PET (polyethylene terephthalate) composite material taking boehmite as flame-retardant enhancer

By using surface-modified boehmite and phosphorus-nitrogen-based flame retardants in PET materials to form a dense carbon layer, the smoke and toxic gas problems of PET materials during combustion are solved, and the flame retardant effect and extreme oxygen index are significantly improved. Reduces the risk of fire accidents.

CN118994859AInactive Publication Date: 2024-11-22ANHUI YISHITONG NEW ENERGY MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411242239.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

PET materials produce a large amount of smoke and toxic gases during combustion, resulting in fire accidents. Traditional halogen-containing flame retardants will also release smoke and hydrogen halide gas during combustion, stimulating the human body and causing secondary disasters.

Method used

Boehmite is used as a flame retardant reinforcer and surface modification treatment is used to improve its dispersion in PET composite materials. Combined with phosphorus and nitrogen flame retardants, Boehmite absorbs heat and produces it when heat decomposed. Al2O3 covers block the combustion rate and form a dense carbon layer to suppress smoke and flame.

Benefits of technology

It significantly improves the flame retardant effect and limit oxygen index of PET composite materials, reduces the production of smoke and toxic gases, enhances the ability to suppress combustion, and avoids the risk of suffocation due to smoke in fire accidents.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a PET composite material taking boehmite as a flame retardant enhancer. A preparation method of the PET composite material comprises the following steps: S1, putting boehmite into a surface modifier solution for surface modification to obtain modified boehmite; and S2, carrying out melt blending on the modified boehmite, a flame-retardant auxiliary agent and PET to obtain the PET composite material. Under the synergistic effect of the boehmite and the flame-retardant additive, the flame-retardant property of PET is enhanced, and the flame-retardant PET has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of flame retardant materials, in particular to a PET composite material using boehmite as a flame retardant reinforcing agent. Background Art

[0002] In recent years, synthetic polymer materials, such as PET, polypropylene (PP), polyamide (PA), etc., have developed rapidly and have been widely used in various fields such as transportation, electronic appliances, daily furniture, interior decoration, food, clothing, housing and transportation. However, since polymer materials are composed of elements such as C, H, O, S, and N, they are flammable in the air, and a large amount of smoke and toxic gases will be generated when burning, which may cause serious fire accidents at the least and may cause death at the worst. The current status of polymer materials forces people to put forward flame retardant requirements for various synthetic materials, especially various decorations and fabrics, such as curtains, wall cloths, carpets, furniture fabrics and bedding, as well as national defense and military industry and various fireproof work clothes, which also require a large amount of flame retardant fabrics. PET, as an important component of polymer materials, is also widely used in the above projects, and PET is a flammable polymer with a limiting oxygen index (LOI) of about 20%, and a large amount of thick smoke will be generated during the combustion process accompanied by molten droplets, so it is also urgent to carry out flame retardant modification of PET.

[0003] The flame retardant method of PET is generally to add flame retardants to the PET matrix for flame retardancy. The traditional flame retardant is a halogen-containing flame retardant, which can make PET obtain good flame retardant effect. However, after adding halogen-containing flame retardants to PET, a large amount of smoke and hydrogen halides will be released during the combustion process, which will irritate the eyes and respiratory system. In addition to causing burns to the human body, it will also cause "secondary disasters". It is reported that most of the people who died in fire accidents caused by PET in the world died of suffocation due to the smoke and toxic gases emitted when PET burned. Because of this, the problem of smoke suppression and harmlessness in PET combustion has received more and more attention and has become an inevitable problem in PET flame retardant research. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a PET composite material using boehmite as a flame retardant reinforcing agent.

[0005] The technical solution of the present invention is achieved in this way:

[0006] The present invention provides a PET composite material using boehmite as a flame retardant reinforcing agent, and the preparation method of the PET composite material is as follows:

[0007] S1: placing boehmite in a surface modifier solution for surface modification to obtain modified boehmite;

[0008] S2: melt-blending the modified boehmite, the flame retardant additive and PET to obtain the PET composite material.

