Method for preparing electromagnetic wave-absorbing material and electromagnetic wave-absorbing material
By adjusting the nickel-iron molar ratio and controlling the microstructure, a multi-band, wide-frequency electromagnetic absorbing material was prepared, solving the problems of large thickness and narrow absorption band of traditional materials, and realizing efficient absorption of electromagnetic waves of multiple frequency bands.
Patent Information
- Application Number
- CN202410874820.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional electromagnetic absorbing materials are thick and have a narrow effective absorption band, making them unsuitable for complex operating environments and electromagnetic radiation of various frequencies.
By adjusting the nickel-iron molar ratio and combining it with microstructure control strategies, electromagnetic absorbing materials with multi-band, wide frequency domain and thin thickness were prepared. Electromagnetic absorbing materials with zero-dimensional nanospheres, two-dimensional nanosphere-rod hybrid structures and three-dimensional lotus-shaped nanorod structures were formed by using nickel-iron particle compounds and intermediate substances in different proportions.
The system achieves efficient absorption of electromagnetic waves in multiple frequency bands with thin thickness. The zero-dimensional nanosphere structure has an absorption rate of 99.96% at 17.12 GHz, the two-dimensional nanosphere-rod hybrid structure has an absorption rate of 94.48% at 15.04 GHz, and the three-dimensional lotus-shaped nanorod structure has an absorption rate of 97.51% at 15.20 GHz, meeting the requirements for electromagnetic wave absorption in a wide frequency range and multiple bands.
Smart Images

Figure CN118995133A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electromagnetic absorbing materials, and in particular to a method for preparing high-performance electromagnetic absorbing materials and electromagnetic absorbing materials. Background Art
[0002] The electromagnetic radiation generated by new electronic devices not only harms human health, but also poses a threat to aircraft navigation safety. With the widespread application of new electronic devices, electromagnetic radiation has gradually become a hidden danger. Therefore, in order to reduce the negative effects of electromagnetic radiation, the demand for electromagnetic absorbing materials in the field of electromagnetic protection and anti-interference is growing.
[0003] Traditional metal electromagnetic absorbing materials are not suitable for today's complex use environment due to their large thickness and narrow effective absorption band. In order to minimize the space occupied by electromagnetic absorbing materials in practical applications and to absorb electromagnetic waves radiated from electronic devices with different working frequency bands, electromagnetic absorbing materials with thin thickness and wide band absorption capacity have become the focus of research. Summary of the invention
[0004] In order to solve the problems of large thickness and narrow effective absorption band of traditional electromagnetic absorbing materials, the present application provides a method for preparing electromagnetic absorbing materials and electromagnetic absorbing materials.
[0005] According to one aspect of the present application, there is provided a method for preparing an electromagnetic absorbing material, comprising:
[0006] Mixing a nickel particle compound and an iron particle compound in a set molar ratio into the first solution to form a first mixed solution;
[0007] adding a predetermined amount of an intermediate substance to the first mixed solution to form a second mixed solution;
[0008] Heating, keeping warm and cooling the second mixed solution, and collecting by centrifugation to obtain a first centrifugal product;
[0009] Purifying the first centrifugal product and collecting it by centrifugation to obtain a second centrifugal product;
[0010] The second centrifugal product is subjected to a carbonization and doping treatment to obtain an electromagnetic wave absorbing material with a microstructure.
[0011] According to an exemplary embodiment of the present application, the set molar ratio includes 3:1, and the electromagnetic absorbing material includes an electromagnetic absorbing material with a zero-dimensional nanosphere structure.
[0012] According to an exemplary embodiment of the present application, the set molar ratio includes 2:2, and the electromagnetic absorbing material includes an electromagnetic absorbing material with a two-dimensional nanosphere-rod hybrid structure.
[0013] According to an exemplary embodiment of the present application, the set molar ratio includes 1:3, and the electromagnetic absorbing material includes an electromagnetic absorbing material with a three-dimensional lotus-shaped nanorod structure.
[0014] According to an exemplary embodiment of the present application, the nickel particle compound includes nickel nitrate hexahydrate, the iron particle compound includes ferric chloride hexahydrate, the first solution includes an N,N-dimethylformamide-ethanol-water mixed solution with a volume ratio of 1:1:1, and the intermediate substance includes dihydroxyterephthalic acid.
