CoNi / C nanofiber with adjustable high electromagnetic wave absorption performance and preparation method thereof
Magnetic CoxNiy/C nanofibers are prepared through electrospinning technology, which solves the problem of poor performance of existing electromagnetic wave absorption materials, and achieves low density, high absorption performance and wide bandwidth electromagnetic wave absorption effect, which is suitable for industrial production and a variety of applications Scene.
Patent Information
- Application Number
- CN202211721561.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The existing electromagnetic wave absorption materials have poor performance, insufficient maximum reflection loss value and narrow effective absorption bandwidth, which cannot meet the needs of high-performance electromagnetic wave absorption.
Electrospinning technology is used to prepare magnetic CoxNiy/C nanofibers. By precisely controlling the calcining temperature and time, the CoNi alloy and carbon nanofibers achieve optimal adaptation, achieving synergistic effects and impedance matching of the electrical/magnetic components.
It has achieved low density, high absorption performance and significantly increased effective absorption bandwidth, and has the potential to become a new high-efficiency microwave absorber. The preparation method is simple to operate and low cost, which is suitable for large-scale industrial production.
Smart Images

Figure CN116145288B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of materials and relates to electromagnetic wave absorbing materials, and in particular to a magnetic metal oxide / carbon composite absorbing material with adjustable high electromagnetic wave absorption performance and a preparation method thereof. Background Art
[0002] With the rapid development of electronic devices and the widespread application of wireless communications, electromagnetic interference pollution has become a serious problem. Electromagnetic radiation not only interferes with the function of equipment, but also poses a threat to human health. At the same time, stealth aircraft play an increasingly important role in military penetration and active attacks. Based on this, the research on electromagnetic wave absorbing materials has received widespread attention, and the performance requirements of materials are becoming higher and higher. Magnetic metals (such as Co, Ni, Fe) not only have the advantages of high magnetic permeability, high saturation magnetization and high Snoke limit, but also have low cost and excellent magnetic loss performance. It has broad application prospects in absorbing materials. Carbon materials have good chemical stability and thermal stability, excellent dielectric properties and low density. Optimizing the composite of magnetic materials and carbon materials can not only overcome the defects of high density of magnetic materials, but also improve electromagnetic matching and synergistic effects, and achieve better electromagnetic wave absorption than single absorbing materials.
[0003] However, only by reasonably balancing the magnetic components and dielectric components of magnetic materials / carbon nanomaterials can the synergistic effect of magnetic loss and dielectric loss be achieved, and ideal impedance matching can be achieved to meet the high performance requirements of electromagnetic wave absorbing materials. Jiang Qiaorong et al. from Xiamen University used 1,2-propylene glycol as a reducing agent and hydrothermally synthesized cobalt chloride hexahydrate and nickel chloride hexahydrate at 170°C to form a chain CoNi alloy structure. However, the material has too strong dielectric loss capacity, resulting in a maximum reflection loss value of -6dB, and only weak wave absorption performance. Zhou Suhua et al. from Northwestern Polytechnical University prepared CoNi alloy nanoparticles by dissolving cobalt acetate tetrahydrate and nickel acetate tetrahydrate in ethylene glycol using a hydrothermal method. The maximum reflection loss of the material reached -30.4dB, but the effective absorption bandwidth was only 1.9GHz, which still could not meet the wide absorption requirements of wave absorbing materials. Therefore, pursuing the matching of electric / magnetic components to prepare high-performance electromagnetic wave absorbing materials has always been a difficult problem faced by researchers. At present, there are no reports on the preparation of high-performance electromagnetic wave absorbing materials. Summary of the invention
[0004] In view of the problem that the electromagnetic wave absorption material in the prior art has poor performance, the present invention provides a magnetic Co with adjustable high electromagnetic wave absorption performance. x Ni y / C nanofiber composite absorbing material and preparation method thereof. The composite absorbing material of the present invention not only has low density and strong absorbing performance, but also has a significantly increased effective absorption bandwidth, and has the potential to become a new type of high-efficiency microwave absorber. In addition, the preparation method provided by the present invention is simple to operate, low in cost, suitable for industrial large-scale production, and has broad commercial application prospects and economic benefit prospects.
