Expanded double-sided adhesive tape as well as preparation method and application thereof
By using a combined design of inorganic expansion coating and pressure-sensitive adhesive layer in the expansion double-sided adhesive tape, the problems of poor expansion effect and poor flame retardant insulation performance during combustion are solved, and the expansion reaction at high temperature is achieved Taking into account both the adhesive properties, an effective fire-proof and heat-insulating layer is formed.
Patent Information
- Application Number
- CN202411340353.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-22
AI Technical Summary
The existing flame-retardant double-sided adhesive tape has poor expansion effect when burned, and has poor flame-retardant and thermal insulation performance, and cannot guarantee good bonding and flame-retardant performance at the same time.
Design of expanded double-sided adhesive tape including release paper layer, pressure-sensitive adhesive layer and inorganic expansion coating. By adding phosphate, oxalate, borate and other components to the inorganic expansion coating, high-temperature foaming is formed. The agent and binder are sandwiched between the pressure-sensitive adhesive layer to ensure adhesion and flame retardancy, and catalyzed expansion reaction at high temperatures.
The expansion reaction at high temperature is achieved, forming a fire-resistant and heat-resistant insulation layer that is resistant to high temperature and low heat conduction, preventing the flame from expanding and spreading, while maintaining good bonding performance, solving the problem of contradiction between adhesion and flame retardancy.
Smart Images

Figure CN118995072A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of double-sided adhesive tapes, and in particular to an expanded double-sided adhesive tape and a preparation method and application thereof. Background Art
[0002] Flame retardant double-sided tape, as a tape with special functions, has become an indispensable product in modern society. It can be used in many industries such as automobiles, home appliances, electronics industry, new energy batteries, energy storage, fire-fighting equipment, etc., and occupies an important position in the tape industry.
[0003] Flame retardant double-sided tape is usually made by coating flame retardant glue on both sides of the tape. Its flame retardant performance is closely related to the formula of the flame retardant glue, and the fire rating can meet UL94-V0, etc. Existing flame retardant glue usually adds flame retardant to the binder (such as acrylic resin) to improve the flame retardant performance. However, the addition of flame retardant often leads to a decrease in the binder content, thereby reducing the bonding performance of the double-sided tape and failing to bond the fixed object well.
[0004] In addition, the existing flame-retardant double-sided adhesive tape can only prevent itself from burning when heated, but cannot suppress the spread of flames and combustion. When encountering open flames or high temperatures, it has poor expansion effect, poor flame-retardant and heat-insulating properties, and may even shrink and eventually burn to ashes. Summary of the invention
[0005] In response to the problems raised by the background technology, the first purpose of the present invention is to propose an expandable double-sided adhesive tape, which has good adhesion and flame retardancy, plays the role of isolating the spread of flame and heat insulation, meets the needs of fire prevention and heat insulation, and solves the technical problems that the existing flame retardant double-sided adhesive tape has poor expansion effect, poor flame retardant and heat insulation performance, and cannot simultaneously ensure good bonding performance and flame retardant performance.
[0006] The second object of the present invention is to provide a method for preparing the above-mentioned expandable double-sided adhesive tape, which has a simple and easy-to-control process and low cost, and the prepared expandable double-sided adhesive tape has good adhesion and flame retardancy.
[0007] The third object of the present invention is to propose the application of any of the above-mentioned expandable double-sided adhesive tapes in the fields of electronics, transportation and construction.
[0008] To achieve the above-mentioned purpose, the present invention provides an expandable double-sided adhesive tape, comprising a release paper layer, a pressure-sensitive adhesive layer and an inorganic expandable coating; the pressure-sensitive adhesive layer is provided on the upper and lower surfaces of the inorganic expandable coating respectively, and the release paper layer is provided on the surface of the pressure-sensitive adhesive layer away from the inorganic expandable coating; the inorganic expandable coating comprises the following components in parts by weight: 100 parts of water, 40-80 parts of phosphate, 1-20 parts of oxalate, 10-30 parts of carbonate, 1-5 parts of borate, 1-5 parts of magnesium oxide, 1-20 parts of boehmite, 0.5-5 parts of dispersant and 10-20 parts of binder.
[0009] Optionally, the adhesive is acrylic emulsion, and the pressure-sensitive adhesive layer is polyacrylate pressure-sensitive adhesive.
[0010] Optionally, the inorganic expansion coating has a thickness of 0.1 mm to 0.5 mm.
[0011] Optionally, the pressure-sensitive adhesive layer is formed by compounding a substrate layer and two adhesive layers, and the two adhesive layers are respectively coated on the upper and lower surfaces of the substrate layer.
[0012] Optionally, the material of the substrate layer is any one of cotton paper, non-woven fabric, PET film, polyimide film, polycarbonate film or polyvinyl chloride film.
[0013] Optionally, both the phosphate and the borate are ammonium salts.
[0014] Optionally, the carbonate is an ammonium salt, and the oxalate is an ammonium salt or a compound formed by oxalic acid and an organic amine.
[0015] Optionally, the dispersant is any one of sodium tripolyphosphate, sodium tartrate or polyethylene glycol.