[0015] According to an exemplary embodiment of the present application, heating, keeping warm and cooling the second mixed solution includes: heating the second mixed solution to 120° C. at a heating rate of 5° C. / min, and cooling to room temperature after keeping warm for 24 hours.
[0016] According to an exemplary embodiment of the present application, the purification process includes: washing the first centrifugal product using an N,N-dimethylformamide solution, anhydrous ethanol, and deionized water, respectively.
[0017] According to an exemplary embodiment of the present application, the number of washings includes 3 times, and the washing time of each time includes 12 hours.
[0018] According to an exemplary embodiment of the present application, the carbonization doping process includes: heating the second centrifugal product from room temperature to a set temperature at a set heating rate under a protective atmosphere, and keeping the temperature for a predetermined time.
[0019] According to an exemplary embodiment of the present application, the protective atmosphere includes an argon atmosphere, the set heating rate includes 2° C. / min, the set temperature includes 800° C., and the predetermined time includes 2 hours.
[0020] According to another aspect of the present application, an electromagnetic absorbing material prepared by the above method is provided.
[0021] In the method for preparing electromagnetic absorbing materials provided in the present application, a high-performance electromagnetic absorbing material is prepared by a material microstructure control strategy based on crystal growth theory according to the different absorbing characteristics exhibited by different material microstructures when facing electromagnetic waves. By adjusting the nickel-iron molar ratio in the precursor, a controllable multidimensional microstructure electromagnetic absorbing material from zero-dimensional nanospheres to three-dimensional lotus-shaped nanorods can be obtained. Among them, the electromagnetic absorbing material with a three-dimensional lotus-shaped nanorod structure can form more conductive networks and achieve a wider absorption bandwidth; the electromagnetic absorbing material with a two-dimensional nanosphere-rod hybrid structure has an effective absorption bandwidth of 4.88GHz and achieves an absorption rate of 94.48% at 15.04GHz; the electromagnetic absorbing material with a zero-dimensional nanosphere structure can provide more defect sites and achieve higher reflection loss. The maximum reflection loss at 17.12GHz is -34.29dB, the absorption rate is 99.96%, and the effective absorption bandwidth is 3.30GHz.
[0022] The electromagnetic absorbing material prepared by the method provided in the present application has the properties of multi-band, wide frequency domain and thin thickness, and can be used in the fields of anti-electromagnetic interference, radar wave absorption, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without exceeding the scope of protection required by the present application.
[0024] Figure 1 A schematic diagram of the overall process of preparing an electromagnetic absorbing material according to an exemplary embodiment of the present application is shown;
[0025] Figure 2 The method flow for preparing an electromagnetic absorbing material according to the first exemplary embodiment of the present application is shown;
[0026] Figure 3 A SEM schematic diagram of an electromagnetic absorbing material according to a first exemplary embodiment of the present application is shown;
[0027] Figure 4 A schematic diagram showing the test results of the electromagnetic absorbing material according to the first exemplary embodiment of the present application is shown;
[0028] Figure 5 The method flow for preparing an electromagnetic absorbing material according to a second exemplary embodiment of the present application is shown;
[0029] Figure 6 A SEM schematic diagram of an electromagnetic absorbing material according to a second exemplary embodiment of the present application is shown;
[0030] Figure 7 A schematic diagram showing the test results of the electromagnetic absorbing material according to the second exemplary embodiment of the present application is shown;
[0031] Figure 8 The method flow for preparing an electromagnetic absorbing material according to the third exemplary embodiment of the present application is shown;
[0032] Fig. 9 A SEM schematic diagram of an electromagnetic absorbing material according to a third exemplary embodiment of the present application is shown;
[0033] Fig.10 A schematic diagram of test results of an electromagnetic absorbing material according to a third exemplary embodiment of the present application is shown. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.
[0035] The terms "first", "second", etc. of the present application are used to distinguish different objects, rather than to describe a predetermined order. In addition, the terms "including" and "having" of the present application and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices.
