Insulated wire material resistant to high-temperature aging and cracking
By adding modified carbon nanotubes and core-shell particles to the insulating wire material, the problem of aging and cracking of polyvinyl chloride materials at high temperatures is solved, the flexibility and impact resistance of the insulating wire are improved, and good heat resistance and Aging resistance improves the overall performance of the material.
Patent Information
- Application Number
- CN202411183215.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-22
AI Technical Summary
Existing insulating wire materials are prone to aging and cracking at high temperatures, have poor thermal stability and insufficient impact resistance, especially in the fields of high-voltage and high-frequency conversion technology.
By adding modified carbon nanotubes and core-shell particles to the polyvinyl chloride material, the carbon nanotubes are modified with macromolecular anti-aging agents, combined with silica coated nanoalumina and maleic anhydride grafted SEBS elastomer, and post-emulsification is used Technology prepares insulating wire materials with excellent flexibility, impact resistance and heat resistance.
It significantly improves the flexibility and impact resistance of the insulating wire material, extends the oxidation induction time, maintains good heat resistance, enhances the aging resistance of the material, and avoids the decline in mechanical properties caused by thermal oxygen aging.
Smart Images

Figure BDA0005012806590000071 
Figure BDA0005012806590000081 
Figure BDA0005012806590000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of insulating wires, and in particular relates to an insulating wire material resistant to high temperature aging and cracking. Background Art
[0002] Insulated wire is a special insulated wire material, mainly used in various power transformers, communication transformers, electric coils, motors and other electronic components. With the continuous expansion of the application field of insulated wires, people's requirements for insulated wires are getting higher and higher, especially in the field of high voltage and high frequency conversion technology, which requires not only good conductivity of the metal conductor, but also the insulation layer, which needs to have good high temperature resistance and impact resistance.
[0003] Existing insulated wires with excellent insulation layer performance use polyvinyl chloride materials as the insulation layer. Polyvinyl chloride has good corrosion resistance, insulation, chemical stability and stable electrical properties, but its thermal stability is poor. When the temperature is high, it is easy to decompose and cause the product to change color. In addition, the intermolecular force of polyvinyl chloride is very strong, its own toughness is insufficient, and its impact resistance is extremely poor. It is easy to be brittle when impacted. In order to improve the impact resistance of polyvinyl chloride, the existing technology adds toughening modifiers, such as ethylene-vinyl acetate copolymers, synthetic rubber, etc., to the polyvinyl chloride body. However, the addition of toughening modifiers can easily cause thermal oxidation aging of the insulated wire during use, resulting in a further decrease in its mechanical properties. Summary of the invention
[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide an insulating wire material that is resistant to high temperature aging cracking. By adding modified carbon nanotubes and core-shell particles, the insulating wire material is endowed with excellent flexibility, impact resistance, aging resistance and heat resistance.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] An insulating wire material resistant to high temperature aging cracking comprises the following raw materials in parts by weight: 60-70 parts of polyvinyl chloride, 5-10 parts of modified carbon nanotubes, 2-5 parts of core-shell particles, 1-2 parts of plasticizer, 0.1-0.5 parts of lubricant, and 1-3 parts of stabilizer;
[0007] The modified carbon nanotubes are prepared by introducing a macromolecular antioxidant into the carbon nanotube structure by chemical reaction, wherein the macromolecular antioxidant is prepared by using p-phenylenediamine and glycidyl ether as reaction monomers; the core-shell particles are prepared by using a post-emulsification technology, with a silicon dioxide-coated nano-alumina as a rigid core and a maleic anhydride-grafted SEBS elastomer as a flexible shell.
[0008] Preferably, the plasticizer is one or more combinations of dioctyl adipate, dimethyl phthalate, dioctyl phthalate, and diisodecyl phthalate; the stabilizer is a calcium zinc stabilizer; and the lubricant is one of polyethylene wax and oxidized polyethylene wax.