[0009] Boehmite absorbs a large amount of heat during the thermal decomposition process. The water vapor released by the thermal decomposition evaporates and absorbs heat. It also plays a role in diluting the combustible gas produced by the decomposition of the matrix. The generated Al2O3 solid covers the surface of the matrix to block and delay the combustion rate, thereby achieving the effect of flame retardancy and smoke suppression.

[0010] Furthermore, in step S1, the boehmite particle size is 0.5-2 μm.

[0011] Furthermore, the surface modifier in step S1 is a silane coupling agent.

[0012] Furthermore, the silane coupling agent is γ-aminopropyltriethoxysilane.

[0013] Inorganic powders such as boehmite are generally micrometer-sized or even smaller particles. Due to their small particle size, they have a large specific surface area and high surface energy, and are very prone to agglomeration. In addition, inorganic powder materials are polar hydrophilic minerals, while polymer matrices are generally non-polar hydrophobic groups. The two have poor compatibility and are usually difficult to disperse evenly in polymers. Therefore, if inorganic powders are directly filled or overfilled, it will inevitably lead to a decrease in the mechanical properties of the composite material or even severe embrittlement.

[0014] The basic principle of inorganic powder surface modification is to utilize the groups on the powder surface to react with the surface modifier (i.e. coupling agent) to change its surface from hydrophobic to hydrophilic, thereby enhancing the interfacial compatibility between the powder particles and the polymer matrix, making the particles less likely to agglomerate and well dispersed in the polymer matrix.

[0015] The general formula of silane coupling agent is generally expressed as YR-SiX3, where the X group can undergo hydrolysis reaction and generate silanol (Si-OH), X can be halogen, alkoxy, acetoxy, etc., and Y can react with the polymer matrix to improve the compatibility of silane and polymer. The X group is hydrolyzed into Si-OH, and the adjacent Si-OH is dehydrated and condensed into polysiloxane. Si-OH forms hydrogen bonds with OH on the surface of the substrate. The formed hydrogen bonds undergo dehydration reaction during heating to form stable covalent bonds with boehmite. The Y group can react chemically with the polymer matrix or entangle the molecular chain, so that the other end of the silane coupling agent and the polymer matrix undergo physical or chemical action, so that they act more closely together.

[0016] Furthermore, the surface modifier solution solvent in step S1 is an organic solvent.

[0017] Furthermore, the organic solvent is ethanol.

[0018] First, the coupling agent is diluted with a solvent in a certain proportion. The dilution solvent is required not to react with the coupling agent to affect its performance. After pretreatment, the coupling agent can cover the filler well, and then stir and mix with the polymer and other additives. The coupling agent is easy to disperse evenly, and can prevent the coupling agent from having unnecessary side reactions with the polymer and other additives that affect the coupling effect.

[0019] Furthermore, the flame retardant additive in step S2 includes phosphorus-based and nitrogen-based flame retardants.

[0020] Furthermore, the phosphorus-based flame retardant is AlPi.

[0021] Furthermore, the nitrogen-based flame retardant is MPP.

[0022] AlPi can partially evaporate to form methyl diethylphosphinate and enter the gas phase, and further form PO· free radicals under the high temperature of the flame. PO· combines with H· and HO· free radicals in the flame to suppress the flame in the gas phase.

[0023] MPP decomposes under heat to produce polyphosphoric acid, melamine, NH3, N2, CO2, H2O and other substances. Polyphosphoric acid and part of melamine remain in the condensed phase, and the decomposed non-combustible gas is released into the gas phase, which plays a role in diluting the concentration of combustible gas.

[0024] Furthermore, the mass of the boehmite is 1-5wt% of the mass of PET.

[0025] Furthermore, the mass of the surface modifier is 1-3wt% of the mass of the boehmite.

[0026] Furthermore, the mass of the phosphorus-based flame retardant is 200-400wt% of the mass of the modified boehmite.

