Modified polylactic acid aerogel for oil-water separation and preparation method thereof

By adding carbon powder and nanosilicon dioxide to the polylactic acid aerogel and sonicating it with ethanol and silane coupling agents, an efficient modified polylactic acid aerogel was prepared, solving the problem of existing materials in complex environments. The problems of low separation efficiency and environmental pollution have achieved efficient and environmentally friendly oil-water separation.

CN118994712AActive Publication Date: 2024-11-22WUHAN TEXTILE UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410992164.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-22
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing materials used for oil-water separation are prone to clogging when treating high-concentration suspended solid wastewater, have high costs, are at a high risk of environmental pollution, and the separation efficiency is reduced in complex and multi-oil environments.

Method used

Using modified polylactic acid aerogel, the hydrophobic properties and separation of aerogel are improved by adding carbon powder and nanosilicon dioxide to the polylactic acid masterbatch, and ultrasonic treatment and freeze-dried use of ethanol and silane coupling agents. efficiency.

Benefits of technology

It improves the oil-water separation efficiency, avoids secondary environmental pollution, and the material is degradable, making it suitable for oil-water separation in complex and multi-oil environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994712A_ABST
    Figure CN118994712A_ABST
Patent Text Reader

Abstract

The invention provides modified polylactic acid aerogel for oil-water separation and a preparation method thereof.The preparation method comprises the steps that carbon powder dispersion liquid is prepared, polylactic acid master batches are placed in the carbon powder dispersion liquid to be stirred for preset time, the obtained solution is subjected to ultrasonic treatment and freezing, then taken out and placed in a freeze dryer to be freeze-dried, and aerogel is obtained; and placing the aerogel in a dispersed nano silicon dioxide solution, and carrying out ultrasonic treatment for a preset time by taking ethanol and a silane coupling agent as dispersion liquid, so as to obtain the modified polylactic acid aerogel for oil-water separation. According to the preparation method, the bio-based degradable material polylactic acid is taken as a matrix, and the carbon powder is added into the polylactic acid material in a blending manner, so that the photothermal conversion efficiency and the separation efficiency of the polylactic acid aerogel are improved. Ethanol and a silane coupling agent are added on a matrix of the aerogel, so that nano silicon dioxide can be effectively grafted to the surface of the polylactic acid aerogel, the hydrophobic property of the polylactic acid aerogel is improved, and the oil-water separation efficiency of the polylactic acid aerogel is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aerogels, and in particular to a modified polylactic acid aerogel for oil-water separation and a preparation method thereof. Background Art

[0002] The impact of seawater pollution caused by oil spills and the increase in industrial oily wastewater discharge on water quality, aquatic ecosystems and human health is an urgent problem to be solved. The materials currently used for oil-water separation mainly include the following categories: 1. Inorganic ceramic membrane materials. This type of material is widely used in the field of oil-water separation due to its high temperature resistance, corrosion resistance, high mechanical strength, strong anti-pollution ability, large permeability, easy cleaning, good separation performance and long service life. Despite its excellent performance, its cost is relatively high, and it is easy to clog when treating wastewater with high concentrations of suspended solids, requiring regular cleaning and maintenance. 2. Hydrophobic and oleophilic materials. This type of material has the characteristics of selectively adsorbing oil but not water. It is widely used in the treatment of oily wastewater and can effectively adsorb and separate oil from water. It is particularly suitable for wastewater generated by catering, metal processing, grain and oil processing, leather processing and other industries, but it may be affected by changes in temperature and pH value, resulting in a decrease in separation efficiency. In addition, in a complex multi-oil environment, the material may be difficult to maintain efficient selective separation and is easily contaminated by non-target substances, affecting the separation efficiency. 3. Modified nanofibers: Through the modification of nanofibers, selective permeability or rejection of oil or water can be achieved, thereby achieving the purpose of oil-water separation. However, its manufacturing process is complicated, the cost is high, and it may cause unknown risks to human health and the environment. In particular, during the disposal of treated materials, strict control is required to avoid environmental pollution.

