Wear-resistant antibacterial easy-to-clean wood floor film and preparation method thereof

By using wooden floor films with silver-clad copper powder, cobalt powder and other components, the wear, invasion and deformation problems of solid wood floors are solved, and the wear resistance, antibacterial mite removal and oil stain removal effects are achieved, which improves the service life and health of the floor. Security.

CN118994883APending Publication Date: 2024-11-22湖南壹鑫科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411206024.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Solid wood floors are prone to wear and tear during use, and are attacked by borers and bacterial mites. When cleaning, water will cause the floor to deform, and the coating on the market produces harmful substances that are harmful to health.

Method used

Use silver-clad copper powder, cobalt powder, crown ether chelated copper sulfate, polyurethane adhesive, graphite chimeric sodium tetraborate, nano-titanium dioxide super hydrophilic self-cleaning coating, rosemary-witch hazel extract and polyester modification A wooden floor film with components such as dimethylpolysiloxane is prepared by ultrasonic stirring and mechanical stirring to form a film that is wear-resistant, antibacterial and easy to clean.

Benefits of technology

It realizes the wear resistance and antibacterial mite removal effect of the floor, easily and effectively removes oil and stains, and increases the fresh odor, which improves the service life and health and safety of the floor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994883A_ABST
    Figure CN118994883A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wood floor film preparation, and particularly discloses a wear-resistant antibacterial easy-to-clean wood floor film and a preparation method thereof. The wear-resistant antibacterial easy-to-clean wood floor film is prepared from the following components in parts by weight: 2-4 parts of silver-coated copper powder, 1-3 parts of cobalt powder, 1-2 parts of crown ether chelated copper sulfate, 60-80 parts of a polyurethane adhesive, 4-6 parts of graphite chimeric sodium tetraborate, 2-4 parts of floral water, 5-10 parts of a nano titanium dioxide type super-hydrophilic self-cleaning coating, 3-5 parts of a rosemary-witch hazel extract and 12-15 parts of an oil-resistant agent. The wear-resistant antibacterial easy-to-clean wood floor film is high in stability, wear-resistant, antibacterial, capable of preventing insect pests, easy to clean and capable of effectively prolonging the service life of a solid wood floor, the prepared wear-resistant antibacterial easy-to-clean wood floor film is high in environmental protection property and simple in preparation process, cost is saved, labor intensity is reduced, and the wear-resistant antibacterial easy-to-clean wood floor film is worthy of popularization and application. The actual use requirement is met, the equipment requirement is low, the operability is high, and good social popularization and application are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid wood flooring, and more specifically discloses a wear-resistant, antibacterial and easy-to-clean wood flooring film and a preparation method thereof. Background Art

[0002] Solid wood flooring is a floor decoration material formed by drying and processing natural wood. Also known as log wood flooring, it is a floor directly processed from solid wood. It has the natural texture of wood, can keep warm in winter and cool in summer, is comfortable to the feet and safe to use.

[0003] However, in actual use, with the widespread application of solid wood floors in indoor homes and public places, solid wood floors are in contact with the ground for a long time, are easily worn, and are attacked by termites, bacteria and mites. In addition, the floor will be deformed when it comes into contact with water during cleaning, which seriously affects the service life of the solid wood floors. The coating tools on the market will produce a large amount of harmful substances during production, which will seriously endanger people's health and safety. Summary of the invention

[0004] The present invention mainly provides a wear-resistant, antibacterial and easy-to-clean wooden floor film and a preparation method thereof, aiming to solve the above-mentioned problems of easy wear, attack by termites and bacteria mites, and deformation of the floor when exposed to water during cleaning.

[0005] The present invention provides a wear-resistant, antibacterial and easy-to-clean wooden floor film, comprising the following components in parts by weight: 2-4 parts of silver-coated copper powder, 1-3 parts of cobalt powder, 1-2 parts of crown ether chelated copper sulfate, 60-80 parts of polyurethane adhesive, 4-6 parts of graphite-embedded sodium tetraborate, 2-4 parts of floral water, 5-10 parts of nano-titanium dioxide type super hydrophilic self-cleaning coating, 3-5 parts of rosemary-witch hazel extract, and 12-15 parts of oil-resistant agent.