[0016] The present invention also provides a method for preparing an expandable double-sided adhesive tape, which is used to prepare any of the above-mentioned expandable double-sided adhesive tapes, comprising the following steps:
[0017] Step S1, preparing an inorganic intumescent coating according to the component dosage of the inorganic intumescent coating: adding the phosphate, the oxalate, the carbonate and the borate into water, stirring and dissolving, and preparing slurry A; adding the boehmite and the magnesium oxide into the slurry A, stirring and dispersing, and then respectively adding the dispersant and the binder, mixing evenly, to obtain the inorganic intumescent coating;
[0018] Step S2, coating and drying of a carrier substrate: using a release paper roll with a pressure-sensitive adhesive as the carrier substrate, uniformly coating the inorganic expansion coating prepared in step S1 on the surface of the pressure-sensitive adhesive, and after drying in an oven to remove moisture, the inorganic expansion coating forms the inorganic expansion coating on the surface of the pressure-sensitive adhesive to prepare an intermediate adhesive tape;
[0019] Step S3, laminating the intermediate tape: using another roll of release paper with a pressure-sensitive adhesive as a laminating material, laminating it on the surface of the inorganic expandable coating of the intermediate tape to obtain the expandable flame-retardant double-sided adhesive tape.
[0020] The present invention also proposes the use of any one of the above-mentioned expandable double-sided adhesive tapes in the fields of electronic appliances, transportation and construction.
[0021] Compared with the prior art, the embodiments of the present invention have the following beneficial effects:
[0022] 1. The intumescent flame-retardant double-sided adhesive tape provided by the present invention has good adhesion and flame retardancy, and solves the problem of the contradiction between the adhesion and flame retardancy of the existing flame-retardant double-sided adhesive tape: by sandwiching the inorganic intumescent coating between the two layers of the pressure-sensitive adhesive layer, after the release paper layer is torn off, the contact surface between the intumescent double-sided adhesive tape and the adhered object is still the pressure-sensitive adhesive layer, and the pressure-sensitive adhesive layer can provide good adhesion to the adherend, so that the intumescent double-sided adhesive tape can maintain good adhesion performance and will not cause the adhesion to decrease due to the addition of flame retardants; when encountering combustion, the intumescent flame-retardant double-sided adhesive tape will undergo a foaming reaction at high temperature; not only will it not burn itself, but its volume will expand to a large extent, and a high-temperature resistant, low-thermal conductive fireproof and heat-insulating layer will be formed, which has the effect of preventing the expansion and spread of flames.
[0023] 2. By adding the binder into the inorganic expandable coating, the binder penetrates and diffuses between the pressure-sensitive adhesive layers, thereby forming a good bonding force between the inorganic expandable coating and the pressure-sensitive adhesive layer, preventing the inorganic expandable coating from falling off the pressure-sensitive adhesive layer, and further ensuring the bonding and flame retardancy of the expandable double-sided adhesive tape.
[0024] 3. By adding a higher content of the phosphate, the expansion reaction of the inorganic expansion coating can be catalyzed at high temperature, the expansion ratio can be increased, and a high-temperature adhesive can be formed with the borate to maintain the structural stability of the inorganic expansion coating during the high-temperature expansion process, preventing the expansion layer from rupturing or falling off prematurely, thereby preventing the transfer of flames and heat.
[0025] 4. By using ammonium salt / amine salt as a high-temperature foaming agent, the decomposition of ammonium salt / amine salt at high temperature will absorb a large amount of heat to play a cooling role. At the same time, the ammonia produced by the decomposition of ammonium salt / amine salt can inhibit free radical reactions and terminate chain combustion reactions, which can play an active fire extinguishing effect and improve the flame retardant and heat insulation effects.
[0026] 5. The inorganic expansion coating of the present invention uses water as a solvent, which is environmentally friendly and non-toxic, and helps to reduce environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic structural diagram of an expandable double-sided adhesive tape according to an embodiment of the present invention;
[0028] Figure 2 is a schematic structural diagram of an expandable double-sided adhesive tape according to another embodiment of the present invention;
[0029] Figure 3 This is a physical picture of Example 1 of the expandable double-sided adhesive tape of the present invention;
[0030] Figure 4 This is a real picture of Example 1 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (before burning);
[0031] Figure 5 This is a real picture of the embodiment 1 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (when burning);
[0032] Figure 6 This is a real picture of Example 1 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (after burning);
[0033] Figure 7 This is a physical picture of the comparative example 1 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (before burning);
[0034] Figure 8 This is a real picture of the comparative example 1 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (when burning);
[0035] Fig. 9 This is a real picture of the comparative example 1 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (after burning);
[0036] Fig.10 This is a real picture of Example 2 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (before burning);
[0037] Fig.11 This is a real picture of Example 2 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (when burning);
[0038] Fig.12 This is a real picture of Example 2 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (after burning);
[0039] Fig.13 This is a real picture of the comparative example 2 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (before burning);
[0040] Fig.14 This is a real picture of the comparative example 2 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (when burning);
[0041] Fig.15 This is a real picture of the comparative example 2 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (after burning);
[0042] Fig.16 This is a real picture of the comparative example 3 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (before burning);
[0043] Fig.17 This is a real picture of the comparative example 3 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (when burning);
[0044] Fig.18 This is a real picture of the comparative example 3 of the expandable double-sided adhesive tape of the present invention attached to a metal iron sheet (after burning);
[0045] Fig.19 The present invention is a process flow chart of the preparation of the expandable double-sided adhesive tape. DETAILED DESCRIPTION
[0046] In order to facilitate the understanding of the present invention, the present invention is described more fully below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0047] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0048] See also Figure 1 The present invention provides an expandable double-sided adhesive tape, comprising a release paper layer 1, a pressure-sensitive adhesive layer 2 and an inorganic expandable coating 3; the pressure-sensitive adhesive layer 2 is provided on the upper and lower surfaces of the inorganic expandable coating 3, respectively, and the release paper layer 1 is provided on the surface of the pressure-sensitive adhesive layer 2 away from the inorganic expandable coating 3; the inorganic expandable coating 3 comprises the following components in parts by weight: 100 parts of water, 40-80 parts of phosphate, 1-20 parts of oxalate, 10-30 parts of carbonate, 1-5 parts of borate, 1-5 parts of magnesium oxide, 1-20 parts of boehmite, 0.5-5 parts of dispersant and 10-20 parts of binder.