[0005] The technical solution of the present invention is: magnetic Co with adjustable high electromagnetic wave absorption performance x Ni y A method for preparing a Co / C nanofiber (x, y represents the molar ratio of Co salt and Ni salt added during preparation), comprising the following steps:
[0006] (1) Preparation of solvent system: Weigh appropriate amounts of PAN (polyacrylonitrile) and DMF (N,N-dimethylformamide) and dissolve them in water, and stir them at a temperature of 40 to 60° C. for 8 to 12 hours to obtain a solvent system with sufficient surface tension. The weight ratio of PAN to DMF is 1.6:(15-18).
[0007] (2) Preparing a precursor solution: Weigh appropriate amounts of metal salts Ni(NO3)2·6H2O and Co(NO3)2·6H2O, add them to the solvent system prepared in step (1), and stir at room temperature for 8 to 12 hours to obtain a precursor solution. Adding metal salts to the solvent system not only provides nickel and cobalt sources, but also enhances the conductivity of the solution, which is beneficial for the high-voltage electric field of subsequent electrospinning to overcome the surface tension of the polymer nano-solution, making the spun fibers fluffy and filamentous.
[0008] The weight ratio of the metal salt to PAN is (35-75): 100. The molar ratio of Ni(NO3)2·6H2O to Co(NO3)2·6H2O in the metal salt is 3:1-1:3.
[0009] (3) Spinning: Push the precursor solution into a metal needle of 18-20G standard specification; the feed rate of the precursor solution is 0.005-0.010 mm·s -1 If the propulsion rate is too fast, the electrospun fibers will be uneven in thickness; if the propulsion rate is too slow, the nanofibers will break prematurely. Then, the fibers are spun at a DC voltage of 20 to 22 kV and a distance of 9 to 12 cm between the needle tip and the collector. The electrospun fibers are collected and dried at a temperature of 50 to 60 ° C for 6 to 10 hours to avoid adhesion between the electrospun fibers and damage to the fiber structure.
[0010] (4) Calcination: The electrospun fibers dried in step (3) were heated to 270-290°C for the first time, and pre-oxidized and calcined in an air atmosphere for 2-3 hours to stabilize the morphology of the one-dimensional carbon nanofibers. Then, the temperature was raised to 680-720°C for the second time, and calcined in a nitrogen atmosphere for 3-4 hours to fully carbonize the pre-oxidized electrospun fibers to obtain Co x Ni y / C nanofibers. The rates of the first and second heating are both 2-5℃·min -1 . First, one-dimensional nanofibers were prepared by electrospinning.
[0011] In this step, the CoNi alloy (magnetic component) and carbon nanofiber (dielectric component) of the one-dimensional magnetic nanofibers are precisely controlled to obtain the best matching electromagnetic loss capacity. The synergistic effect of the electric / magnetic components meets the impedance matching requirements of high-performance absorbing materials, thereby obtaining CoNi nanofibers with excellent microwave absorption performance. x Ni y / C nanofibers.
[0012] The CoNi / C nanofibers are prepared by the method described above. The CoNi / C nanofibers are specifically a three-dimensional network structure formed by one-dimensional nanofibers, and CoNi alloy particles are attached to the nanofibers. The CoNi / C nanofibers have ideal impedance matching, which can allow most electromagnetic waves to enter the fiber and propagate; and the three-dimensional conductive network composed of carbon fibers provides sufficient space for the reflection and scattering of electromagnetic waves, expands the propagation path of electromagnetic waves, and further enhances energy loss.