[0006] Preferably, the silver-coated copper powder is a silver-coated copper powder with a particle size of 5-8 μm; The cobalt powder is 500 mesh ultrafine cobalt powder; The crown ether chelated copper sulfate is a chelate of 18-crown ether-6 and anhydrous copper sulfate, 18-crown ether-6: anhydrous copper sulfate (W / W) = 1 / 2, and the preparation method is to heat anhydrous copper sulfate powder and dissolve it in 50°C 20 times weight ratio methanol, add 18-crown ether-6 and stir for 20 minutes, evaporate the methanol under reduced pressure at 40°C, and grind the obtained solid in a grinder to obtain crown ether chelated copper sulfate; The polyurethane adhesive is a commercially available polyurethane adhesive; The graphite-embedded sodium tetraborate is an intercalation of 2000 mesh ultrafine graphite and sodium tetraborate, with graphite: sodium tetraborate (W / W) = 1 / 1. The preparation method is to dissolve sodium tetraborate in 60°C hot water with a weight ratio of 10 times, add 2000 mesh ultrafine graphite and stir for 10 minutes, reduce pressure at 60°C to concentrate to obtain a solid, grind and crush, and obtain graphite-embedded sodium tetraborate; The floral water is commercially available floral water; The nano-titanium dioxide type super-hydrophilic self-cleaning coating is a commercially available nano-titanium dioxide type super-hydrophilic self-cleaning coating; The rosemary-witch hazel extract is an ethanol extract concentrate of rosemary-witch hazel powder, and the preparation method comprises the following steps: crushing rosemary and witch hazel, adding them to ethanol in a weight ratio of 10 times, heating at 60° C., stirring and extracting for 2 hours, filtering, and concentrating the filtrate under reduced pressure at 45° C. to obtain the rosemary-witch hazel extract; The oil-resistant agent is polyester-modified dimethyl polysiloxane.

[0007] The present invention also provides a method for preparing a wear-resistant, antibacterial and easy-to-clean wooden floor film, comprising the following steps: S1, crown ether chelated copper sulfate powder and graphite intercalated sodium tetraborate powder are mixed uniformly with ultrasonic stirring under argon protection to obtain powder 1; S2, adding floral water, nano titanium dioxide type super hydrophilic self-cleaning coating, rosemary-witch hazel extract, and polyester-modified dimethyl polysiloxane to the polyurethane adhesive in sequence, and mixing them evenly to obtain a mixed adhesive 1; S3, adding the powder 1, silver-coated copper powder and cobalt powder obtained in step S1 to the mixed adhesive 1 obtained in step S2, and mixing them evenly.

[0008] Preferably, in step S1, the ultrasonic stirring mixing time is 10 min, the mixing stirring temperature is room temperature, and the ultrasonic frequency is 40 KHz.

[0009] Preferably, in step S2, the mixing method is mechanical stirring, and the mixing time is 1 min.

[0010] Preferably, in step S3, the mixing method is mechanical stirring, and the mixing time is 2 minutes.

[0011] The present invention has the following beneficial effects: (1) The silver-coated copper powder, cobalt powder and crown ether chelated copper sulfate used in the present invention all have bactericidal and disinfecting effects. The cobalt powder also has the effect of purifying dust in the room, and the crown ether chelated copper sulfate also has the effect of slow-release insecticide. (2) The polyester-modified dimethylpolysiloxane and nano-titanium dioxide-based super-hydrophilic self-cleaning coating added in the present invention also have the function of oil resistance, which can effectively remove oily components; (3) The rosemary-witch hazel extract added in the present invention has a killing effect on mites that are ubiquitous in life, can effectively inhibit mites, and has a bactericidal effect, and has a certain health care effect on human skin; (4) The floral water added in the present invention can not only repel insects and mosquitoes, but also increase the fresh smell of the floor; (5) The graphite-embedded sodium tetraborate added in the present invention has the property of wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] The present invention is further described in detail below with reference to the accompanying drawings and specific implementation methods.

[0013] Figure 1 The figure is a schematic diagram of the chemical structure of crown ether chelated copper sulfate of the present invention. DETAILED DESCRIPTION

[0014] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.