[0049] The intumescent flame-retardant double-sided adhesive tape provided by the present invention has good adhesion and flame retardancy at the same time: by sandwiching the inorganic intumescent coating 3 between the two layers of the pressure-sensitive adhesive layer 2, after the release paper layer 1 is torn off, the contact surface between the intumescent double-sided adhesive tape and the adhered object is the pressure-sensitive adhesive layer 2, and the pressure-sensitive adhesive layer 2 can provide good adhesion to the adhered object, so that the intumescent double-sided adhesive tape can maintain good adhesion performance and will not cause the adhesion to decrease due to the addition of flame retardants; when encountering combustion, the intumescent flame-retardant double-sided adhesive tape will undergo a foaming reaction at high temperature; not only will it not burn itself, but its volume will expand to a large extent, and a fireproof and heat-insulating layer with high temperature resistance and low thermal conductivity will be formed, which has the effect of preventing the expansion and spread of flames; the pressure-sensitive adhesive layer 2 provides good adhesion to the adhered object, and the inorganic intumescent coating 3 provides good high temperature resistance, low thermal conductivity, and flame retardancy to prevent the expansion and spread of flames, thereby solving the problem of the contradiction between the adhesion and flame retardancy of the existing flame-retardant double-sided adhesive tape.
[0050] By adding the binder into the inorganic expansion coating 3, the binder penetrates and diffuses between the pressure-sensitive adhesive layers 2, so that good bonding force is formed between the inorganic expansion coating 3 and the pressure-sensitive adhesive layer 2, thereby preventing the inorganic expansion coating 3 from falling off the pressure-sensitive adhesive layer 2, and further ensuring the bonding and flame retardancy of the expandable double-sided adhesive tape.
[0051] In the formula of the inorganic expansion coating 3, the carbonate and the oxalate act as high-temperature foaming agents to achieve foaming, expansion and heat insulation; the boehmite and the magnesium oxide play a role in high temperature resistance and heat insulation; by adding a higher content of the phosphate, the expansion reaction of the inorganic expansion coating 3 can be catalyzed at high temperature, the expansion ratio of the inorganic expansion coating 3 can be increased, and the flame retardant performance can be improved.
[0052] To further illustrate, the adhesive is acrylic emulsion, and the pressure-sensitive adhesive layer 2 is polyacrylate pressure-sensitive adhesive.
[0053] The composition of the binder is consistent with that of the pressure-sensitive adhesive layer 2, both of which are polyacrylic acid. The pressure-sensitive adhesive layer 2 is similarly compatible with the binder in the inorganic expansion coating 3, and mutual penetration and diffusion will occur, thereby forming a strong interface bonding force, thereby forming good bonding force between the pressure-sensitive adhesive layer 2 and the inorganic expansion coating 3.
[0054] To further illustrate, the thickness of the inorganic expansion coating 3 is 0.1 mm to 0.5 mm.
[0055] The thickness of the inorganic expansion coating 3 is set to 0.1 mm to 0.5 mm. By setting a reasonable thickness, the thinner inorganic expansion coating 3 shows stronger flame retardant and fireproof performance, while ensuring the performance of the expansion double-sided adhesive tape, reducing material consumption and reducing production costs, so that the overall thickness of the expansion double-sided adhesive tape is thinner and the weight is lighter, which can be suitable for application scenarios that need to control thickness or weight, thereby improving practicality.
[0056] See also Figure 2 , further illustrating that the pressure-sensitive adhesive layer 2 is composed of a substrate layer 22 and two adhesive layers 21 , and the two adhesive layers 21 are respectively covered on the upper and lower surfaces of the substrate layer 22 .
[0057] The pressure-sensitive adhesive layer 2 is composed of two adhesive layers 21 and a substrate layer 22. By providing the substrate layer 22, additional support can be provided for the pressure-sensitive adhesive layer 2, so that the expandable double-sided adhesive tape is more stable and less prone to cracking during use, and can be used in scenarios requiring higher mechanical strength.
[0058] In other embodiments, the pressure-sensitive adhesive layer 2 can also be set to only one layer of the adhesive layer 21, which can make the pressure-sensitive adhesive layer 2 thinner and more flexible to use, thereby increasing the application scenarios of the expandable double-sided adhesive tape, such as application scenarios that need to save space or pursue product lightweighting, or application in pasting to various curved surfaces and irregular surfaces.