[0013] The molar ratio of Co to Ni in the nanofiber is 3:1-1:3. As the molar ratio of cobalt to nickel in the nanofiber decreases, the surface of the nanofiber tends to be smoother. The more wrinkles on the nano surface, the larger the specific surface area of the carbon fiber, which is conducive to causing multiple reflections and scattering of electromagnetic waves, extending the transmission path, and enhancing its ability to attenuate electromagnetic wave energy.
[0014] Beneficial effects of the present invention:
[0015] (1) The present invention provides a magnetic CoNi / C nanofiber composite absorbing material with adjustable electromagnetic wave absorption performance. It not only has low density and strong absorbing performance, but also has a significantly increased effective absorption bandwidth, and has the potential to become a new type of high-efficiency microwave absorber.
[0016] (2) The preparation method of the magnetic CoNi / C nanofiber composite absorbing material provided by the present invention achieves the best adapted electromagnetic loss capacity, so that the prepared composite absorbing material has excellent electromagnetic microwave absorption performance, thus having a significant improvement.
[0017] (3) The preparation method of the magnetic CoNi / C nanofiber composite absorbing material provided by the present invention is simple to operate, low in cost, and suitable for industrial mass production; and the microwave absorption performance of the material can be adjusted by changing the molar ratio of the metal, thereby adapting to different needs and being more flexible. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Attached Figure 1 This is the SEM image of Co3Ni1 / C prepared in Example 1;
[0019] Attached Figure 2 This is the SEM image of Co1Ni1 / C prepared in Example 2;
[0020] Attached Figure 3 This is the SEM image of Co1Ni3 / C prepared in Example 3;
[0021] Attached Figure 4 Co prepared in Example 1-3 x Ni y / C XRD pattern;
[0022] Attached Figure 5 This is the reflection loss spectrum of Co3Ni1 / C prepared in Example 1;
[0023] Attached Figure 6 This is the reflection loss spectrum of Co1Ni1 / C prepared in Example 2;
[0024] Attached Figure 7 This is the reflection loss spectrum of Co1Ni3 / C prepared in Example 3. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with the embodiments.
[0026] Raw materials: Nickel nitrate hexahydrate (Ni(NO3)2·6H2O), cobalt nitrate hexahydrate (Co(NO3)2·6H2O), and N,N-dimethylformamide (DMF) were all from Sinopharm Chemical Reagent Co., Ltd., and polyacrylonitrile (PAN, Mw=150000) was from Aladdin Reagent (Shanghai) Co., Ltd.
[0027] Example 1: Magnetic Co3Ni1 / C nanofibers with high electromagnetic wave absorption performance
[0028] Step 1, weigh 1.6 g PAN and 16 g DMF, mix them, and stir them magnetically at 40°C for 12 h. Then, weigh 1 mmol Ni(NO3)2·6H2O and 3 mmol Co(NO3)2·6H2O, add them to the solution, mix them, and continue stirring for 12 h.
[0029] Step 2: The obtained precursor solution is loaded into a syringe and pushed into a 20G standard metal needle through the syringe at a feed rate of 0.010 mm·s -1 At the same time, under a DC voltage of 21 kV, the distance between the needle tip of the syringe and the collector was 12 cm, and the collected electrospun fibers were dried at 50-60°C for 10 h.
[0030] Step 3, the dried electrospun fiber was calcined in air at 290°C for 3 h, and then calcined in a nitrogen atmosphere at 720°C for 4 h to obtain a product labeled Co3Ni1 / C (3, 1 indicates that the molar ratio of Co salt to Ni salt added during preparation is 3:1), and the heating rate was 2-5°C·min -1 .
[0031] Step 4, weigh the obtained Co3Ni1 / C to be 0.62 g.
[0032] Comparative Example 1:
[0033] Different from Example 1, the solvent and the metal salt are added together and mixed.
[0034] Step 1, weigh 1.6 g PAN, 16 g DMF, 1 mmol Ni(NO3)2·6H2O and 3 mmol Co(NO3)2·6H2O, mix them, and stir them magnetically at 40°C for 12 h.