[0009] Preferably, the method for preparing the modified carbon nanotubes comprises the following steps:
[0010] A. Place p-phenylenediamine and glycidyl ether in a reactor, add toluene solvent, stir and mix, heat to 95-110°C after mixing evenly, react for 10-12 hours, cool to room temperature after the reaction is completed, remove the solvent by rotary evaporation, and prepare a macromolecular antioxidant;
[0011] B. Take carbon nanotubes in a mixed solution of concentrated sulfuric acid and concentrated nitric acid, place at 70-90°C for reaction for 4-6 hours, filter and wash the product until it is neutral and dry it, place the obtained carboxylated carbon nanotubes in a reactor, add thionyl chloride and N,N-dimethylformamide, ultrasonically disperse for 0.5-1 hour, then place at 70-80°C for reflux reaction for 20-24 hours, and after the reaction is completed, rotary evaporate and dry to prepare acyl chloride carbon nanotubes;
[0012] C. Take the acyl chloride carbon nanotubes and the macromolecular antioxidant in a reactor, add N,N-dimethylformamide and pyridine, and react at 75-90°C in a nitrogen atmosphere for 20-24 hours. After the reaction is completed, filter, wash and dry to prepare modified carbon nanotubes.
[0013] Preferably, the molar ratio of p-phenylenediamine to glycidyl ether in step A is 3 to 3.5:1.
[0014] Preferably, in step C, the mass ratio of the acyl chloride carbon nanotubes to the macromolecular antioxidant is 1 to 2.5:1.
[0015] Preferably, the method for preparing the core-shell particles comprises the following steps:
[0016] (1) Nano-alumina, ethanol and deionized water are placed in a reactor, ammonia water is added to adjust the pH value of the system to 11-12, ultrasonically dispersed uniformly, and then placed in a water bath at 25-35° C. and heated at a constant temperature for 0.5-1 h, tetraethyl silicate is dissolved in a mixed solution of ethanol and deionized water, mixed uniformly, and allowed to stand for 15-30 min, and then added to the reactor to continue the reaction for 20-24 h. After the reaction is completed, the solution is centrifuged, washed, and dried to prepare silica-coated nano-alumina;
[0017] (2) ultrasonically dispersing the silica-coated nano-alumina in anhydrous ethanol, adding 3-aminopropyltriethoxysilane and deionized water, stirring and mixing, placing at 65-75° C. for 5-6 hours, and after the reaction is completed, centrifuging, washing, and drying to prepare modified silica-coated nano-alumina;
[0018] (3) Maleic anhydride grafted SEBS was dissolved in cyclohexane, modified silica-coated nano-alumina and N,N'-dicyclohexylcarbodiimide were added and ultrasonically dispersed uniformly, and the mixture was placed at 75-95°C for condensation and reflux for 20-24 hours to obtain an oil phase solution, Tween 80 and Span 80 were dissolved in deionized water to obtain an aqueous phase solution, and the oil phase solution was slowly added dropwise to the aqueous phase solution at 3000-4700 rpm, and then the homogenizer was increased to 9000-9500 rpm for emulsification for 3-5 minutes, and finally the mixture was placed in a water bath at 40-50°C for rotary evaporation to remove the solvent, and core-shell particles were prepared after centrifugation, washing and drying.
[0019] Preferably, in step (2), the mass ratio of maleic anhydride grafted SEBS to modified silica-coated nano-alumina is 1:2-10.
[0020] Preferably, in step (2), the mass ratio of Tween 80 to Span 80 is 3.7-4.2:1.
[0021] Preferably, the preparation method of the insulating wire material is specifically as follows: pouring parts by weight of polyvinyl chloride, modified carbon nanotubes, plasticizer, lubricant, and stabilizer into a mixer, stirring and mixing, pouring the core-shell particles into the mixer, continuing to stir and mix for 1 to 2 hours, discharging the material, and preparing the insulating wire material.
[0022] Beneficial effects of the present invention:
[0023] The invention uses p-phenylenediamine and glycidyl ether as reaction monomers to synthesize a macromolecular antioxidant, wherein the epoxy group in the glycidyl ether structure reacts with the amino group at one end of the p-phenylenediamine, and then the macromolecular antioxidant is further grafted with acyl chloride carbon nanotubes, so that the amino group in the macromolecular antioxidant structure reacts with the acyl chloride group on the surface of the carbon nanotube, thereby firmly combining the macromolecular antioxidant with the carbon nanotube through a chemical bond, giving the macromolecular antioxidant excellent anti-migration performance, and generating a plurality of anti-aging functional groups -NH through the reaction, thereby enhancing the aging protection effect of the macromolecular antioxidant, and at the same time, after the surface of the carbon nanotube is modified by the macromolecular antioxidant, the surface lipophilicity of the carbon nanotube is improved, which is conducive to the dispersion of the carbon nanotubes and avoids the agglomeration of the carbon nanotubes, which leads to the reduction of the mechanical properties of the material.