[0015] Embodiment 1: The components of the wear-resistant, antibacterial and easy-to-clean wood floor film and the weight proportions of each component are: 2 parts of silver-coated copper powder 1 part ultrafine cobalt powder 1 part crown ether chelated copper sulfate Polyurethane adhesive 60 parts Graphite intercalated sodium tetraborate 4 parts 2 parts of floral water Nano titanium dioxide super hydrophilic self-cleaning coating 5 parts Rosemary-Witch Hazel Extract 3 parts Polyester modified dimethyl polysiloxane 12 parts: (1) 10 g of crown ether chelated copper sulfate powder and 40 g of graphite intercalated sodium tetraborate powder were added to a reaction bottle, and the mixture was stirred and mixed at room temperature for 10 min at 40 kHz ultrasonic wave under argon protection to obtain powder 1; (2) 20 g of floral water, 50 g of nano titanium dioxide super hydrophilic self-cleaning coating, 30 g of rosemary-witch hazel extract, and 120 g of polyester-modified dimethyl polysiloxane were sequentially added to 600 g of polyurethane adhesive, and mechanically stirred and mixed for 1 min to obtain a mixed adhesive 1; (3) Add the powder 1 obtained in step S1, 20 g of silver-coated copper powder and 10 g of ultrafine cobalt powder to the mixed adhesive 1 obtained in step S2, and stir mechanically for 2 min to obtain the obtained product.

[0016] Embodiment 2: The components of the wear-resistant, antibacterial and easy-to-clean wood floor film and the weight proportions of each component are: 3 parts of silver-coated copper powder 2 parts of ultrafine cobalt powder 1.5 parts crown ether chelated copper sulfate Polyurethane adhesive 70 parts Graphite intercalated sodium tetraborate 5 parts 3 parts of floral water 7.5 parts of nano titanium dioxide super hydrophilic self-cleaning coating Rosemary-Witch Hazel Extract 4 parts Polyester modified dimethyl polysiloxane 13.5 parts: (1) 15 g of crown ether chelated copper sulfate powder and 50 g of graphite intercalated sodium tetraborate powder were added to a reaction bottle, and the mixture was stirred and mixed at room temperature for 10 min at 40 kHz ultrasonic wave under argon protection to obtain powder 1; (2) 30 g of floral water, 75 g of nano titanium dioxide super hydrophilic self-cleaning coating, 40 g of rosemary-witch hazel extract, and 135 g of polyester-modified dimethyl polysiloxane were sequentially added to 700 g of polyurethane adhesive, and mechanically stirred for 1 min to obtain a mixed adhesive 1; (3) Add the powder 1 obtained in step S1, 30 g of silver-coated copper powder and 20 g of ultrafine cobalt powder to the mixed adhesive 1 obtained in step S2, and mix them by mechanical stirring for 2 min.

[0017] Embodiment three: The components of the wear-resistant, antibacterial and easy-to-clean wood floor film and the weight proportions of each component are: Silver-coated copper powder 4 parts 3 parts of ultrafine cobalt powder 2 parts crown ether chelated copper sulfate Polyurethane adhesive 80 parts Graphite intercalated sodium tetraborate 5 parts 4 parts of floral water Nano titanium dioxide super hydrophilic self-cleaning coating 10 parts Rosemary-Witch Hazel Extract 5 parts 15 parts of polyester modified dimethyl polysiloxane: (1) 20 g of crown ether chelated copper sulfate powder and 60 g of graphite intercalated sodium tetraborate powder were added to a reaction bottle, and the mixture was stirred and mixed at room temperature for 10 min at 40 kHz ultrasonic wave under argon protection to obtain powder 1; (2) 40 g of floral water, 100 g of nano titanium dioxide type super hydrophilic self-cleaning coating, 50 g of rosemary-witch hazel extract, and 150 g of polyester-modified dimethyl polysiloxane were sequentially added to 800 g of polyurethane adhesive, and mechanically stirred and mixed for 1 min to obtain a mixed adhesive 1; (3) Add the powder 1 obtained in step S1, 40 g of silver-coated copper powder and 30 g of ultrafine cobalt powder to the mixed adhesive 1 obtained in step S2, and stir mechanically for 2 min to obtain the obtained product.