[0059] To further explain, the material of the substrate layer 22 is any one of tissue paper, non-woven fabric, PET film, polyimide film, polycarbonate film or polyvinyl chloride film.
[0060] Different materials can be selected as the substrate layer 22 according to different pasting requirements. For example, the tissue paper has good water resistance and weather resistance; the PET film, the polyimide film and the polycarbonate film all have good physical and mechanical properties, excellent impact resistance, high tensile strength and bending strength, excellent electrical properties, etc.
[0061] To further illustrate, both the phosphate and the borate are ammonium salts.
[0062] When ammonium phosphate is decomposed by heat, phosphorus pentoxide and ammonia will be produced. Phosphorus pentoxide is usually a gas flame retardant, which can react with the combustion products in the combustibles to form phosphates, forming a protective film on the surface to prevent the flame from spreading further. When ammonium borate is decomposed by heat, boron oxide glass and ammonia will be produced. Boron oxide has a low melting point and is a viscous liquid at high temperatures. It forms a low-melting-point viscous glass with phosphates, which plays a role of high-temperature bonding, so that the expansion layer of the inorganic expansion coating 3 after foaming and expansion can maintain structural stability, thereby improving the flame retardant and heat insulation effects.
[0063] At the same time, the ammonia produced by the thermal decomposition of the ammonium phosphate salt and the ammonium borate salt can inhibit free radical reactions, terminate chain combustion reactions, and play an active fire extinguishing effect, so that the intumescent flame retardant double-sided adhesive tape can truly prevent combustion, solving the problem that the existing flame retardant double-sided adhesive tape can only prevent the tape itself from burning when heated, but cannot inhibit flame spread and combustion.
[0064] To further illustrate, the carbonate is an ammonium salt, and the oxalate is an ammonium salt or a compound formed by oxalic acid and an organic amine.
[0065] The carbonate and the oxalate are used as high-temperature foaming agents to achieve foaming, expansion and heat insulation. The carbonate is an ammonium salt, and the oxalate is a compound formed by an ammonium salt or oxalic acid and an organic amine, which will produce ammonia gas when decomposed at high temperature, and can absorb a large amount of heat to achieve a cooling effect. At the same time, the generated ammonia gas can also inhibit free radical reactions, terminate chain combustion reactions, and achieve an active fire extinguishing effect.
[0066] Further, the dispersant is any one of sodium tripolyphosphate, sodium tartrate or polyethylene glycol.
[0067] Using any one of the sodium tripolyphosphate, the sodium tartrate or the polyethylene glycol as the dispersant plays a role in improving the dispersibility and uniformity of the inorganic expansion coating 3 .
[0068] See also Fig.19 The present invention also provides a method for preparing an expandable double-sided adhesive tape, which is used to prepare any of the above-mentioned expandable double-sided adhesive tapes, comprising the following steps:
[0069] Step S1, preparing an inorganic intumescent coating according to the component dosage of the inorganic intumescent coating 3: adding the phosphate, the oxalate, the carbonate and the borate into water, stirring and dissolving, and preparing slurry A; adding the boehmite and the magnesium oxide into the slurry A, stirring and dispersing, and then respectively adding the dispersant and the binder, mixing evenly, to obtain the inorganic intumescent coating;
[0070] Step S2, coating and drying of a carrier substrate: using a release paper roll with a pressure-sensitive adhesive as the carrier substrate, uniformly coating the inorganic expansion coating prepared in step S1 on the surface of the pressure-sensitive adhesive, and after drying in an oven to remove moisture, the inorganic expansion coating forms the inorganic expansion coating 3 on the surface of the pressure-sensitive adhesive, thereby preparing an intermediate adhesive tape;
[0071] Step S3, laminating the intermediate tape: using another roll of release paper with a pressure-sensitive adhesive as a laminating material, laminating it on the surface of the inorganic expandable coating 3 of the intermediate tape to obtain the expandable flame-retardant double-sided adhesive tape.
[0072] The method for preparing the intumescent flame-retardant double-sided adhesive tape of the present invention is to directly coat the inorganic intumescent coating on the release paper with a pressure-sensitive adhesive, form the inorganic intumescent coating 3 after oven drying, and then adhere another release paper roll with a pressure-sensitive adhesive to obtain the finished product. The entire process is easy to control and implement, and the cost is low.
[0073] To further illustrate, when the inorganic expansion coating is coated on the surface of the pressure-sensitive adhesive, the coating thickness of the inorganic expansion coating 3 can be controlled by controlling the gap between the scraper of the coating machine.
[0074] The inorganic expansion coating 3 is formulated with water as a solvent, which is environmentally friendly and non-toxic, and helps to reduce environmental pollution.
[0075] The present invention also proposes the use of any one of the above-mentioned expandable double-sided adhesive tapes in the fields of electronic appliances, transportation and construction.
[0076] The expandable double-sided adhesive tape has both good bonding properties and flame retardant and fireproof properties, and can be used to bond and fix various substrates, including metal materials, inorganic non-metallic materials, polymer materials, building materials and composite materials. It can be applied to battery bonding, automotive interior bonding, automotive wiring bonding, wire packaging, distribution box fixing, air conditioning fixing, electronic and electrical industry, home appliances, construction, signs and display devices, fire-fighting equipment fixing and other scenes with flame retardant and fireproof requirements.