[0024] The present invention adopts a sol-gel method to prepare silica-coated nano-alumina, and uses 3-aminopropyltriethoxysilane to surface-functionalize silica-coated nano-alumina, and then reacts the maleic anhydride group on the maleic anhydride grafted SEBS molecular chain with the amino group on the surface of the silica-coated nano-alumina, and adopts a post-emulsification technology to prepare core-shell particles. The modified silica-coated nano-alumina has better dispersibility in the matrix, can effectively prevent the extension of microcracks, and can effectively buffer part of the energy, so that the toughness of the insulating wire material is improved, and it has excellent heat resistance and can be used as a medium to transfer and absorb heat. In addition, the maleic anhydride grafted SEBS elastomer is grafted on the surface of the silica-coated nano-alumina, with the silica-coated nano-alumina as a rigid core and the maleic anhydride grafted SEBS elastomer as a flexible shell, giving the insulating wire material excellent heat resistance and impact resistance. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In the examples and comparative examples of the present invention, the maleic anhydride grafted SEBS is produced by Dongguan Xingyuan Chemical Co., Ltd.; the carbon nanotubes are produced by Nanjing Xianfeng Nanomaterial Technology Co., Ltd., with a diameter of 30 to 50 nm and a length of 0.5 to 2 μm.
[0027] Embodiment 1 A method for preparing modified carbon nanotubes comprises the following steps:
[0028] A. Take 3.3g of p-phenylenediamine and 2.6g of glycidyl ether in a reactor, add 100mL of toluene solvent and stir to mix, mix evenly and heat to 100°C, react for 12h, cool to room temperature after the reaction is completed, remove the solvent by rotary evaporation, and prepare a macromolecular antioxidant;
[0029] B. Take 2g of carbon nanotubes in a mixture of 90mL of concentrated sulfuric acid and 30mL of concentrated nitric acid, place it at 85°C for 6h, filter and wash the product until it is neutral and dry it, place the obtained carboxylated carbon nanotubes in a reactor, add 100mL of dichlorothionyl and 5mL of N,N-dimethylformamide, ultrasonically disperse for 1h, then place it at 80°C for reflux reaction for 24h, and after the reaction is completed, rotary evaporate and dry it to prepare acyl chloride carbon nanotubes;
[0030] C. Take 2.5g of acyl chloride carbon nanotubes and 1.2g of macromolecular antioxidant in a reactor, add 200mL of N,N-dimethylformamide and 0.15mL of pyridine, and react at 85°C in a nitrogen atmosphere for 24h. After the reaction is completed, filter, wash and dry to prepare modified carbon nanotubes.
[0031] Example 2 A method for preparing core-shell particles comprises the following steps:
[0032] (1) 2 g of nano-alumina, 25 mL of ethanol and 25 mL of deionized water were placed in a reactor, ammonia water was added to adjust the pH value of the system to 11, ultrasonic dispersion was uniformly performed, and the mixture was placed in a 30°C water bath and heated at a constant temperature for 1 h. 10 mL of tetraethyl silicate was dissolved in a mixed solution of 20 mL of ethanol and 5 mL of deionized water, mixed uniformly, and allowed to stand for 30 min. The mixture was added to the reactor and the reaction was continued for 24 h. After the reaction was completed, the mixture was centrifuged, washed, and dried to obtain silica-coated nano-alumina.