[0036] Reference to "embodiment" herein means that the predetermined features, structures, or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0037] Generally, electromagnetic absorbing materials can be divided into two categories according to the basic components of the materials: carbon-based electromagnetic absorbing materials and metal-based electromagnetic absorbing materials. Among them, carbon-based electromagnetic absorbing materials absorb electromagnetic waves through the transmission loss (i.e., dielectric loss) generated by the conductive network, and the high specific surface area presented by carbon-based electromagnetic absorbing materials in different forms brings good interface polarization loss; however, carbon-based electromagnetic absorbing materials have the characteristics of high return loss and narrow effective absorption bandwidth, which cannot meet the needs of broadband absorption. Metal-based electromagnetic absorbing materials have good magnetic loss capacity based on their unique magnetic properties, and metal nanoparticles with different microstructures enhance the electromagnetic absorbing performance with their unique hysteresis loss; however, magnetic metal nanoparticles often aggregate due to the accumulation of a large number of positive and negative charges on the surface, thereby causing electromagnetic waves to be reflected on their surface, which also cannot meet the needs of electromagnetic wave absorption in practical applications.
[0038] To this end, the present application combines the porous conductive path structure of carbon-based electromagnetic absorbing materials with the magnetic nanoparticle characteristics of metal-based electromagnetic absorbing materials, aiming to provide a metal organic framework (MOF) derivative as an electromagnetic absorbing material. Based on the microstructure control strategy, the present application can prepare an electromagnetic absorbing material with absorption characteristics such as wide frequency domain, multi-band and thin thickness by adjusting the molar ratio of nickel and iron in the precursor.
[0039] Hereinafter, exemplary embodiments of the present application will be described in detail with reference to the accompanying drawings.
[0040] Figure 1 A schematic diagram of the overall process of preparing an electromagnetic absorbing material according to an exemplary embodiment of the present application is shown.
[0041] In an exemplary embodiment of the present application, a high-performance electromagnetic absorbing material is obtained based on a microstructure control strategy. Among them, the microstructure control strategy can be: controlling the surface energy of the crystal by controlling the molar ratio of two metal particles (for example, iron particles and nickel particles). The surface energy of a crystal can be defined as the work done by the crystal to form a new surface per unit area; according to the crystal growth theory, the surface energy of the crystal is directly related to the degree of supersaturation during the crystal growth process; a higher degree of supersaturation is conducive to the formation of crystals with higher surface energy; on the contrary, crystals surrounded by surfaces with lower surface energy are more stable, while crystals with higher surface energy tend to continue to grow until the surface energy is reduced to a stable level. Accordingly, with different degrees of supersaturation caused by different nickel / iron molar ratios, the position of the high surface energy surface of the crystal will change, which prompts the crystal to grow along the high surface energy surface until a stable structure with lower surface energy is reached. Therefore, by adjusting the molar ratio, the microstructure of the electromagnetic absorbing material can be controlled according to the principles of crystal growth theory, thereby obtaining a high-performance electromagnetic absorbing material.
[0042] See also Figure 1The overall process of preparing the electromagnetic absorbing material provided in this application includes the following steps.
[0043] First, a compound containing nickel particles and a compound containing iron particles are mixed into a first solution according to a set molar ratio, so that they are fully mixed to form a first mixed solution. According to an exemplary embodiment of the present application, the compound containing nickel particles can be nickel nitrate hexahydrate; the compound containing iron particles can be ferric chloride hexahydrate; and the first solution can be a N, N-dimethylformamide (DMF)-ethanol-water mixed solution. According to an exemplary embodiment of the present application, the set molar ratio between nickel nitrate hexahydrate and ferric chloride hexahydrate can be one of 3:1, 2:2 or 1:3. As an example, a total of 6.25mmol of nickel nitrate hexahydrate and ferric chloride hexahydrate can be mixed into 150mL of N, N-dimethylformamide (DMF)-ethanol-water solution according to a set molar ratio, wherein the volume ratio between N, N-dimethylformamide (DMF), ethanol and water can be 1:1:1. According to an exemplary embodiment of the present application, in order to allow the mixed compounds to be fully mixed, they can be fully mixed by stirring (e.g., ultrasonic oscillation), and the stirring time can be 25-35 minutes.