[0077] (I) Example 1 and Comparative Example 1:
[0078] (1) Example 1: An expandable double-sided adhesive tape, comprising a release paper layer 1, a pressure-sensitive adhesive layer 2 and an inorganic expandable coating 3; the pressure-sensitive adhesive layer 2 is provided on the upper and lower surfaces of the inorganic expandable coating 3, respectively, and the release paper layer 1 is provided on the surface of the pressure-sensitive adhesive layer 2 away from the inorganic expandable coating 3; the pressure-sensitive adhesive layer 2 is composited by a substrate layer 22 and two adhesive layers 21, the two adhesive layers 21 are respectively covered on the upper and lower surfaces of the substrate layer 22, and the substrate layer 22 is cotton paper; the thickness of the inorganic expandable coating 3 is 0.24 mm; in parts by weight, the inorganic expandable coating 3 comprises the following components: 100 parts of water, 55 parts of phosphate (ammonium polyphosphate), 12 parts of oxalate (ammonium oxalate), 5 parts of borate (ammonium borate), 10 parts of carbonate (ammonium bicarbonate), 20 parts of boehmite, 4 parts of magnesium oxide, 0.5 parts of dispersant (polyethylene glycol PEG-10000) and 18 parts of binder (acrylic emulsion).
[0079] The preparation method of Example 1 is:
[0080] Step S1, preparing an inorganic expansion coating according to the component dosage of the inorganic expansion coating 3: adding 55 parts of ammonium polyphosphate, 12 parts of ammonium oxalate, 5 parts of ammonium borate and 10 parts of ammonium bicarbonate to 100 parts of water, stirring for 1 hour to dissolve part of the salt, and preparing slurry A; adding 20 parts of boehmite and 4 parts of magnesium oxide to the slurry A, stirring and dispersing, and then adding 0.5 parts of the dispersant (polyethylene glycol PEG-10000) respectively, stirring for 10 minutes, and finally adding 18 parts of the binder (acrylic emulsion), stirring and mixing evenly, transferring to a ball mill, and ball milling at a speed of 300 rpm for 2 hours to obtain the inorganic expansion coating;
[0081] Step S2, coating and drying of the carrier substrate: a release paper roll with a pressure-sensitive adhesive (the release paper roll with a pressure-sensitive adhesive is a common non-flame-retardant cotton paper double-sided tape) is used as the carrier substrate, fed into a coating machine, unwound, and the inorganic expansion coating prepared in step S1 is evenly coated on the surface of the pressure-sensitive adhesive, and the coating thickness of the inorganic expansion coating is adjusted by adjusting the gap of the scraper. After drying in an oven to remove moisture, the inorganic expansion coating forms the inorganic expansion coating 3 on the surface of the pressure-sensitive adhesive, thereby preparing an intermediate tape;
[0082] Step S3, laminating the intermediate tape: using another roll of release paper with pressure-sensitive adhesive (the release paper with pressure-sensitive adhesive is ordinary non-flame-retardant cotton paper double-sided tape) as a laminating material, laminating it on the surface of the inorganic expandable coating 3 of the intermediate tape to obtain the expandable flame-retardant double-sided adhesive tape.
[0083] (2) Comparative Example 1: A commercially available ordinary non-flame retardant cotton paper double-sided tape, which is the same model as the release paper roll with pressure-sensitive adhesive used in Example 1.
[0084] (3) Result analysis:
[0085] See also Figure 3 As shown in Table 1, the total thickness of the intumescent flame-retardant double-sided adhesive tape prepared in Example 1 is 0.64 mm, wherein the thickness of the release paper roll with pressure-sensitive adhesive is 0.2 mm (including a 0.1 mm thick release paper layer 1 and a 0.1 mm thick pressure-sensitive adhesive layer 2), and the thickness of the inorganic intumescent coating 3 is 0.24 mm; please continue to refer to Figure 4 , tear off the release paper layer 1 of the intumescent flame retardant double-sided adhesive tape, and stick it on a metal iron sheet with a thickness of 0.6 mm, and the total thickness is measured to be about 1.1 mm; please continue to refer to Figure 5 , the other release paper layer 1 of the intumescent flame retardant double-sided adhesive tape was torn off and then directly burned with a butane spray gun flame, and no obvious flame spread occurred; please continue to refer to Figure 6 , the measured thickness after burning reached 5.6mm; after deducting the thickness of the metal iron sheet itself, the thickness of the sample after burning (5mm) was obtained. The thickness of the sample in Example 1 expanded from the initial 0.44mm to 5mm, expanding by 11.4 times, showing excellent expansion flame retardancy. The adhesive properties (initial adhesion, peeling force and holding force) of the expansion flame retardant double-sided adhesive tape were measured. The test results are shown in Table 1. It can be seen that the initial adhesion, peeling force and holding force all meet the requirements of the standard value, which is close to the non-flame retardant cotton paper double-sided adhesive tape in Comparative Example 1, and there is no decrease in adhesive performance. It should be noted that the performance test method and quality judgment are carried out in accordance with the following standards: ① The test standard for initial adhesion is Method A (inclined rolling ball method) in GB / T 4852-2002 "Test method for initial adhesion of pressure-sensitive adhesive tapes (rolling ball method)"; ② The test standard for peeling force is Method 1 (test method for 180° peeling strength of adhesive tape and stainless steel) in GB / T 2792-2014 "Test method for peel strength of adhesive tapes"; ③ The test standard for holding force is Method A (test method for holding adhesion of adhesive tape and vertical standard steel plate) in GB / T 4851-2014 "Test method for holding adhesion of adhesive tapes" ; See also Figure 7 , the ordinary non-flame retardant cotton paper double-sided tape of comparative example 1 was attached to a metal iron sheet with a thickness of 0.6 mm, and the total thickness was measured to be 0.8 mm, that is, after deducting the thickness of the metal iron sheet, the thickness of the ordinary non-flame retardant cotton paper double-sided tape of comparative example 1 was 0.2 mm (including a 0.1 mm thick release paper layer and a 0.1 mm thick pressure-sensitive adhesive layer); please continue to refer to Figure 8 , tear off the release paper layer and directly burn it with a butane torch flame, and you can see obvious flame diffusion; please continue to refer to Fig. 9 After burning, the thickness of comparative example 1 was measured to be 0.75 mm. After deducting the thickness of the metal iron sheet itself, the thickness of the sample after burning was (0.15 mm). The thickness of the sample increased from the initial 0.1 mm to 0.15 mm, which only increased by 50%, in sharp contrast to Example 1.