[0035] Step 2: The obtained precursor solution is loaded into a syringe and pushed into a 20G standard metal needle through the syringe at a feed rate of 0.010 mm·s -1 At the same time, under a DC voltage of 21 kV, the distance between the needle tip of the syringe and the collector was 12 cm, and the collected electrospun fibers were dried at 50-60°C for 10 h.
[0036] Step 3, calcining the dried electrospun fiber in air at 290°C for 3 h, and then calcining it in a nitrogen atmosphere at 720°C for 4 h. To distinguish it from Example 1, the obtained product is labeled as Co3Ni1 / C-1, and the heating rate is 2-5°C·min -1 .
[0037] Step 4: The mass of the obtained Co3Ni1 / C-1 is weighed to be 0.33 g. Compared with Example 1, the yield is reduced by nearly 47%.
[0038] Example 2: Magnetic Co1Ni1 / C nanofibers with high electromagnetic wave absorption performance
[0039] Step 1, weigh 1.6 g PAN and 18 g DMF, mix them, and stir them magnetically at 50°C for 10 h. Then, weigh 1 mmol Ni(NO3)2·6H2O and 1 mmol Co(NO3)2·6H2O, add them to the solution, mix them, and continue stirring for 10 h.
[0040] Step 2: The obtained precursor solution is loaded into a syringe and pushed into a 19G standard metal needle through the syringe at a feed rate of 0.008 mm·s -1 At the same time, under a DC voltage of 21 kV, the distance between the needle tip of the syringe and the collector was 11 cm, and the collected electrospun fibers were dried at 50-60°C for 8 h.
[0041] Step 3, calcining the dried electrospun fiber in air at 280°C for 2.5 h, and then calcining it in nitrogen atmosphere at 700°C for 3.5 h, to obtain a product labeled Co1Ni1 / C (1, 1 indicates that the molar ratio of Co salt to Ni salt added during preparation is 1:1), and the heating rate is 2-5°C·min -1 .
[0042] Step 4, weigh the obtained Co1Ni1 / C to be 1.25 g.
[0043] Comparative Example 2:
[0044] Different from Example 2, the solvent and the metal salt are added together and mixed.
[0045] Step 1, weigh 1.6 g PAN, 18 g DMF, 1 mmol Ni(NO3)2·6H2O and 1 mmol Co(NO3)2·6H2O, mix them, and stir them magnetically at 50°C for 10 h.
[0046] Step 2: The obtained precursor solution is loaded into a syringe and pushed into a 19G standard metal needle through the syringe at a feed rate of 0.008 mm·s -1 At the same time, under a DC voltage of 21 kV, the distance between the needle tip of the syringe and the collector was 11 cm, and the collected electrospun fibers were dried at 50-60°C for 8 h.
[0047] Step 3, calcining the dried electrospun fiber in air at 280°C for 2.5 h, and then calcining it in a nitrogen atmosphere at 700°C for 3.5 h. In order to distinguish it from Example 2, the obtained product is marked as Co1Ni1 / C-1, and the heating rate is 2-5°C·min -1 .
[0048] Step 4: The mass of the obtained Co1Ni1 / C-1 is weighed to be 0.54 g. Compared with Example 2, the yield is reduced by nearly 57%.
[0049] Example 3: Magnetic Co1Ni3 / C nanofibers with high electromagnetic wave absorption performance
[0050] Step 1, weigh 1.6 g PAN and 17 g DMF, mix them, and stir them magnetically at 60°C for 8 h. Then, weigh 3 mmol Ni(NO3)2·6H2O and 1 mmol Co(NO3)2·6H2O, add them to the solution, mix them, and continue stirring for 8 h.
[0051] Step 2: The obtained precursor solution is loaded into a syringe and pushed into a 18G standard metal needle through the syringe at a feed rate of 0.006 mm·s -1 At the same time, under a DC voltage of 20 kV, the distance between the needle tip of the syringe and the collector was 9 cm, and the collected electrospun fibers were dried at 50-60°C for 6 h.