[0044] Next, the first mixed solution is added to the reaction vessel, and a predetermined amount of the intermediate substance is added for thorough mixing to form a second mixed solution. According to an exemplary embodiment of the present application, the intermediate substance may be dihydroxyterephthalic acid (H4DOBDC), which serves to provide a reaction template for the nickel particle compound and the iron particle compound; for 6.25 mmol of nickel nitrate hexahydrate and ferric chloride hexahydrate, the amount of dihydroxyterephthalic acid (H4DOBDC) may be 2.1 mmol (i.e., 0.416 g). According to an exemplary embodiment of the present application, in order to allow the mixed compounds to be fully mixed, they may be fully mixed by stirring (e.g., ultrasonic oscillation), and the stirring time may be 25-35 minutes. According to an exemplary embodiment of the present application, the reaction vessel may be a hydrothermal reactor.
[0045] Next, the second mixed solution is heated, kept warm, and cooled, and then the first centrifugal product is obtained by centrifugal collection. According to the exemplary embodiment of the present application, the reactor can be placed in a tubular furnace for heating; for example, heated to 110-130°C at a heating rate of 5°C / min; after keeping warm for 24 hours, cooled to room temperature; the centrifugal collection process can be to take the cooled reactor out of the heating furnace and collect it by centrifugation at a certain speed (for example, 7500rpm), and the collection time can be 10 minutes.
[0046] Next, the first centrifugal product is purified and the second centrifugal product is obtained by centrifugal collection. According to the exemplary embodiment of the present application, in order to purify the first centrifugal product, the first centrifugal product can be washed with DMF solution, anhydrous ethanol, and deionized water respectively. For example, 35mL of DMF solution can be used to perform a first purification treatment (e.g., washing) on the first centrifugal product, the number of washings can be 3 times, the washing time for each washing can be 12h, and centrifugal collection is performed again after washing; 35mL of anhydrous ethanol and deionized water are used to perform a second purification treatment (e.g., washing) on the centrifugal collection product to remove DMF, the number of washings can be 3 times, the washing time for each washing can be 6h, and centrifugal collection is performed again after washing; finally, the centrifugal collection product is dried at room temperature to obtain the second centrifugal product.
[0047] Finally, the second centrifugal product is subjected to carbonization doping treatment to obtain an electromagnetic absorbing material. According to an exemplary embodiment of the present application, the dried second centrifugal product can be placed in a tubular furnace, heated to 800°C at a heating rate of 2°C / min from room temperature under a protective atmosphere (e.g., argon atmosphere), and kept warm for a predetermined time (e.g., 2h) to perform carbonization doping treatment. The final product is the prepared electromagnetic absorbing material.
[0048] In the above process, electromagnetic absorbing materials with different microstructures can be obtained by setting different precursor metal molar ratios. For example, the precursor metal molar ratio can be set to 3:1, 2:2 or 1:3, respectively, to obtain electromagnetic absorbing materials with zero-dimensional nanosphere structure, electromagnetic absorbing materials with two-dimensional nanorod-sphere hybrid structure, and electromagnetic absorbing materials with three-dimensional lotus-shaped nanorod structure.
[0049] Figure 2 The method flow for preparing an electromagnetic absorbing material according to the first exemplary embodiment of the present application is shown; Figure 3 A SEM schematic diagram of an electromagnetic absorbing material according to a first exemplary embodiment of the present application is shown; Figure 4 A schematic diagram of test results of an electromagnetic absorbing material according to the first exemplary embodiment of the present application is shown.
[0050] In the first exemplary embodiment of the present application, the molar ratio of the precursor metal is set to 3:1, and the electromagnetic wave absorbing material finally prepared is an electromagnetic wave absorbing material with a zero-dimensional nanosphere structure. Figure 2 As shown, the method for preparing the electromagnetic absorbing material provided in the present application includes the following steps.
[0051] In step S210, a nickel particle compound and an iron particle compound in a first molar ratio are mixed into a first solution to form a first mixed solution. According to an exemplary embodiment of the present application, the first molar ratio is 3:1, the nickel particle compound can be 0.371g of nickel nitrate hexahydrate, and the iron particle compound can be 1.267g of ferric chloride hexahydrate; the first solution can be a solution obtained by mixing N,N-dimethylformamide (DMF)-ethanol-water in a volume ratio of 1:1:1, and the volume of the first solution can be 150mL. According to an exemplary embodiment of the present application, in order to allow the mixed compounds to be fully mixed, they can be fully mixed by stirring (e.g., ultrasonic oscillation), and the stirring time can be 30 minutes.
