Steel and mold

By optimizing the steel composition, especially by increasing the Mo content, decreasing the Si content, and controlling the Mn/Cr ratio, the problems of hot cracking and large cracks in large-size molds were solved, achieving high manufacturability and machinability, improving impact value and fracture toughness, and extending creep rupture time.

CN118996285AInactive Publication Date: 2024-11-22DAIDO STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410615473.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-17
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies struggle to prevent thermal cracking and large cracks when manufacturing large-sized molds, while maintaining the manufacturability and machinability of the steel.

Method used

By optimizing the composition of steel, controlling the content of elements such as C, V, Mn, Cr, Mo, and Si, increasing the Mo content, decreasing the Si content, and optimizing the Mn/Cr ratio, high hardenability and resistance to softening are ensured, the formation of residual austenite is prevented, and thermal conductivity and resistance to hot cracking are improved.

Benefits of technology

It effectively prevents the occurrence of hot cracks and large cracks in large-size molds, maintains excellent manufacturability and machinability, extends creep rupture time, improves impact value and fracture toughness, and ensures high-temperature tensile strength and softening resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996285A_ABST
    Figure CN118996285A_ABST
Patent Text Reader

Abstract

The present invention relates to a steel material comprising: 0.23 mass% < = C < = 0.39 mass%; 0.03 mass% < = V < = 0.30 mass%; 6.60 mass% < = Mn + Cr < = 7.40 mass%; mn / Cr < = 0.150; mn > = 0.60 mass%; cr < = 6.60 mass%; cu + Ni < = 0.84 mass%; 0.01 mass% < = Si < = 0.40 mass%; 2.00 mass% < = Mo < = 3.50 mass%; 0.001% by mass < = Al < = 0.080% by mass; and 0.003 mass% < = N < = 0.040 mass%, with the balance being Fe and unavoidable impurities.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a steel material and a mold, and more particularly to a steel material suitable for manufacturing a large-mass and large-size mold and a mold using the steel material. Background Art

[0002] Since stress and heat are repeatedly applied to the mold during use, mold steel is required to have a variety of excellent properties, such as hardness, impact resistance, thermal crack resistance, and wear resistance. Therefore, various proposals have been made in the prior art regarding steels having these properties.

[0003] For example, Patent Document 1 discloses a hot working tool steel including predetermined contents of C, Si, Mn, Cr, Mo, and V, with the balance being Fe and inevitable impurities.

[0004] The manufacturing process of the mold includes a hardening and tempering (abbreviated as HT) method and a pre-hardening (abbreviated as PH) method. The HT method is a method of giving the mold the required hardness and toughness "after" machining. On the other hand, the PH method is a method of giving the mold the required hardness and toughness "before" machining.

[0005] In the case of using any one of the HT method and the PH method to manufacture a mold, the larger the size of the mold, the more likely it is to generate heat checks and large cracks. This is believed to be because the cooling rate during quenching decreases as the size of the mold increases, and the high-temperature strength and toughness of the steel material decrease. It is also because the larger the size of the mold, the greater the thermal and mechanical stresses acting on the mold during use.

[0006] On the other hand, the manufacturability (spheroidizing annealing (SA) performance, machinability) of steel materials that hardly generate hot cracks or large cracks is generally low in many cases. In addition, there has been no example of a steel material that can prevent hot cracks or large cracks without significantly impairing manufacturability even when applied to a large-sized mold.

[0007] Patent Document 1: JP2011-001572A Summary of the invention

[0008] An object of the present invention is to provide a steel material capable of manufacturing a mold excellent in durability (thermal crack resistance and / or macrocrack resistance) without significantly impairing manufacturability (SA performance and / or machinability).