[0018] Embodiment 4: The components of the wear-resistant, antibacterial and easy-to-clean wood floor film and the weight proportions of each component are: 2 parts of silver-coated copper powder 1 part ultrafine cobalt powder 1 part crown ether chelated copper sulfate Polyurethane adhesive 80 parts Graphite intercalated sodium tetraborate 4 parts 2 parts of floral water 5 parts of nano titanium dioxide super hydrophilic self-cleaning coating Rosemary-Witch Hazel Extract 3 parts 12 parts of polyester modified dimethyl polysiloxane (1) 10 g of crown ether chelated copper sulfate powder and 40 g of graphite intercalated sodium tetraborate powder were added to a reaction bottle, and the mixture was stirred and mixed at room temperature for 10 min at 40 kHz ultrasonic wave under argon protection to obtain powder 1; (2) 20 g of floral water, 50 g of nano titanium dioxide super hydrophilic self-cleaning coating, 30 g of rosemary-witch hazel extract, and 120 g of polyester-modified dimethyl polysiloxane were sequentially added to 800 g of polyurethane adhesive, and mechanically stirred and mixed for 1 min to obtain a mixed adhesive 1; (3) Add the powder 1 obtained in step S1, 20 g of silver-coated copper powder and 10 g of ultrafine cobalt powder to the mixed adhesive 1 obtained in step S2, and mix them mechanically for 2 min.

[0019] Embodiment five: The components of the wear-resistant, antibacterial and easy-to-clean wood floor film and the weight proportions of each component are: Silver-coated copper powder 4 parts 3 parts of ultrafine cobalt powder 2 parts crown ether chelated copper sulfate Polyurethane adhesive 60 parts Graphite intercalated sodium tetraborate 5 parts 4 parts of floral water Nano titanium dioxide super hydrophilic self-cleaning coating 10 parts Rosemary-Witch Hazel Extract 5 parts 15 parts of polyester modified dimethyl polysiloxane (1) 20 g of crown ether chelated copper sulfate powder and 60 g of graphite intercalated sodium tetraborate powder were added to a reaction bottle, and the mixture was stirred and mixed at room temperature for 10 min at 40 kHz ultrasonic wave under argon protection to obtain powder 1; (2) 40 g of floral water, 100 g of nano titanium dioxide super hydrophilic self-cleaning coating, 50 g of rosemary-witch hazel extract, and 150 g of polyester-modified dimethyl polysiloxane were sequentially added to 600 g of polyurethane adhesive, and mechanically stirred and mixed for 1 min to obtain a mixed adhesive 1; (3) Add the powder 1 obtained in step S1, 40 g of silver-coated copper powder and 30 g of ultrafine cobalt powder to the mixed adhesive 1 obtained in step S2, and stir mechanically for 2 min to obtain the obtained product.

[0020] Comparative Example 1 Same as Example 1, except that graphite-embedded sodium tetraborate is not added.

[0021] Comparative Example 2 The same as Example 1, except that no silver-coated copper powder, crown ether chelated copper sulfate and cobalt powder are added.

[0022] Comparative Example 3 Same as Example 1, except that polyester-modified dimethyl polysiloxane is not added.

[0023] Comparative Example 4 Same as Example 1, except that the rosemary-witch hazel extract is not added.

[0024] Comparative Example 5 The same as Example 1, except that the nano titanium dioxide type super hydrophilic self-cleaning coating is not added.

[0025] Specific data comparing the wear-resistant, antibacterial and easy-to-clean wood floor films prepared in the examples and comparative examples are shown in Table 1.

[0026] Table 1 Test results of wear-resistant, antibacterial and easy-to-clean wooden floor films of the embodiments and comparative examples Friction weight loss / mg Surface colonies Number of mites per unit area Degreasing effect Embodiment 1 44 nd 18 completely Embodiment 2 43 nd 18 completely Embodiment 3 42 nd 16 completely Embodiment 4 48 nd 20 completely Embodiment 5 40 nd 16 completely Comparative Example 1 155 nd 18 completely Comparative Example 2 49 8 19 completely Comparative Example 3 55 nd 18 A little oil stain Comparative Example 4 46 nd 66 completely Comparative Example 5 45 nd 19 A little oil stain Note: nd means not detected.