[0003] Aerogel, as a nanoporous material, has unique advantages such as high specific surface area, low density, and high pore size, and has broad application prospects in oil-water separation. Polylactic acid (PLA) is a biodegradable material. Compared with oil-water separation materials made of other materials, aerogel used to prepare oil-water separation will not cause secondary pollution to the environment after use.

[0004] In view of this, it is necessary to design an improved modified polylactic acid aerogel for oil-water separation and a preparation method thereof. Summary of the invention

[0005] In view of the above-mentioned defects of the prior art, the object of the present invention is to provide a modified polylactic acid aerogel for oil-water separation and a preparation method thereof, so as to improve the oil-water separation efficiency of the polylactic acid aerogel without causing secondary pollution to the environment.

[0006] To achieve the above object, the present invention provides a method for preparing a modified polylactic acid aerogel for oil-water separation, comprising the following steps:

[0007] S1. Weigh a predetermined amount of carbon powder, and perform ultrasonic treatment with an organic solvent as a dispersant to obtain a carbon powder dispersion;

[0008] S2. Weigh a predetermined amount of polylactic acid masterbatch, place it in the carbon powder dispersion described in step S1 and stir it for a predetermined time. After the stirring is completed, the resulting solution is ultrasonically treated, frozen, taken out and placed in a freeze dryer for freeze drying to obtain an aerogel;

[0009] S3. placing the aerogel described in step S2 in a dispersed nano-silicon dioxide solution, using ethanol and a silane coupling agent as a dispersion liquid, and ultrasonicating for a predetermined time to obtain a modified polylactic acid aerogel for oil-water separation.

[0010] As a further improvement of the present invention, the mass of the carbon powder is 1-2% of the mass of the polylactic acid masterbatch.

[0011] As a further improvement of the present invention, in step S1, the organic solvent is dioxane, and the ultrasonic time is 1 to 2 hours.

[0012] As a further improvement of the present invention, in step S2, the stirring rate is 500-600 r / min, the stirring temperature is 35-45° C., and the stirring time is 10-12 h.

[0013] Furthermore, the ultrasonic time is 30 to 40 minutes; the freezing temperature is -30 to -20°C, and the freezing time is 5 to 8 hours; the freeze-drying time is 46 to 50 hours, and the cold trap temperature of the freeze dryer is -65 to -60°C.

[0014] As a further improvement of the present invention, in step S3, the ultrasonic time is 30 to 40 minutes.

[0015] Furthermore, the mass ratio of the aerogel to the nano-silicon dioxide is 3:(1-2); and the mass ratio of the ethanol to the silane coupling agent is 10:(1-2).

[0016] The present invention also provides a modified polylactic acid aerogel for oil-water separation, which is prepared by the above-mentioned preparation method of the modified polylactic acid aerogel for oil-water separation.

[0017] The beneficial effects of the present invention are:

[0018] The invention provides a modified polylactic acid aerogel for oil-water separation and a preparation method thereof. The invention comprises the following steps: preparing a carbon powder dispersion, placing a polylactic acid masterbatch in the carbon powder dispersion and stirring for a predetermined time, taking out the obtained solution after ultrasonication and freezing and placing it in a freeze dryer for freeze drying to obtain an aerogel, placing the aerogel in a dispersed nano-silicon dioxide solution, using ethanol and a silane coupling agent as a dispersion liquid, and ultrasonication to obtain a modified polylactic acid aerogel for oil-water separation. The invention uses polylactic acid, a bio-based degradable material, as a matrix, and blends and adds carbon powder into the polylactic acid material to improve the photothermal conversion efficiency and separation efficiency of the polylactic acid aerogel. Due to the hydrophilicity of the polylactic acid material, the polylactic acid aerogel needs to be hydrophobically modified. Ethanol and a silane coupling agent are added to the matrix of the aerogel so that the nano-silicon dioxide can be effectively grafted to the surface of the polylactic acid aerogel, thereby improving the hydrophobicity of the polylactic acid aerogel and thus improving the oil-water separation efficiency of the polylactic acid aerogel.