[0052] Step 3, calcining the dried electrospun fiber in air at 270°C for 2 h, and then calcining it in a nitrogen atmosphere at 680°C for 3 h, to obtain a product labeled Co1Ni3 / C (1, 3 indicates that the molar ratio of Co salt to Ni salt added during preparation is 1:3), and the heating rate is 2-5°C·min -1 .
[0053] Step 4, weigh the mass of the obtained Co1Ni3 / C to be 0.98 g.
[0054] Comparative Example 3:
[0055] Different from Example 3, the solvent and the metal salt are added together and mixed.
[0056] Step 1, weigh 1.6 g PAN, 17 g DMF, 3 mmol Ni(NO3)2·6H2O and 1 mmol Co(NO3)2·6H2O, mix them, and stir them magnetically at 60°C for 8 h.
[0057] Step 2: The obtained precursor solution is loaded into a syringe and pushed into a 18G standard metal needle through the syringe at a feed rate of 0.006 mm·s -1 At the same time, under a DC voltage of 20 kV, the distance between the needle tip of the syringe and the collector was 9 cm, and the collected electrospun fibers were dried at 50-60°C for 6 h.
[0058] Step 3, the dried electrospun fiber was calcined in air at 270°C for 2 h, and then calcined in a nitrogen atmosphere at 680°C for 3 h. To distinguish it from Example 3, the obtained product was labeled Co1Ni3 / C-1, and the heating rate was 2-5°C·min -1 .
[0059] Step 4: The mass of the obtained Co1Ni3 / C-1 is weighed to be 0.48 g. Compared with Example 3, the yield is reduced by nearly 51%.
[0060] By comparing Examples 1-3 and Comparative Examples 1-3, it can be seen that the operating steps of first mixing PAN and DMF until the surface tension is sufficient and then adding the metal salt to continue mixing in the present application greatly improve the yield, produce unexpected technical effects, and are non-obvious.
[0061] Example 4: Co prepared in Examples 1-3 x Ni y Characterization of C nanofibers
[0062] 1. SEM Characterization
[0063] The samples were placed on a silicon wafer and the microstructure of the samples was observed using a scanning electron microscope (SEM, Sigma 300). Figure 1 As shown, the Co3Ni1 / C prepared in Example 1 presents a three-dimensional network structure consisting of uniform nanofibers with an average diameter of 1.5 μm. The surface of the nanofibers is wrinkled and CoNi alloy particles are attached to them.
[0064] like Figure 2 As shown, the Co1Ni1 / C prepared in Example 2 presents a three-dimensional network structure composed of uniform nanofibers with an average diameter of 1.5 μm. The surface of the nanofibers has clear stripes and CoNi alloy particles attached thereto.
[0065] like Figure 3 As shown, the Co1Ni3 / C prepared in Example 3 presents a three-dimensional network structure consisting of uniform nanofibers with an average diameter of 1.5 μm. The surface of the nanofibers is smooth, and CoNi alloy particles are attached to them.
[0066] In summary, the structures of the CoNi / C nanofibers prepared in Examples 1-3 are all three-dimensional network structures composed of one-dimensional nanofibers, and CoNi alloy particles are attached to the nanofibers. The only difference is that the surface morphology of the nanofibers is different. As the cobalt-nickel molar ratio decreases, the surface of the nanofibers tends to be smooth. The more wrinkles on the nano surface, the larger the specific surface area of the carbon fiber, which is conducive to causing multiple reflections and scattering of electromagnetic waves, extending the transmission path, and enhancing the ability of its electromagnetic wave energy attenuation. In addition, the three-dimensional conductive network composed of carbon fibers provides enough space for the reflection and scattering of electromagnetic waves, expands the propagation path of electromagnetic waves, and further enhances energy loss.