[0086] Table 1 Test results of Example 1 and Comparative Example 1
[0087]
[0088] (II) Example 2 and Comparative Example 2:
[0089] (1) Example 2: An expandable double-sided adhesive tape, comprising a release paper layer 1, a pressure-sensitive adhesive layer 2 and an inorganic expandable coating 3; the pressure-sensitive adhesive layer 2 is provided on the upper and lower surfaces of the inorganic expandable coating 3, respectively, and the release paper layer 1 is provided on the surface of the pressure-sensitive adhesive layer 2 away from the inorganic expandable coating 3; the pressure-sensitive adhesive layer 2 is composited by a substrate layer 22 and two adhesive layers 21, the two adhesive layers 21 are respectively covered on the upper and lower surfaces of the substrate layer 22, and the substrate layer 22 is a PET film; the thickness of the inorganic expandable coating 3 is 0.35 mm; in parts by weight, the inorganic expandable coating 3 comprises the following components: 100 parts of water, 60 parts of phosphate (ammonium polyphosphate), 15 parts of oxalate (ammonium oxalate), 2 parts of borate (ammonium borate), 15 parts of carbonate (ammonium bicarbonate), 15 parts of boehmite, 5 parts of magnesium oxide, 2 parts of dispersant (sodium tartrate) and 20 parts of binder (acrylic emulsion).
[0090] The preparation method of Example 2 is:
[0091] Step S1, preparing an inorganic expansion coating according to the component dosage of the inorganic expansion coating 3: adding 60 parts of ammonium polyphosphate, 15 parts of ammonium oxalate, 2 parts of ammonium borate and 15 parts of ammonium bicarbonate to 100 parts of water, stirring for 1 hour to dissolve part of the salt, and preparing slurry A; adding 15 parts of boehmite and 5 parts of magnesium oxide to the slurry A, and then adding 2 parts of the dispersant (sodium tartrate) respectively, stirring for 10 minutes, and finally adding 20 parts of the binder (acrylic emulsion), stirring and mixing evenly, transferring to a ball mill, and ball milling at a speed of 300 rpm for 2 hours to obtain the inorganic expansion coating;
[0092] Step S2, coating and drying of a carrier substrate: a release paper roll with a pressure-sensitive adhesive (the release paper roll with a pressure-sensitive adhesive is a common non-flame-retardant PET double-sided tape) is used as the carrier substrate, fed into a coating machine, unwound, and the inorganic expansion coating prepared in step S1 is evenly coated on the surface of the pressure-sensitive adhesive, and the coating thickness of the inorganic expansion coating is adjusted by adjusting the gap of the scraper. After drying in an oven to remove moisture, the inorganic expansion coating forms the inorganic expansion coating 3 on the surface of the pressure-sensitive adhesive, thereby preparing an intermediate tape;
[0093] Step S3, laminating the intermediate tape: another roll of release paper with pressure-sensitive adhesive (the release paper with pressure-sensitive adhesive is a common non-flame-retardant PET double-sided tape) is used as a laminating material and is laminated to the surface of the inorganic expandable coating 3 of the intermediate tape to obtain the expandable flame-retardant double-sided tape.
[0094] (2) Comparative Example 2: A commercially available common non-flame retardant PET double-sided tape, which is the same model as the release paper roll with pressure-sensitive adhesive used in Example 2.