[0019] In the present invention, the addition of a silane coupling agent can effectively improve the grafting rate of nano-silica, and the silane coupling agent can provide more loading sites for the nano-silica, greatly improving the stability of the grafted and modified nano-silica, and the addition of ethanol can further improve the grafting rate of the silica; the addition of a silane coupling agent to the silica can give more groups to the surface of the nano-silica in the presence of rich functional groups, and under the condition of ethanol activation, the thiol groups on the silica are combined with the unsaturated bonds in the polylactic acid resin by chemical bonds, thereby fundamentally avoiding the loss of the silica. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a characterization diagram related to the modified polylactic acid aerogel for oil-water separation provided by the present invention.

[0021] Figure 2 This is a diagram showing the adsorption effect of the modified polylactic acid aerogel for oil-water separation provided by the present invention.

[0022] Figure 3 This is an optical photograph of the solution after oil-water separation of the present invention.

[0023] Figure 4 This is a diagram of the nano-silicon dioxide grafting mechanism provided by the present invention. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0025] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0026] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0027] The present invention provides a method for preparing a modified polylactic acid aerogel for oil-water separation, comprising the following steps:

[0028] S1. Weigh a predetermined amount of carbon powder, and perform ultrasonic treatment using an organic solvent as a dispersant to obtain a carbon powder dispersion.

[0029] Specifically, the mass of the carbon powder is preferably 1-2% of the mass of the polylactic acid masterbatch, the organic solvent is preferably dioxane, and the ultrasonication time is preferably 1-2 hours.

[0030] S2. Weigh a predetermined amount of polylactic acid masterbatch, place it in the carbon powder dispersion in step S1 and stir for a predetermined time. After stirring, the resulting solution is ultrasonicated and frozen, then taken out and placed in a freeze dryer for freeze drying to obtain aerogel.

[0031] Specifically, the stirring rate is preferably 500-600 r / min, the stirring temperature is preferably 35-45°C, and the stirring time is preferably 10-12 h; the ultrasonic time is preferably 30-40 min; the freezing temperature is preferably -30--20°C, and the freezing time is preferably 5-8 h; the preferred freeze-drying time is 46-50 h, and the freeze dryer cold trap temperature is preferably -65--60°C.

[0032] S3. placing the aerogel in step S2 in a dispersed nano-silicon dioxide solution, using ethanol and a silane coupling agent as a dispersion liquid, and ultrasonicating for a predetermined time to obtain a modified polylactic acid aerogel for oil-water separation.

[0033] Specifically, the mass ratio of aerogel to nano-silica is preferably 3:(1-2); the mass ratio of ethanol to silane coupling agent is preferably 10:(1-2); and the ultrasonic time is preferably 30-40 min.

[0034] The preparation method of the modified polylactic acid aerogel for oil-water separation provided by the present invention will be described below in conjunction with specific embodiments.

[0035] Example 1

[0036] Example 1 provides a method for preparing a modified polylactic acid aerogel for oil-water separation, comprising the following steps:

[0037] S1. Weigh 0.015 g of carbon powder and perform ultrasonic treatment for 1 h using dioxane as a dispersant to obtain a carbon powder dispersion;

[0038] S2. Weigh 1.5 g of polylactic acid masterbatch, place it in the carbon powder dispersion and stir for 12 hours, the stirring rate is 600 r / min, and the stirring temperature is 40°C; after the stirring is completed, the resulting solution is ultrasonicated for 30 minutes, placed in a -20°C refrigerator and frozen for 6 hours, and after the freezing is completed, it is taken out and placed in a freeze dryer for freeze drying for 48 hours, and the cold trap temperature of the freeze dryer is -60°C to obtain an aerogel;

[0039] S3. Place the aerogel in a dispersed nano-silica solution, use ethanol and silane coupling agent as the dispersion liquid, the mass ratio of aerogel to nano-silica is 3:1, the mass ratio of ethanol to silane coupling agent is 10:1, and ultrasonicate for 30 minutes to obtain modified polylactic acid aerogel for oil-water separation.

[0040] Embodiment 2-4

[0041] Examples 2-4 respectively provide a method for preparing a modified polylactic acid aerogel for oil-water separation. Compared with Example 1, the only difference is that the carbon powder in Example 2 is 0.030 g, the mass ratio of aerogel to nano-silicon dioxide in Example 3 is 3:2, and the mass ratio of ethanol to silane coupling agent in Example 4 is 10:2. The other experimental parameters and conditions are basically the same as those in Example 1 and will not be repeated here.

