements as claimed in claim 4, characterized in that: The reaction temperature is 40 to 100° C., and the reaction time is 1 to 24 hours.

10. The method for preparing a high refractive index polymer material containing sulfur and selenium elements as claimed in claim 4, characterized in that: The reverse precipitant is one of methanol, ethanol, ether, n-hexane and ethyl acetate or a mixture of several of them in any volume ratio; the volume ratio of the reaction mixture to the reverse precipitant is 1:8-15.

Citation Information

Patent Citations

  • Polyimide polymer containing selenium and preparation method and application thereof

    CN106565955A

  • New selenium-containing aliphatic compound

    JP1999140046A

  • Selenium-containing transparent optical material

    US6124424A