[0033] (2) 5 g of silica-coated nano-alumina was ultrasonically dispersed in 120 mL of anhydrous ethanol, 1.2 g of 3-aminopropyltriethoxysilane and 7 mL of deionized water were added, stirred and mixed, and reacted at 70° C. for 6 h. After the reaction was completed, the modified silica-coated nano-alumina was prepared by centrifugation, washing and drying;
[0034] (3) 1.25 g of maleic anhydride grafted SEBS was dissolved in 35 mL of cyclohexane, 2.7 g of modified silica-coated nano-alumina and 0.12 g of N,N'-dicyclohexylcarbodiimide were added and ultrasonically dispersed uniformly, and the mixture was placed at 85°C for condensation and reflux for 24 h to obtain an oil phase solution, 11.2 g of Tween 80 and 2.8 g of Span 80 were dissolved in 350 mL of deionized water to obtain an aqueous phase solution, and the oil phase solution was slowly added dropwise to the aqueous phase solution at 3200 rpm, and then the homogenizer was increased to 9000 rpm for emulsification for 3 min, and finally the mixture was placed in a 45°C water bath for rotary evaporation to remove the solvent, and core-shell particles were prepared after centrifugation, washing, and drying.
[0035] Example 3 An insulating wire material resistant to high temperature aging cracking comprises the following raw materials in parts by weight: 62 parts of polyvinyl chloride, 5 parts of modified carbon nanotubes prepared in Example 1, 2 parts of core-shell particles prepared in Example 2, 1 part of plasticizer dioctyl adipate, 0.1 part of lubricant polyethylene wax, and 1 part of calcium zinc stabilizer.
[0036] The preparation method of the above-mentioned insulating wire material is specifically as follows: pour weight parts of polyvinyl chloride, modified carbon nanotubes, plasticizer, lubricant, and stabilizer into a mixer, stir and mix, pour the core-shell particles into the mixer, continue stirring and mixing for 2 hours, discharge the material, and prepare the insulating wire material.
[0037] Example 4 An insulating wire material resistant to high temperature aging cracking comprises the following raw materials in parts by weight: 66 parts of polyvinyl chloride, 7 parts of modified carbon nanotubes prepared in Example 1, 4 parts of core-shell particles prepared in Example 2, 2 parts of plasticizer dioctyl adipate, 0.3 parts of lubricant oxidized polyethylene wax, and 2 parts of calcium zinc stabilizer.
[0038] The preparation method of the above insulating wire material is the same as that of Example 3.
[0039] Example 5 An insulating wire material resistant to high temperature aging cracking comprises the following raw materials in parts by weight: 70 parts of polyvinyl chloride, 10 parts of modified carbon nanotubes prepared in Example 1, 5 parts of core-shell particles prepared in Example 2, 2 parts of plasticizer dioctyl adipate, 0.5 parts of lubricant oxidized polyethylene wax, and 3 parts of calcium zinc stabilizer.
[0040] The preparation method of the above insulating wire material is the same as that of Example 3.
[0041] Comparative Example 1 An insulating wire material resistant to high temperature aging cracking comprises the following raw materials in parts by weight: 70 parts of polyvinyl chloride, 10 parts of carbon nanotubes, 5 parts of core-shell particles prepared in Example 2, 2 parts of plasticizer dioctyl adipate, 0.5 parts of lubricant oxidized polyethylene wax, and 3 parts of calcium zinc stabilizer.
[0042] The preparation method of the above insulating wire material is the same as that of Example 3.
[0043] Comparative Example 2: An insulating wire material resistant to high temperature aging cracking, comprising the following raw materials in parts by weight: 70 parts of polyvinyl chloride, 10 parts of modified carbon nanotubes prepared in Example 1, 5 parts of maleic anhydride grafted SEBS, 2 parts of plasticizer dioctyl adipate, 0.5 parts of lubricant oxidized polyethylene wax, and 3 parts of calcium zinc stabilizer.
[0044] The preparation method of the above insulating wire material is the same as that of Example 3.
[0045] Comparative Example 3: An insulating wire material resistant to high temperature aging cracking, comprising the following raw materials in parts by weight: 70 parts of polyvinyl chloride, 10 parts of modified carbon nanotubes prepared in Example 1, 4 parts of silica-coated nano-alumina prepared in Example 2, 1 part of maleic anhydride grafted SEBS, 2 parts of plasticizer dioctyl adipate, 0.5 parts of lubricant oxidized polyethylene wax, and 3 parts of calcium zinc stabilizer.
[0046] The preparation method of the above insulating wire material is the same as that of Example 3.
[0047] Performance Testing
[0048] (1) Mechanical property testing: The insulating wire materials prepared in Examples 3-5 and Comparative Examples 1-3 were subjected to a tensile property test using a universal mechanical testing machine in accordance with GB / T 1040.2-2022, an impact strength test in accordance with GB / T 1043.1-2008, and a bending strength test in accordance with GB / T 9341-2008. The data results are shown in Table 1.