[0042] Comparative Examples 1-3

[0043] Comparative Examples 1-3 respectively provide a method for preparing a modified polylactic acid aerogel for oil-water separation. Compared with Example 1, the only difference is that the carbon powder in Comparative Example 1 is 0.075 g, the mass ratio of aerogel to nano-silica in Comparative Example 2 is 1:1, and the mass ratio of ethanol to silane coupling agent in Comparative Example 3 is 10:3. The other experimental parameters and conditions are basically the same as those in Example 1 and will not be repeated here.

[0044] The performance of the prepared modified polylactic acid aerogel for oil-water separation was tested, and the results are shown in the following table.

[0045] Table 1 Performance test results

[0046]

[0047] As can be seen from Table 1, the carbon powder blended modified aerogel prepared by the method of the present invention has an extremely high specific surface area and nano-scale pores, and the adsorption capacity is higher than that of most traditional materials. Compared with the adsorption rate of macroporous adsorption materials, the adsorption rate is slightly slower, but in the nanoporous structure, the adsorption process is more stable and continuous. The surface chemical properties and pore size distribution of the aerogel material have a significant effect on the adsorption rate. The aerogel separation efficiency is high, especially the chemically modified aerogel material can be hydrophobic or lipophilic, so that it performs well in oil-water separation.

[0048] In Comparative Example 1, excessive carbon powder was added, resulting in excessive carbon powder filling the pores of the aerogel, resulting in a decrease in pore size and a decrease in porosity. The addition of carbon powder may enhance the hardness and rigidity of the aerogel, but at the same time may reduce its elastic modulus and toughness. This is because the hardness of carbon powder is higher than that of PLA, and its addition may cause uneven stress distribution inside the aerogel, thereby affecting its compressive and tensile strength.

[0049] In Comparative Example 2, excessive addition of nano-silicon dioxide causes the pore structure of the aerogel to become more complex, the pore size to decrease, the porosity to decrease, and the aerogel to become brittle, reducing its elasticity and toughness. This is because too much nano-SiO2 may cause internal stress concentration in the material, thereby reducing the overall mechanical properties of the material. An appropriate amount of nano-SiO2 can enhance the mechanical strength of PLA aerogel.

[0050] In Comparative Example 3, excessive silane coupling agent was added, resulting in excessive crosslinking between PLA molecular chains, which increased the crosslinking density of the aerogel, causing the pore structure of the aerogel to become dense, the porosity to decrease, and the agglomeration of the nanofiller. This is because excessive coupling agent may cause strong interactions between filler particles, thereby reducing dispersibility and affecting the uniformity of the aerogel, further causing the material to become brittle, reducing its elasticity and toughness, and thus affecting its impact resistance and fatigue resistance.

[0051] like Figure 1 As shown, the characterization diagrams of pure polylactic acid aerogel, modified polylactic acid aerogel for oil-water separation prepared in Example 1, and aerogel prepared in Comparative Example 1 show that, when an appropriate amount of carbon powder and nano-silica grafted with a silane coupling agent are added, the aerogel in Example 1 exhibits a better microscopic morphology than the pure polylactic acid aerogel and the microscopic morphology of Comparative Example 1, which is specifically manifested in the uniform distribution of pore size in Example 1. This good structure ensures that the various properties of Example 1 reach the optimal state.

[0052] Prepare an oil-water mixed solution containing Sudan IV and Tween-80 and conduct an oil-water separation experiment. Figure 2As shown, from left to right are the oil-water mixed solution and the solution adsorbed by the aerogel prepared in Comparative Example 1 and Example 1. It can be seen that Example 1 has the best oil-water separation effect.

[0053] like Figure 3 As shown in the figure, it is an optical microscope picture of the solution after oil-water separation. Figure 2 The separation effects shown correspond to each other. The oil-water separation effect can be judged from the diameter of the oil droplets, among which the oil-water separation effect of Example 1 is the best.