[0052] In step S220, a predetermined amount of an intermediate substance is added to the first mixed solution to form a second mixed solution. For example, the first mixed solution can be added to a reaction vessel first, and then a predetermined amount of an intermediate substance is added to the reaction vessel for thorough mixing. According to an exemplary embodiment of the present application, the intermediate substance can be dihydroxyterephthalic acid (H4DOBDC), and the amount of dihydroxyterephthalic acid (H4DOBDC) can be 0.416 g. According to an exemplary embodiment of the present application, in order to allow the mixed compounds to be fully mixed, they can be fully mixed by stirring (e.g., ultrasonic oscillation), and the stirring time can be 30 minutes. According to an exemplary embodiment of the present application, the reaction vessel can be a hydrothermal reactor.
[0053] In step S230, the second mixed solution is heated, kept warm, and cooled, and then the first centrifugal product is obtained by centrifugal collection. According to an exemplary embodiment of the present application, the reactor can be placed in a tubular furnace for heating; for example, heated to 120°C at a heating rate of 5°C / min; kept warm for 24 hours, and then cooled to room temperature; the centrifugal collection process can be to take the cooled reactor out of the heating furnace and centrifuge at a certain speed (for example, 7500rpm) for collection, and the collection time can be 10 minutes.
[0054] In step S240, the first centrifugal product is purified and a second centrifugal product is obtained by centrifugal collection. According to an exemplary embodiment of the present application, in order to purify the first centrifugal product, the first centrifugal product can be washed with a DMF solution, anhydrous ethanol, and deionized water. For example, 35 mL of a DMF solution can be used to perform a first purification treatment (e.g., washing) on the first centrifugal product, the number of washings can be 3 times, the washing time for each washing can be 12 hours, and centrifugal collection is performed again after washing; next, 35 mL of anhydrous ethanol or deionized water are used to perform a second purification treatment (e.g., washing) on the centrifugal collection product to remove DMF, the number of washings can be 3 times, the washing time for each washing can be 6 hours, and centrifugal collection is performed again after washing; finally, the centrifugal collection product is dried at room temperature to obtain a second centrifugal product.
[0055] In step S250, the second centrifugal product is subjected to carbonization doping treatment to obtain an electromagnetic absorbing material with a first microstructure. According to an exemplary embodiment of the present application, the dried second centrifugal product can be placed in a tubular furnace, heated from room temperature to 800°C at a heating rate of 2°C / min under a protective atmosphere (e.g., argon atmosphere), and kept at this temperature for a predetermined time (e.g., 2h) to perform carbonization doping treatment. Figure 3 As shown, the present application provides a Figure 2 The electromagnetic absorbing material prepared by the method shown; Figure 2 The electromagnetic wave absorbing material with the first microstructure finally obtained by the method shown is an electromagnetic wave absorbing material with a zero-dimensional nanosphere structure.
[0056] After electromagnetic performance tests, such as Figure 4 As shown, the electromagnetic absorbing material with a zero-dimensional nanosphere structure prepared by the method provided in the first exemplary embodiment of the present application has a maximum reflection loss of -34.29 dB at 17.12 GHz, an absorptivity of 99.96%, an effective absorption bandwidth of 3.30 GHz, and exhibits a strong high return loss capability.
[0057] Figure 5 The method flow for preparing an electromagnetic absorbing material according to a second exemplary embodiment of the present application is shown; Figure 6 A SEM schematic diagram of an electromagnetic absorbing material according to a second exemplary embodiment of the present application is shown; Figure 7 A schematic diagram of test results of an electromagnetic absorbing material according to a second exemplary embodiment of the present application is shown.
[0058] In the first exemplary embodiment of the present application, the molar ratio of the precursor metal is set to 2:2, and the electromagnetic wave absorbing material finally prepared is an electromagnetic wave absorbing material of a two-dimensional nanosphere-rod hybrid structure. Figure 5As shown, the method for preparing the electromagnetic absorbing material provided in the present application includes the following steps.
[0059] In step S510, the nickel particle compound and the iron particle compound in the second molar ratio are mixed into the first solution to form a first mixed solution. According to an exemplary embodiment of the present application, the first molar ratio is 2:2, the nickel particle compound can be 0.743g of nickel nitrate hexahydrate, and the iron particle compound can be 0.845g of ferric chloride hexahydrate; the first solution can be a solution obtained by mixing N,N-dimethylformamide (DMF)-ethanol-water in a volume ratio of 1:1:1, and the volume of the first solution can be 150mL. According to an exemplary embodiment of the present application, in order to allow the mixed compounds to be fully mixed, they can be fully mixed by stirring (e.g., ultrasonic oscillation), and the stirring time can be 30 minutes.