[0027] Furthermore, the mass of the nitrogen-based flame retardant is 100-300wt% of the mass of the modified boehmite.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] 1. In the gas phase: AlPi can partially evaporate to form methyl diethylphosphinate, which further forms PO· free radicals under the high temperature of the flame. PO· combines with H· and HO· free radicals in the flame to suppress the flame in the gas phase. MPP produces non-combustible substances when heated, which plays a role in diluting the concentration of combustible gas.

[0030] 2. In the condensed phase: the polyphosphoric acid and part of melamine decomposed by MPP, methyl diethylphosphinate produced by AlPi and Al2O3 decomposed by boehmite work together to form a dense and continuous carbon layer on the surface of the matrix, which plays a good barrier role.

[0031] 3. Boehmite absorbs heat when it is decomposed by heat, delaying the decomposition of the system. The Al2O3 produced by the decomposition covers the surface of the substrate, which can play a certain barrier effect. At the same time, it reacts with PET, polyphosphoric acid and melamine in the condensed phase to form carbon. Al2O3 can also be used as a reaction carrier to promote the carbonization reaction, making the reaction more complete and the barrier layer formed more fine and dense. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Reagent Description:

[0034] Boehmite, γ-aminopropyltriethoxysilane, ethanol, AlPi, MPP, analytical grade, Shanghai Aladdin Biochemical Technology Co., Ltd.

[0035] Example 1

[0036] S1: 2 g of γ-aminopropyltriethoxysilane was dissolved in 500 g of ethanol, and after mixing evenly, 100 g of boehmite with a particle size of 0.5 μm was added, and after mixing evenly again, the mixture was dried at 120° C. for 2 h to obtain the modified boehmite.

[0037] S2: 30 g of the modified boehmite, 90 g of AlPi, 60 g of MPP and 1000 g of PET dried at 100° C. for 10 h were added into a twin-screw extruder to prepare the PET composite material.

[0038] Example 2

[0039] The difference between this embodiment and embodiment 1 is that the particle size of the boehmite in step S1 is 1 μm.

[0040] The other parts are exactly the same as those in Example 1.

[0041] Example 3

[0042] The difference between this embodiment and embodiment 1 is that the particle size of the boehmite in step S1 is 2 μm.

[0043] The other parts are exactly the same as those in Example 1.

[0044] Example 4

[0045] The difference between this embodiment and embodiment 1 is that the amount of γ-aminopropyltriethoxysilane added in step S1 is 1 g.

[0046] The other parts are exactly the same as those in Example 1.

[0047] Example 5

[0048] The difference between this embodiment and embodiment 1 is that the amount of γ-aminopropyltriethoxysilane added in step S1 is 3 g.

[0049] The other parts are exactly the same as those in Example 1.

[0050] Example 6

[0051] The difference between this embodiment and embodiment 1 is that in step S2, the amount of modified boehmite added is 10 g, the amount of AlPi added is 30 g, and the amount of MPP added is 20 g.

[0052] The other parts are exactly the same as those in Example 1.

[0053] Example 7

[0054] The difference between this embodiment and embodiment 1 is that in step S2, the amount of modified boehmite added is 50 g, the amount of AlPi added is 150 g, and the amount of MPP added is 100 g.

[0055] The other parts are exactly the same as those in Example 1.

[0056] Example 8

[0057] The difference between this embodiment and embodiment 1 is that the amount of AlPi added in step S2 is 60 g.

[0058] The other parts are exactly the same as those in Example 1.

[0059] Example 9

[0060] The difference between this embodiment and embodiment 1 is that the amount of AlPi added in step S2 is 120 g.

[0061] The other parts are exactly the same as those in Example 1.

[0062] Example 10

[0063] The difference between this embodiment and embodiment 1 is that the amount of MPP added in step S2 is 30 g.

[0064] The other parts are exactly the same as those in Example 1.

[0065] Embodiment 11

[0066] The difference between this embodiment and embodiment 1 is that the amount of MPP added in step S2 is 90 g.

[0067] The other parts are exactly the same as those in Example 1.