[0054] like Figure 4 As shown, it is a diagram of the nano-silicon dioxide grafting mechanism provided by the present invention, wherein R is an organic functional group, and according to the type of coupling agent, R can be a mercapto group, an amino group, an epoxy group, a vinyl group, a cyano group, etc. The silane coupling agent reacts with water to generate silanols and alcohols, and a condensation reaction occurs between the silanols to form a silicon-oxygen bond, and the silanols react with the inorganic surface hydroxyl groups to form a chemical bond, and the organic functional groups in the silane coupling agent are combined with the organic material. Through the above steps, the silane coupling agent can form a stable chemical bond between the organic and inorganic materials, thereby improving the compatibility and performance of the materials.

[0055] In summary, the present invention uses bio-based degradable material polylactic acid as a matrix, and blends carbon powder into the polylactic acid material to improve the light-to-heat conversion efficiency and separation efficiency of polylactic acid aerogel. Ethanol and silane coupling agent are added to the aerogel matrix, so that nano-silicon dioxide can be effectively grafted onto the surface of polylactic acid aerogel, improving the hydrophobic properties of polylactic acid aerogel, thereby improving the oil-water separation efficiency of polylactic acid aerogel.

[0056] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing modified polylactic acid aerogel for oil-water separation, characterized in that: The following steps are involved: S1. Weigh a predetermined amount of carbon powder, and perform ultrasonic treatment with an organic solvent as a dispersant to obtain a carbon powder dispersion; S2. Weigh a predetermined amount of polylactic acid masterbatch, place it in the carbon powder dispersion described in step S1 and stir it for a predetermined time. After the stirring is completed, the resulting solution is ultrasonically treated, frozen, taken out and placed in a freeze dryer for freeze drying to obtain an aerogel; S3. placing the aerogel described in step S2 in a dispersed nano-silicon dioxide solution, using ethanol and a silane coupling agent as a dispersion liquid, and ultrasonicating for a predetermined time to obtain a modified polylactic acid aerogel for oil-water separation.

2. The method for preparing modified polylactic acid aerogel for oil-water separation according to claim 1, characterized in that: The mass of the carbon powder is 1-2% of the mass of the polylactic acid masterbatch.

3. The method for preparing modified polylactic acid aerogel for oil-water separation according to claim 1, characterized in that: In step S1, the organic solvent is dioxane, and the ultrasonication time is 1 to 2 hours.

4. The method for preparing modified polylactic acid aerogel for oil-water separation according to claim 1, characterized in that: In step S2, the stirring rate is 500-600 r / min, the stirring temperature is 35-45° C., and the stirring time is 10-12 h.

5. The method for preparing modified polylactic acid aerogel for oil-water separation according to claim 1, characterized in that: In step S2, the ultrasonic treatment time is 30 to 40 minutes.

6. The method for preparing modified polylactic acid aerogel for oil-water separation according to claim 5, characterized in that: The freezing temperature is -30 to -20°C, and the freezing time is 5 to 8 hours.

7. The method for preparing modified polylactic acid aerogel for oil-water separation according to claim 6, characterized in that: The freeze drying time is 46 to 50 hours, and the cold trap temperature of the freeze dryer is -65 to -60°C.

8. The method for preparing modified polylactic acid aerogel for oil-water separation according to claim 1, characterized in that: In step S3, the ultrasonic treatment time is 30 to 40 minutes.

9. The method for preparing modified polylactic acid aerogel for oil-water separation according to claim 8, characterized in that: The mass ratio of the aerogel to the nano-silicon dioxide is 3:(1-2); the mass ratio of the ethanol to the silane coupling agent is 10:(1-2).

10. A modified polylactic acid aerogel for oil-water separation, characterized in that: The modified polylactic acid aerogel for oil-water separation is prepared by the preparation method of any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of biodegradable oil and water separation porous film

    CN108816055A

  • Degradable high-hydrophobicity aerogel porous material and preparation method thereof

    CN114085418A

  • Efficient oil-water separation composite foam based on surface engineering and preparation method thereof

    CN114425269A

  • Degradable zipper

    CN118006097A