[0067] 2. XRD pattern
[0068] The samples were made into powders and used for X-ray diffraction (XRD, Shimadzu XRD-7000) test to obtain the crystal structure of the samples. Figure 4 Co prepared in Example 1-3 x Ni y / C nanofiber material XRD pattern.
[0069] Depend on Figure 4 It can be seen that for the Co3Ni1 / C sample prepared in Example 1, the Co1Ni1 / C sample prepared in Example 2, and the Co1Ni3 / C sample prepared in Example 3, there are peaks at 2θ=25°, which is due to the synthesis of amorphous C. Among them, for the Co1Ni1 / C sample prepared in Example 2, the peak at 2θ=25° is the strongest, indicating that it has the most amorphous C. The inventors speculate that this may lead to its relatively weak microwave absorption performance. In addition, for the samples prepared in Examples 1-3, they all have characteristic peaks at 2θ=44.3°, 51.6° and 76.0°. These characteristic peaks correspond to the (111), (200) and (220) crystal planes of face-centered cubic structure Ni (JCPDS No.04-0850) and Co (JCPDS No.15-0806), respectively, which proves the synthesis of CoNi alloy in the composite material. It is precisely because of the Co prepared in this application that x Ni y The CoNi alloy in the C / C nanofiber material provides a magnetic component, which enables the synergistic effect of the dielectric and magnetic components to achieve impedance matching, thereby realizing efficient microwave absorption performance.
[0070] 3. Reflection loss spectrum
[0071] Electromagnetic parameters were measured at 2-18 GHz using a vector network analyzer (Agilent N5222A). The sample was uniformly mixed with paraffin wax (50 wt % each) and pressed into a ring to obtain a standard ring (Φ in :3.04mm,Φ out :7.00mm). The reflection loss (RL) value of the sample is calculated according to the transmission line theory, and the formula is as follows:
[0072]
[0073]
[0074] In the formula, Z0 and Z in are the free space impedance and the sample input impedance, μ r and ε rare the relative magnetic permeability and dielectric constant of the sample, respectively, d, c and f are the thickness of the sample, the speed of light in a vacuum and the microwave frequency, respectively. The lower the RL value, the better the absorbing performance. The bandwidth with an RL value lower than -10dB is called the effective absorption bandwidth. When it is less than -10dB, -20dB or -30dB, it means that 90%, 99% or more than 99.9% of the electromagnetic energy is absorbed by the absorbing material.
[0075] Figure 5 This is the reflection loss spectrum of the Co3Ni1 / C nanofiber prepared in Example 1. As can be seen from the figure, the Co3Ni1 / C nanofiber has excellent electromagnetic wave absorption performance, and when the matching thickness is 2.7mm and the frequency is 9.5GHz, the minimum reflection loss is -57.75dB, and the effective absorption bandwidth is 3.84GHz (8.10-11.94GHz).
[0076] Figure 6 This is the reflection loss spectrum of the Co1Ni1 / C nanofiber prepared in Example 2. As can be seen from the figure, the Co1Ni1 / C nanofiber has excellent electromagnetic wave absorption performance, and when the matching thickness is 2.7mm and the frequency is 12.0GHz, the minimum reflection loss is -42.52dB, and the effective absorption bandwidth is 5.14GHz (9.80-14.94GHz).
[0077] Figure 7 This is the reflection loss spectrum of the Co1Ni3 / C nanofiber prepared in Example 3. As can be seen from the figure, the Co1Ni3 / C nanofiber has excellent electromagnetic wave absorption performance. When the matching thickness is 2.4mm and the frequency is 13.5GHz, the minimum reflection loss is -42.24dB, and the effective absorption bandwidth is 5.86GHz (11.18-17.04GHz).