[0060] In step S520, a predetermined amount of an intermediate substance is added to the first mixed solution to form a second mixed solution. For example, the first mixed solution can be first added to a reaction vessel, and then a predetermined amount of an intermediate substance is added to the reaction vessel for thorough mixing. According to an exemplary embodiment of the present application, the intermediate substance can be dihydroxyterephthalic acid (H4DOBDC), and the amount of dihydroxyterephthalic acid (H4DOBDC) can be 0.416 g. According to an exemplary embodiment of the present application, in order to allow the mixed compounds to be fully mixed, they can be fully mixed by stirring (e.g., ultrasonic oscillation), and the stirring time can be 30 minutes. According to an exemplary embodiment of the present application, the reaction vessel can be a hydrothermal reactor.
[0061] In step S530, the second mixed solution is heated, kept warm, and cooled, and then the first centrifugal product is obtained by centrifugal collection. According to an exemplary embodiment of the present application, the reactor can be placed in a tubular furnace for heating; for example, heated to 120°C at a heating rate of 5°C / min; kept warm for 24 hours, and then cooled to room temperature; the centrifugal collection process can be to take the cooled reactor out of the heating furnace and centrifuge at a certain speed (for example, 7500rpm) for collection, and the collection time can be 10 minutes.
[0062] In step S540, the first centrifugal product is purified and a second centrifugal product is obtained by centrifugal collection. According to an exemplary embodiment of the present application, in order to purify the first centrifugal product, the first centrifugal product can be washed with a DMF solution, anhydrous ethanol, and deionized water. For example, 35 mL of a DMF solution can be used to perform a first purification treatment (e.g., washing) on the first centrifugal product, the number of washings can be 3 times, the washing time for each washing can be 12 hours, and centrifugal collection is performed again after washing; next, 35 mL of anhydrous ethanol or deionized water are used to perform a second purification treatment (e.g., washing) on the centrifugal collection product to remove DMF, the number of washings can be 3 times, the washing time for each washing can be 6 hours, and centrifugal collection is performed again after washing; finally, the centrifugal collection product is dried at room temperature to obtain a second centrifugal product.
[0063] In step S550, the second centrifugal product is subjected to a carbonization doping treatment to obtain an electromagnetic absorbing material with a second microstructure. According to an exemplary embodiment of the present application, the dried second centrifugal product can be placed in a tubular furnace, and heated from room temperature to 800°C at a heating rate of 2°C / min under a protective atmosphere (e.g., an argon atmosphere), and kept at this temperature for a predetermined time (e.g., 2 hours) to perform a carbonization doping treatment. Figure 6 As shown, the present application provides a Figure 5 The electromagnetic absorbing material prepared by the method shown; Figure 5 The second microstructure finally obtained by the method shown is an electromagnetic wave absorbing material of a two-dimensional nanorod-sphere hybrid structure.
[0064] After electromagnetic performance tests, such as Figure 7 As shown, the electromagnetic absorbing material of the two-dimensional nanorod-sphere hybrid structure prepared by the method provided in the second exemplary embodiment of the present application has an effective absorbing bandwidth of 4.88 GHz and achieves a maximum return loss of -12.58 dB at 15.04 GHz, equivalent to an absorption rate of 94.48%.
[0065] Figure 8 The method flow for preparing an electromagnetic absorbing material according to the third exemplary embodiment of the present application is shown; Fig. 9 A SEM schematic diagram of an electromagnetic absorbing material according to a third exemplary embodiment of the present application is shown; Fig.10 A schematic diagram of test results of an electromagnetic absorbing material according to a third exemplary embodiment of the present application is shown.
[0066] In the third exemplary embodiment of the present application, the molar ratio of the precursor metal is set to 1:3, and the electromagnetic wave absorbing material finally prepared is an electromagnetic wave absorbing material with a three-dimensional lotus-shaped nanorod structure. Figure 8As shown, the method for preparing the electromagnetic absorbing material provided in the present application includes the following steps.