[0068] Tests and Results

[0069] Limiting oxygen index (LOI) test: Tested according to GB / T2406-1993, sample size 150mm×8.0mm×4.0mm.

[0070] Vertical burning (UL-94) test: Tested according to UL94-1985, the sample size is 127mm×12.7mm×3.2mm.

[0071] The results are shown in Table 1

[0072] Table 1

[0073] project LOI(%) UL-94 Rating Example 1 34 V0 Example 2 32 V0 Example 3 29 V0 Example 4 27 V1 Example 5 34 V0 Example 6 29 HB Example 7 35 HB Example 8 28 HB Example 9 38 V1 Example 10 32 V1 Embodiment 11 34 V0 PET 24 V2

[0074] It can be seen from Examples 1-3 and PET in Table 1 that boehmite can significantly improve the flame retardant effect and LOI of PET composite materials, and the particle size will affect the LOI.

[0075] It can be seen from Table 1 Examples 1, 4-5 that the flame retardant effect and LOI of the PET composite material increase with the increase in the amount of γ-aminopropyltriethoxysilane. When the amount of γ-aminopropyltriethoxysilane is 2wt% of boehmite, the flame retardant effect and LOI continue to increase with the amount, and the performance improvement is not obvious.

[0076] It can be seen from Examples 1, 6-7 in Table 1 that boehmite can significantly improve the flame retardant effect and LOI of PET composite materials. When the amount of boehmite is further increased, the flame retardant effect deteriorates, indicating that the amount of boehmite added cannot be too much, as excessive addition can easily destroy the synergistic system of AlPi and MPP.

[0077] As shown in Table 1, Examples 1, 8-11, with the increase in the amount of AlPi added, the flame retardant effect of the flame retardant system is getting better and better, and the oxygen index is slightly improved. When the mass ratio of AlPi to MPP is 3:2, the flame retardant effect is the best. When the amount of AlPi is further increased, the flame retardant effect of the flame retardant system begins to deteriorate, and it cannot pass the UL-94 test (3.2mm) V-0 test, and only passes the V-1 level, but the oxygen index is very high. MPP has an effect on the flame retardant effect of PET composite materials, but the influence on the oxygen index is not very large.

[0078] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A PET composite material with boehmite as a flame retardant reinforcing agent, characterized in that: The preparation method of the PET composite material is: S1: placing boehmite in a surface modifier solution for surface modification to obtain modified boehmite; S2: melt-blending the modified boehmite, the flame retardant additive and PET to obtain the PET composite material.

2. The PET composite material with boehmite as a flame retardant reinforcing agent according to claim 1, characterized in that: The boehmite particle size in step S1 is 0.5-2 μm.

3. The PET composite material with boehmite as a flame retardant reinforcing agent according to claim 1, characterized in that: The surface modifier in step S1 is a silane coupling agent.

4. The PET composite material with boehmite as a flame retardant reinforcing agent according to claim 1, characterized in that: The surface modifier solution solvent in step S1 is an organic solvent.

5. The PET composite material with boehmite as a flame retardant reinforcing agent according to claim 1, characterized in that: The flame retardant additive in step S2 includes phosphorus-based and nitrogen-based flame retardants.

6. The PET composite material with boehmite as a flame retardant reinforcing agent according to claim 1, characterized in that: The mass of the boehmite is 1-5 wt % of the mass of PET.

7. The PET composite material with boehmite as a flame retardant reinforcing agent according to claim 1, characterized in that: The mass of the surface modifier is 1-3 wt % of the mass of the boehmite.

8. A PET composite material with boehmite as a flame retardant reinforcing agent according to claim 1 or 5, characterized in that: The mass of the phosphorus-based flame retardant is 200-400wt% of the mass of the modified boehmite.

9. A PET composite material with boehmite as a flame retardant reinforcing agent according to claim 1 or 5, characterized in that: The mass of the nitrogen-based flame retardant is 100-300 wt % of the mass of the modified boehmite.

Citation Information

Patent Citations

  • PET material and preparation method thereof

    CN115678216A