[0049] Table 1 Test results of mechanical properties of samples
[0050]
[0051] From the data in Table 1, it can be seen that the insulating wire materials prepared in Examples 3-5 of the present invention have excellent flexibility and impact resistance and are not easy to break. In Comparative Example 1, the carbon nanotubes were not modified, in Comparative Example 2, the core-shell particles were replaced with maleic anhydride grafted SEBS, and in Comparative Example 3, the silica-coated nano-alumina and maleic anhydride grafted SEBS were not grafted. The mechanical properties of Comparative Examples 1-3 were measured to be lower than those of Examples 3-5.
[0052] (2) Aging resistance test: The insulating wire materials prepared in Examples 3-5 and Comparative Examples 1-3 were placed in a HJ881 air thermal aging test chamber for high-temperature thermal oxidation aging at 100°C. The aging cycle was divided into four test cycles of 3, 6, 12, and 24 days. Five samples were taken in each cycle, and each sample was subjected to an oxidation induction time test. The data results are shown in Table 2.
[0053] Table 2 Test results of aging resistance of samples
[0054]
[0055] From the data in Table 2, it can be seen that the oxidation induction time of the insulating wire materials prepared in Examples 3-5 of the present invention is relatively long, and after 24 days of thermal oxidative aging, the oxidation induction time is still relatively long, so it has good aging resistance. In Comparative Example 1, the carbon nanotubes were not modified, and the oxidation induction time was significantly shortened. The reason is that the carbon nanotubes added in the components are not modified with macromolecular antioxidants on the surface, so the thermal oxidative aging resistance is poor.
[0056] (3) Heat resistance test: The insulating wire materials prepared in Examples 3-5 and Comparative Examples 1-3 were placed in a TGA-103 thermogravimetric analyzer, respectively. Under nitrogen protection, the temperature was increased from room temperature to 800°C at a heating rate of 5°C / min. The initial decomposition temperature of the material was recorded and its heat resistance was evaluated. Generally speaking, the higher the initial decomposition temperature, the stronger the heat resistance, and vice versa. The data results are shown in Table 3.
[0057] Table 3 Test results of heat resistance of samples
[0058]
[0059] From the data in Table 3, it can be seen that the insulating wire materials prepared in Examples 3-5 of the present invention have a high initial decomposition temperature and good heat resistance. In Comparative Example 2, the nano-alumina coated with ungrafted modified silica has a significantly lower heat resistance than that of Examples 3-5.
[0060] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0061] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. An insulating wire material resistant to high temperature aging cracking, characterized in that: The method comprises the following raw materials in parts by weight: 60 to 70 parts of polyvinyl chloride, 5 to 10 parts of modified carbon nanotubes, 2 to 5 parts of core-shell particles, 1 to 2 parts of plasticizer, 0.1 to 0.5 parts of lubricant, and 1 to 3 parts of stabilizer; The modified carbon nanotubes are prepared by introducing a macromolecular antioxidant into the carbon nanotube structure by chemical reaction, wherein the macromolecular antioxidant is prepared by using p-phenylenediamine and glycidyl ether as reaction monomers; the core-shell particles are prepared by using a post-emulsification technology, with a silicon dioxide-coated nano-alumina as a rigid core and a maleic anhydride-grafted SEBS elastomer as a flexible shell.
2. The insulating wire material resistant to high temperature aging cracking according to claim 1, characterized in that: The plasticizer is one or more combinations of dioctyl adipate, dimethyl phthalate, dioctyl phthalate, and diisodecyl phthalate; the stabilizer is a calcium zinc stabilizer; and the lubricant is one of polyethylene wax and oxidized polyethylene wax.