[0067] In step S810, a third molar ratio of nickel particle compound and iron particle compound is mixed into the first solution to form a first mixed solution. According to an exemplary embodiment of the present application, the third molar ratio is 1:3, the nickel particle compound can be 1.115 g of nickel nitrate hexahydrate, and the iron particle compound can be 0.422 g of ferric chloride hexahydrate; the first solution can be a solution obtained by mixing N,N-dimethylformamide (DMF)-ethanol-water in a volume ratio of 1:1:1, and the volume of the first solution can be 150 mL. According to an exemplary embodiment of the present application, in order to allow the mixed compounds to be fully mixed, they can be fully mixed by stirring (such as ultrasonic vibration), and the stirring time can be 30 minutes.
[0068] In step S820, a predetermined amount of an intermediate substance is added to the first mixed solution to form a second mixed solution. For example, the first mixed solution can be added to a reaction vessel first, and then a predetermined amount of an intermediate substance is added to the reaction vessel for thorough mixing. According to an exemplary embodiment of the present application, the intermediate substance can be dihydroxyterephthalic acid (H4DOBDC), and the amount of dihydroxyterephthalic acid (H4DOBDC) can be 0.416 g. According to an exemplary embodiment of the present application, in order to allow the mixed compounds to be fully mixed, they can be fully mixed by stirring (e.g., ultrasonic oscillation), and the stirring time can be 30 minutes. According to an exemplary embodiment of the present application, the reaction vessel can be a hydrothermal reactor.
[0069] In step S830, the second mixed solution is heated, kept warm, and cooled, and then the first centrifugal product is obtained by centrifugal collection. According to an exemplary embodiment of the present application, the reactor can be placed in a tubular furnace for heating; for example, heated to 120°C at a heating rate of 5°C / min; kept warm for 24 hours, and then cooled to room temperature; the centrifugal collection process can be to take the cooled reactor out of the heating furnace and centrifuge at a certain speed (for example, 7500rpm) for collection, and the collection time can be 10 minutes.
[0070] In step S840, the first centrifugal product is purified and a second centrifugal product is obtained by centrifugal collection. According to an exemplary embodiment of the present application, in order to purify the first centrifugal product, the first centrifugal product can be washed with a DMF solution, anhydrous ethanol, and deionized water. For example, 35 mL of a DMF solution can be used to perform a first purification treatment (e.g., washing) on the first centrifugal product, the number of washings can be 3 times, the washing time for each washing can be 12 hours, and centrifugal collection is performed again after washing; next, 35 mL of anhydrous ethanol or deionized water are used to perform a second purification treatment (e.g., washing) on the centrifugal collection product to remove DMF, the number of washings can be 3 times, the washing time for each washing can be 6 hours, and centrifugal collection is performed again after washing; finally, the centrifugal collection product is dried at room temperature to obtain a second centrifugal product.
[0071] In step S850, the second centrifugal product is subjected to a carbonization doping treatment to obtain an electromagnetic absorbing material with a third microstructure. According to an exemplary embodiment of the present application, the dried second centrifugal product can be placed in a tubular furnace, and heated from room temperature to 800°C at a heating rate of 2°C / min under a protective atmosphere (e.g., an argon atmosphere), and kept at this temperature for a predetermined time (e.g., 2 hours) to perform a carbonization doping treatment. Fig. 9 As shown, the present application provides a Figure 8 The electromagnetic absorbing material prepared by the method shown; Figure 8 The electromagnetic wave absorbing material of the third microstructure finally obtained by the method shown is an electromagnetic wave absorbing material of a three-dimensional lotus-shaped nanorod structure.
[0072] After electromagnetic performance tests, such as Fig.10 As shown, the electromagnetic absorbing material with a three-dimensional lotus-shaped nanorod structure prepared by the method provided in the third exemplary embodiment of the present application can achieve broadband absorption with an effective bandwidth of 5.09 GHz when the thickness is only 1.6 mm, and the maximum return loss at a frequency of 15.20 GHz is -16.04 dB, equivalent to an absorption rate of 97.51%.