[0095] (3) Result analysis:
[0096] See also Fig.10 As shown in Table 2, the total thickness of the intumescent flame-retardant double-sided adhesive tape prepared in Example 2 is 0.65 mm, wherein the release paper roll with pressure-sensitive adhesive (thickness 0.15 mm) includes a 0.1 mm thick release paper layer 1, a 0.05 mm thick pressure-sensitive adhesive layer 2 (including two 0.01 mm thick adhesive layers 21 and a 0.03 mm thick substrate layer 22, wherein the substrate layer 22 is a PET film), and the inorganic intumescent coating 3 has a thickness of 0.35 mm; a layer of the release paper layer 1 of the intumescent flame-retardant double-sided adhesive tape is torn off and attached to a metal iron sheet with a thickness of 0.6 mm, and the total thickness is measured to be approximately 1.15 mm; please continue to refer to Fig.11 , the other release paper layer 1 of the intumescent flame retardant double-sided adhesive tape was torn off and then directly burned with a butane spray gun flame, and no obvious flame spread occurred; please continue to refer to Fig.12 After burning, the measured thickness reached 4.5mm. The thickness of the sample after burning was deducted from the thickness of the metal iron sheet itself (3.9mm), that is, the thickness of the sample expanded from the initial 0.45mm to 3.9mm, expanding 8.7 times, showing excellent expansion flame retardancy. The bonding properties (initial adhesion, peeling force and holding force) of the expansion flame retardant double-sided adhesive tape were measured. The test results are shown in Table 2. It can be seen that the initial adhesion, peeling force and holding force all meet the requirements of the standard value, which is close to the ordinary non-flame retardant PET double-sided adhesive tape of Comparative Example 2, and there is no decrease in bonding performance.
[0097] See also Fig.13 , the ordinary non-flame retardant PET double-sided tape of comparative example 2 was attached to a metal iron sheet with a thickness of 0.6 mm, and the total thickness was measured to be 0.75 mm, that is, after deducting the thickness of the metal iron sheet, the thickness of the ordinary non-flame retardant PET double-sided tape of comparative example 2 was 0.15 mm (including a 0.1 mm thick release paper layer and a 0.05 mm thick pressure-sensitive adhesive layer); please continue to refer to Fig.14 , tear off the release paper layer and burn it directly with a butane torch flame. You can see that the PET adhesive layer shrinks and there is obvious flame diffusion; please continue to refer to Fig.15 After burning, the thickness of comparative example 2 was measured to be about 0.63 mm. After deducting the thickness of the metal iron sheet itself, the thickness of the sample after burning was obtained (0.03 mm). The thickness of the sample was reduced from the initial 0.05 mm to 0.03 mm, which was in sharp contrast to Example 2.
[0098] Table 2 Test results of Example 2 and Comparative Example 2
[0099]
[0100] (III) Comparative Example 3
[0101] (1) Comparative Example 3: A commercially available flame retardant cotton paper double-sided tape.
[0102] See also Fig.16 , the flame retardant cotton paper double-sided tape of comparative example 3 is attached to a metal iron sheet with a thickness of 0.6 mm, and the total thickness is measured to be 0.8 mm, that is, after deducting the thickness of the metal iron sheet, the thickness of comparative example 3 is 0.2 mm (including a 0.1 mm thick release paper layer and a 0.1 mm thick pressure-sensitive adhesive layer); please continue to refer to Fig.17 , tear off the release paper layer and directly burn it with a butane torch flame, and you can see obvious flame diffusion; please continue to refer to Fig.18 After burning, the thickness of comparative example 3 was measured to be 0.85 mm, and the thickness of the sample after burning was obtained after deducting the thickness of the metal iron sheet itself (0.25 mm). The thickness of the sample expanded from the initial 0.1 mm to 0.25 mm, which was in sharp contrast to examples 1 and 2. It can be seen that the ordinary flame-retardant cotton paper double-sided tape, although it will also expand in volume when burning with an open flame, the increase is not obvious, and under high-temperature open flame burning, flame spread will still occur, and the flame retardant effect is not good.
[0103] (III) Examples 3 to 7 and Comparative Examples 4 to 5
[0104] (1) The difference between Example 3 and Example 2 is that the pressure-sensitive adhesive layer 2 of the intumescent flame-retardant double-sided adhesive tape prepared in Example 3 is composed of only one layer of the adhesive layer 21, and the rest is the same as Example 2.
[0105] (2) The difference between Examples 4 to 5 and Example 1 is that the thickness of the inorganic expansion coating 3 in Examples 4 to 5 is carried out according to the data in Table 4;
[0106] Table 4 Thickness of inorganic expansion coating (unit: mm)
[0107] sample Example 1 Example 4 Example 5 Thickness of inorganic expansion coating (mm) 0.24 0.1 0.5
[0108] (3) The difference between Examples 6-7 and Comparative Examples 4-5 and Example 1 is that the component contents of the inorganic expansion coating 3 are as shown in Table 5:
[0109] Table 5 Component contents of inorganic expansion coating (unit: in parts by weight)
[0110]
[0111] (4) Result analysis: The test results are shown in Table 6 and compared with the results in Tables 1 and 2.
[0112] The total thickness of the intumescent flame-retardant double-sided adhesive tape prepared in Example 3 is thinner, and no obvious flame diffusion occurs when the sample is directly sprayed with a butane spray gun flame. The expanded thickness after burning is close to that in Example 2, and the bonding performance is also close to that in Example 2, and it has excellent intumescent flame retardancy and bonding performance.