[0027] As shown in Table 1, the wear-resistant, antibacterial and easy-to-clean wooden floor film can have excellent wear resistance, easy oil removal performance and antibacterial and mite removal effects through the cooperation of various components.

[0028] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by ordinary technicians in this technical field within the essential scope of the present invention also fall within the protection scope of the present invention.

Claims

1. A wear-resistant, antibacterial and easy-to-clean wooden floor film. It is characterized in that It comprises the following components by weight: 2-4 parts of silver-coated copper powder, 1-3 parts of cobalt powder, 1-2 parts of crown ether chelated copper sulfate, 60-80 parts of polyurethane adhesive, 4-6 parts of graphite-embedded sodium tetraborate, 2-4 parts of floral water, 5-10 parts of nano-titanium dioxide type super hydrophilic self-cleaning coating, 3-5 parts of rosemary-witch hazel extract, and 12-15 parts of oil-resistant agent.

2. The wear-resistant, antibacterial and easy-to-clean wooden floor film according to claim 1, It is characterized in that The silver-coated copper powder has a particle size of 5-8 μm; The cobalt powder is 500 mesh ultrafine cobalt powder; The crown ether chelated copper sulfate is a chelate of 18-crown ether-6 and anhydrous copper sulfate, 18-crown ether-6: anhydrous copper sulfate (W / W) = 1 / 2, and the preparation method is to heat anhydrous copper sulfate powder and dissolve it in 50°C 20 times weight ratio methanol, add 18-crown ether-6 and stir for 20 minutes, evaporate the methanol under reduced pressure at 40°C, and grind the obtained solid in a grinder to obtain crown ether chelated copper sulfate; The polyurethane adhesive is a commercially available polyurethane adhesive; The graphite-embedded sodium tetraborate is an intercalation of 2000 mesh ultrafine graphite and sodium tetraborate, with graphite: sodium tetraborate (W / W) = 1 / 1. The preparation method is to dissolve sodium tetraborate in 60°C hot water with a weight ratio of 10 times, add 2000 mesh ultrafine graphite and stir for 10 minutes, reduce pressure at 60°C to concentrate to obtain a solid, grind and crush, and obtain graphite-embedded sodium tetraborate; The floral water is commercially available floral water; The nano-titanium dioxide type super-hydrophilic self-cleaning coating is a commercially available nano-titanium dioxide type super-hydrophilic self-cleaning coating; The rosemary-witch hazel extract is an ethanol extract concentrate of rosemary-witch hazel powder, and the preparation method comprises the following steps: crushing rosemary and witch hazel, adding them to ethanol in a weight ratio of 10 times, heating at 60° C., stirring and extracting for 2 hours, filtering, and concentrating the filtrate under reduced pressure at 45° C. to obtain the rosemary-witch hazel extract; The oil-resistant agent is polyester-modified dimethyl polysiloxane.

3. A method for preparing the wear-resistant, antibacterial and easy-to-clean wooden floor film according to any one of claims 1 to 2, It is characterized in that The steps include: S1, crown ether chelated copper sulfate powder and graphite intercalated sodium tetraborate powder were mixed uniformly under ultrasonic stirring under argon protection to obtain powder 1; S2, adding floral water, nano titanium dioxide type super hydrophilic self-cleaning coating, rosemary-witch hazel extract, and polyester-modified dimethyl polysiloxane to the polyurethane adhesive in sequence, and mixing them evenly to obtain a mixed adhesive 1; S3, adding the powder 1, silver-coated copper powder and cobalt powder obtained in step S1 to the mixed adhesive 1 obtained in step S2, and mixing them evenly.

4. The method for preparing the wear-resistant, antibacterial and easy-to-clean wooden floor film according to claim 3, It is characterized in that In the step S1, the ultrasonic stirring mixing time is 10 minutes, the mixing stirring temperature is room temperature, and the ultrasonic frequency is 40 KHz.

5. The method for preparing the wear-resistant, antibacterial and easy-to-clean wooden floor film according to claim 3, It is characterized in that In step S2, the mixing method is mechanical stirring, and the mixing time is 1 min.

6. The method for preparing the wear-resistant, antibacterial and easy-to-clean wooden floor film according to claim 3, It is characterized in that In step S3, the mixing method is mechanical stirring, and the mixing time is 2 minutes.