[0078] Depend on Figure 5-7 It can be seen that from Co3Ni1 / C nanofibers, Co1Ni1 / C nanofibers to Co1Ni3 / C nanofibers, as the proportion of cobalt salt decreases, the minimum reflection loss value gradually moves to high frequency, from 9.5GHz to 13.5GHz; and the effective absorption bandwidth increases from 3.84GHz to 5.86GHz, which is significantly widened. This shows that the one-dimensional magnetic Co prepared by the present invention x Ni y / C nanofiber not only has a minimum reflection loss value of -57.75dB and an effective absorption bandwidth of up to 5.86GHz, but also has excellent electromagnetic wave absorption performance; and the absorption performance can be adjusted by adjusting the ratio of cobalt salt and nickel salt. It is flexible in practical applications and can adapt to various application scenarios.
[0079] In summary, the Co prepared by the method described in this applicationx Ni y / C nanofibers have ideal impedance matching, so most electromagnetic waves can enter the fiber and propagate; the minimum reflection loss value can reach -57.75dB, and the widest effective absorption bandwidth can reach 5.86GHz, which has excellent electromagnetic wave absorption performance. In addition, the inventor unexpectedly discovered that by adjusting the ratio of cobalt salt and nickel salt, the structure of the nanofiber changes, thereby achieving flexible adjustment of the wave absorption performance, and has broad application prospects.
Claims
1. A method for preparing magnetic CoNi / C nanofibers with adjustable high electromagnetic wave absorption performance; characterized in that: The following steps are involved: (1) Preparation of solvent system: Weigh appropriate amounts of PAN and DMF and dissolve them in water. Stir for 8 to 12 hours at a temperature of 40 to 60 °C to obtain a solvent system with sufficient surface tension. (2) Preparing a precursor solution: Weigh appropriate amounts of metal salts Ni(NO3)2•6H2O and Co(NO3)2•6H2O, add them to the solvent system prepared in step (1), and stir at room temperature for 8-12 h to obtain a precursor solution; the weight ratio of the metal salt to PAN is (35-75):100, and the molar ratio of Ni(NO3)2•6H2O to Co(NO3)2•6H2O in the metal salt is 3:1-1:3; (3) Spinning: Push the precursor solution into a 18-20 G standard metal needle; spin at a DC voltage of 20-22 kV and a distance of 9-12 cm between the needle tip and the collector; collect the electrospun fibers and dry them at 50-60 °C for 6-10 h; (4) Calcination: The electrospun fibers dried in step (3) are heated to 270-290°C for the first time and calcined in an air atmosphere for 2-3 h; then heated to 680-720°C for the second time and calcined in a nitrogen atmosphere for 3-4 h to obtain Co with high electromagnetic wave absorption performance. x Ni y / C nanofibers.
2. The method for preparing magnetic CoNi / C nanofibers according to claim 1, characterized in that: The weight ratio of PAN to DMF in step (1) is 1.6:(15-18).
3. The method for preparing magnetic CoNi / C nanofibers according to claim 2, characterized in that: The feed rate of the precursor solution in step (3) is 0.005~0.010 mm·s −1 .
4. The method for preparing magnetic CoNi / C nanofibers according to claim 3, characterized in that: The rate of the first and second heating in step (4) is 2-5 °C·min -1 .
5. CoNi / C nanofibers prepared by the method according to any one of claims 1 to 4.
6. The CoNi / C nanofiber according to claim 5, characterized in that: The CoNi / C nanofibers are specifically a three-dimensional network structure formed by one-dimensional nanofibers, and CoNi alloy particles are attached to the nanofibers.
7. The CoNi / C nanofiber according to claim 6, characterized in that: The molar ratio of Co to Ni in the nanofibers is 3:1-1:3.
Citation Information
Patent Citations
Co / C composite nanofiber microwave absorbent, and preparation method and application thereof
CN103422193A
Ni / C composite nanofiber microwave absorbent, preparation method and application of absorbent
CN103436996A
Magnetic ferrite carbon-based nanofiber wave-absorbing material, preparation method and application
CN113026148A