[0113] The intumescent flame-retardant double-sided adhesive tapes prepared in Examples 4 to 7 did not show obvious flame diffusion after being burned with a butane spray gun flame, and the expansion ratio after burning was close to that of Example 1, showing good intumescent flame retardancy, and the greater the thickness of the inorganic intumescent coating 3, the better the expansion effect. The bonding performance of the intumescent flame-retardant double-sided adhesive tapes prepared in Examples 4 to 7 was close to that of the non-flame-retardant cotton paper double-sided adhesive tape in Comparative Example 1, and there was no decrease in bonding performance.
[0114] The expandable flame-retardant double-sided adhesive tape prepared in Comparative Example 4 has a significantly reduced expansion thickness after the sample is directly sprayed with a butane spray gun flame, and the thermal insulation performance is poor. This shows that since ammonium carbonate and ammonium oxalate are used as high-temperature foaming agents, they will decompose into water vapor, carbon dioxide and ammonia during the heating process, which will have a foaming and expansion effect. When the components of the inorganic expansion coating 3 lack ammonium carbonate and ammonium oxalate, the inorganic expansion coating 3 has a poor thermal expansion and foaming effect, resulting in insufficient thickness of the foamed expansion layer and poor flame retardant and heat-insulating effects.
[0115] The intumescent flame-retardant double-sided adhesive tape prepared in Comparative Example 5 also has a small expansion thickness after the sample is directly sprayed with a butane spray gun flame, and the expansion layer is easy to crack and fall off. It can be seen that due to the reduction in the content of ammonium phosphate and ammonium borate, the expansion ratio of the inorganic intumescent coating 3 is reduced, the inorganic intumescent coating 3 produces less glass liquid when decomposed by heat, and the structural stability of the inorganic intumescent coating 3 during high-temperature expansion is reduced, resulting in insufficient expansion thickness, easy cracking and falling of the expansion layer, and poor flame retardant and heat insulation effects.
[0116] Table 6 Test results of Examples 3 to 7 and Comparative Examples 4 to 5
[0117]
[0118] Table 6 (Continued) Test results of Examples 3 to 7 and Comparative Examples 4 to 5
[0119]
[0120]
[0121] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. An expandable double-sided adhesive tape, It is characterized in that It comprises a release paper layer, a pressure-sensitive adhesive layer and an inorganic expansion coating; the pressure-sensitive adhesive layer is provided on the upper and lower surfaces of the inorganic expansion coating respectively, and the release paper layer is provided on the surface of the pressure-sensitive adhesive layer away from the inorganic expansion coating; The inorganic expansion coating comprises the following components by weight: 100 parts of water, 40-80 parts of phosphate, 1-20 parts of oxalate, 10-30 parts of carbonate, 1-5 parts of borate, 1-5 parts of magnesium oxide, 1-20 parts of boehmite, 0.5-5 parts of dispersant and 10-20 parts of binder.
2. The expandable double-sided adhesive tape according to claim 1, It is characterized in that The adhesive is acrylic emulsion, and the pressure-sensitive adhesive layer is polyacrylate pressure-sensitive adhesive.
3. The expandable double-sided adhesive tape according to claim 1, It is characterized in that The thickness of the inorganic expansion coating is 0.1 mm to 0.5 mm.
4. The expandable double-sided adhesive tape according to claim 1, It is characterized in that The pressure-sensitive adhesive layer is formed by compounding a substrate layer and two adhesive layers, and the two adhesive layers are respectively covered on the upper and lower surfaces of the substrate layer.
5. The expandable double-sided adhesive tape according to claim 4, It is characterized in that The material of the substrate layer is any one of tissue paper, non-woven fabric, PET film, polyimide film, polycarbonate film or polyvinyl chloride film.
6. The expandable double-sided adhesive tape according to claim 1, It is characterized in that The phosphate and the borate are both ammonium salts.
7. The expandable double-sided adhesive tape according to claim 1, It is characterized in that The carbonate is an ammonium salt, and the oxalate is an ammonium salt or a compound formed by oxalic acid and an organic amine.
8. The expandable double-sided adhesive tape according to claim 1, It is characterized in that The dispersant is any one of sodium tripolyphosphate, sodium tartrate or polyethylene glycol.
9. A method for preparing an expandable double-sided adhesive tape, for preparing the expandable double-sided adhesive tape as claimed in any one of claims 1 to 8, It is characterized in that The following steps are involved: Step S1, preparing an inorganic intumescent coating according to the component dosage of the inorganic intumescent coating: adding the phosphate, the oxalate, the carbonate and the borate into water, stirring and dissolving, and preparing slurry A; Add the boehmite and the magnesium oxide to the slurry A, and then add the dispersant and the binder respectively, mix them evenly, and obtain the inorganic intumescent coating; Step S2, coating and drying of a carrier substrate: using a release paper roll with a pressure-sensitive adhesive as the carrier substrate, uniformly coating the inorganic expansion coating prepared in step S1 on the surface of the pressure-sensitive adhesive, and after drying in an oven to remove moisture, the inorganic expansion coating forms the inorganic expansion coating on the surface of the pressure-sensitive adhesive to prepare an intermediate adhesive tape; Step S3, laminating the intermediate tape: using another roll of release paper with a pressure-sensitive adhesive as a laminating material, laminating it on the surface of the inorganic expandable coating of the intermediate tape to obtain the expandable flame-retardant double-sided adhesive tape.
10. Use of the expandable double-sided adhesive tape according to any one of claims 1 to 8 in the fields of electronics, transportation and construction.