[0073] According to the preparation method of electromagnetic absorbing material provided by the present application, by adjusting the molar ratio of nickel and iron in the precursor, a controllable multidimensional microstructure electromagnetic absorbing material from zero-dimensional nanospheres to three-dimensional lotus-shaped nanorods can be obtained. Among them, the electromagnetic absorbing material with a three-dimensional lotus-shaped nanorod structure can form more conductive networks and achieve a wider absorption bandwidth; after electromagnetic performance testing, the three-dimensional lotus-shaped nanorod structure electromagnetic absorbing material can achieve broadband absorption with an effective bandwidth of 5.09GHz when the thickness is only 1.6 mm, and the maximum return loss at a frequency of 15.20GHz is -16.04dB, which is equivalent to an absorption rate of 97.51%. The electromagnetic absorbing material with a two-dimensional nanosphere-rod hybrid structure has an effective absorption bandwidth of 4.88GHz, and achieves a maximum return loss of -12.58dB at 15.04GHz, which is equivalent to an absorption rate of 94.48%. In addition, the electromagnetic absorbing material with a zero-dimensional nanosphere structure can provide more defect sites, achieve higher reflection loss, and show strong high return loss capability; the maximum reflection loss of the electromagnetic absorbing material with a zero-dimensional nanosphere structure is -34.29dB at 17.12GHz, the absorption rate is 99.96%, and the effective absorption bandwidth is 3.30GHz.
[0074] The electromagnetic absorbing material prepared by the method provided in the present application has a microwave absorption capacity that exceeds that of ordinary carbon-based and metal-based absorbing materials, and can be suitable for the actual needs of thin thickness and broadband absorption. In addition, the electromagnetic absorbing material can be customized by controlling the microstructure to meet specific performance requirements.
[0075] The embodiments of the present application are described in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and its core idea of the present application. At the same time, changes or deformations made by those skilled in the art based on the ideas of the present application, the specific implementation methods and the scope of application of the present application, all belong to the scope of protection of the present application. In summary, the content of this specification should not be construed as a limitation on the present application.
Claims
1. A method for preparing an electromagnetic absorbing material, characterized in that: include: Mixing a nickel particle compound and an iron particle compound in a set molar ratio into the first solution to form a first mixed solution; adding a predetermined amount of an intermediate substance to the first mixed solution to form a second mixed solution; Heating, keeping warm and cooling the second mixed solution, and collecting by centrifugation to obtain a first centrifugal product; Purifying the first centrifugal product and collecting it by centrifugation to obtain a second centrifugal product; The second centrifugal product is subjected to a carbonization and doping treatment to obtain an electromagnetic wave absorbing material with a microstructure.
2. The method according to claim 1, characterized in that The set molar ratio includes 3:1, and the electromagnetic absorbing material includes an electromagnetic absorbing material with a zero-dimensional nanosphere structure.
3. The method according to claim 1, characterized in that The set molar ratio includes 2:2, and the electromagnetic absorbing material includes an electromagnetic absorbing material with a two-dimensional nanosphere-rod hybrid structure.
4. The method according to claim 1, characterized in that: The set molar ratio includes 1:3, and the electromagnetic absorbing material includes an electromagnetic absorbing material with a three-dimensional lotus-shaped nanorod structure.
5. The method according to any one of claims 1 to 4, characterized in that The nickel particle compound includes nickel nitrate hexahydrate, the iron particle compound includes ferric chloride hexahydrate, the first solution includes a mixed solution of N,N-dimethylformamide-ethanol-water with a volume ratio of 1:1:1, and the intermediate substance includes dihydroxyterephthalic acid.
6. The method according to any one of claims 1 to 4, characterized in that The heating, heat preservation and cooling of the second mixed solution comprises: The second mixed solution was heated to 120° C. at a heating rate of 5° C. / min, and cooled to room temperature after being kept at this temperature for 24 h.
7. The method according to any one of claims 1 to 4, characterized in that The purification process comprises: Washing the first centrifugal product with N,N-dimethylformamide solution, anhydrous ethanol and deionized water respectively; The washing is performed 3 times, and the washing time for each time is 12 hours.
8. The method according to any one of claims 1 to 4, characterized in that The carbonization doping process comprises: Under a protective atmosphere, the second centrifugal product is heated from room temperature to a set temperature at a set heating rate, and kept warm for a predetermined time.
9. The method according to claim 8, characterized in that The protective atmosphere includes an argon atmosphere, the set heating rate includes 2° C. / min, the set temperature includes 800° C., and the predetermined time includes 2 hours.
10. An electromagnetic absorbing material prepared by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Porous carbon-based electromagnetic absorbing agent and preparation method thereof
CN108521754A