3. The insulating wire material resistant to high temperature aging cracking according to claim 1, characterized in that: The preparation method of the modified carbon nanotubes comprises the following steps: A. Place p-phenylenediamine and glycidyl ether in a reactor, add toluene solvent, stir and mix, heat to 95-110°C after mixing evenly, react for 10-12 hours, cool to room temperature after the reaction is completed, remove the solvent by rotary evaporation, and prepare a macromolecular antioxidant; B. Take carbon nanotubes in a mixed solution of concentrated sulfuric acid and concentrated nitric acid, place at 70-90°C for reaction for 4-6 hours, filter and wash the product until it is neutral and dry it, place the obtained carboxylated carbon nanotubes in a reactor, add thionyl chloride and N,N-dimethylformamide, ultrasonically disperse for 0.5-1 hour, then place at 70-80°C for reflux reaction for 20-24 hours, and after the reaction is completed, rotary evaporate and dry to prepare acyl chloride carbon nanotubes; C. Take the acyl chloride carbon nanotubes and the macromolecular antioxidant in a reactor, add N,N-dimethylformamide and pyridine, and react at 75-90°C in a nitrogen atmosphere for 20-24 hours. After the reaction is completed, filter, wash and dry to prepare modified carbon nanotubes.
4. The insulating wire material resistant to high temperature aging cracking according to claim 3, characterized in that: The molar ratio of p-phenylenediamine to glycidyl ether in step A is 3 to 3.5:
1.
5. The insulating wire material resistant to high temperature aging cracking according to claim 3, characterized in that: In the step C, the mass ratio of the acyl chloride carbon nanotubes to the macromolecular antioxidant is 1-2.5:
1.
6. The insulating wire material resistant to high temperature aging cracking according to claim 1, characterized in that: The method for preparing the core-shell particles comprises the following steps: (1) Nano-alumina, ethanol and deionized water are placed in a reactor, ammonia water is added to adjust the pH value of the system to 11-12, ultrasonically dispersed uniformly, and then placed in a water bath at 25-35° C. and heated at a constant temperature for 0.5-1 h, tetraethyl silicate is dissolved in a mixed solution of ethanol and deionized water, mixed uniformly, and allowed to stand for 15-30 min, and then added to the reactor to continue the reaction for 20-24 h. After the reaction is completed, the solution is centrifuged, washed, and dried to prepare silica-coated nano-alumina; (2) ultrasonically dispersing the silica-coated nano-alumina in anhydrous ethanol, adding 3-aminopropyltriethoxysilane and deionized water, stirring and mixing, placing at 65-75° C. for reaction for 5-6 hours, and after the reaction is completed, centrifuging, washing, and drying to prepare modified silica-coated nano-alumina; (3) Maleic anhydride grafted SEBS was dissolved in cyclohexane, modified silica-coated nano-alumina and N,N'-dicyclohexylcarbodiimide were added and ultrasonically dispersed uniformly, and the mixture was placed at 75-95°C for condensation and reflux for 20-24 hours to obtain an oil phase solution, Tween 80 and Span 80 were dissolved in deionized water to obtain an aqueous phase solution, and the oil phase solution was slowly added dropwise to the aqueous phase solution at 3000-4700 rpm, and then the homogenizer was increased to 9000-9500 rpm for emulsification for 3-5 minutes, and finally the mixture was placed in a water bath at 40-50°C for rotary evaporation to remove the solvent, and core-shell particles were prepared after centrifugation, washing and drying.
7. The insulating wire material resistant to high temperature aging cracking according to claim 6, characterized in that: In the step (2), the mass ratio of maleic anhydride grafted SEBS to modified silica coated nano-alumina is 1:2-10.
8. The insulating wire material resistant to high temperature aging cracking according to claim 6, characterized in that: In the step (2), the mass ratio of Tween 80 to Span 80 is 3.7-4.2:
1.
9. The insulating wire material resistant to high temperature aging cracking according to claim 1, characterized in that: The preparation method of the insulating wire material is specifically as follows: pouring parts by weight of polyvinyl chloride, modified carbon nanotubes, plasticizer, lubricant, and stabilizer into a mixer, stirring and mixing, pouring core-shell particles into the mixer, continuing to stir and mix for 1 to 2 hours, discharging the material, and preparing the insulating wire material.
Citation Information
Cited By
Mute LVT floor and production process
CN119749008A
Silent LVT Flooring and Production Process
CN119749008B
Insulating material composition, insulating material, preparation method of insulating material, insulating material and application of insulating material
CN120775291A
Insulating material compositions, insulating materials and their preparation methods, insulating materials and their applications
CN120775291B
High-temperature-resistant magnesium oxide electrothermal insulating material and preparation method thereof
CN120794576A