[0009] In order to solve the above problems, the steel material according to the present invention comprises:

[0010] 0.23 mass%≤C≤0.39 mass%;

[0011] 0.03 mass%≤V≤0.30 mass%;

[0012] 6.60 mass%≤Mn+Cr≤7.40 mass%;

[0013] Mn / Cr≤0.150;

[0014] Mn ≥ 0.60 mass%;

[0015] Cr≤6.60 mass%;

[0016] Cu+Ni≤0.84 mass%;

[0017] 0.01 mass%≤Si≤0.40 mass%;

[0018] 2.00 mass%≤Mo≤3.50 mass%;

[0019] 0.001 mass % ≤ Al ≤ 0.080 mass %; and

[0020] 0.003 mass%≤N≤0.040 mass%,

[0021] The balance is Fe and inevitable impurities.

[0022] The mold according to the present invention is manufactured from the steel material according to the present invention and has a mass of more than 2000 kg.

[0023] In the present invention, the Si content and the Mo content are optimized to a steel material with low Si and high Mo, so that macro cracks and hot cracks can be prevented even when the mass or size of the steel material is large. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is a schematic diagram of the effect obtained by increasing the Mo content and reducing the Si content.

[0025] Figure 2 This is a graph showing the ranges of the Mn content and the Cr content for obtaining a steel material excellent in SA performance and hardenability.

[0026] Figure 3 It is a graph showing the relationship between the amount of retained austenite and the Mo content.

[0027] Figure 4 It is a graph showing the relationship between creep rupture time and Mo content.

[0028] Figure 5It is a graph showing the relationship between fracture toughness and Si content.

[0029] Figure 6 It is a graph showing the relationship between high temperature tensile strength and Si content.

[0030] Figure 7 is a graph showing the relationship between softening resistance and Si content.

[0031] Figure 8 This is a graph showing the relationship between the critical cooling rate for pearlite precipitation and the Si content.

[0032] Fig. 9 is a diagram showing the temperature transition of the central portion of the block during rapid cooling.

[0033] Fig.10 It is a diagram showing a quenching simulation of a 12.5-ton SKD61 block.

[0034] Hereinafter, embodiments of the present invention will be described in detail. DETAILED DESCRIPTION

[0035] 1. Steel

[0036] 1.1. Composition

[0037] 1.1.1. Main components

[0038] The steel material according to the present invention contains the following elements, with the balance being Fe and inevitable impurities. The types of the added elements, their composition ranges, and the reasons for their limitations are as follows.

[0039] (1) 0.23 mass% ≤ C ≤ 0.39 mass%:

[0040] Fine particles (carbides, carbonitrides) with a diameter of 0.5 μm or less act as "pinning particles" that prevent austenite grains from growing during quenching heating. In the case where the C content is too small, the amount of pinning particles during quenching heating becomes insufficient. As a result, the grains may become coarser, and steel properties such as impact value, fracture toughness value, and ductility may deteriorate.

[0041] When the C content is too small, the martensitic transformation start temperature (Ms point) becomes too high. As a result, the hardenability is improved, but the impact value may be reduced.

[0042] In addition, when the C content is too little, it is difficult to obtain a hardness of 45HRC or more by tempering at 560°C to 600°C. In order to ensure high thermal crack resistance, a hardness of 45HRC or more is required. When the C content is too little, the softening resistance is reduced. Therefore, even if a hardness of 45HRC or more is obtained after quenching and tempering, the hardness will decrease during use as a mold, and the tensile strength at high temperature may decrease. In this case, (2) and (3) in Table 1 described later cannot be met.

[0043] Therefore, the C content needs to be 0.23% by mass or more. The C content is preferably 0.25% by mass or more, and more preferably 0.27% by mass or more.

[0044] On the other hand, when the C content is too high, coarse carbides or carbonitrides may crystallize during the casting process. These crystals will become "foreign matter" that reduces the impact value. Therefore, (4) in Table 1 described later is necessary. It is difficult to dissolve and eliminate coarse foreign matter by heat treatment (homogenizing heat treatment, normalizing and spheroidizing annealing). Even after quenching and tempering, coarse foreign matter is often not completely dissolved and remains. During the homogenizing heat treatment, the coarse foreign matter will dissolve and reduce in size, but coarse foreign matter with a diameter of more than 5 μm can still be observed. Foreign matter that is not completely dissolved and remains will become the starting point of fracture and lead to a decrease in impact value and fatigue strength.

[0045] In addition, in the case of forming the ingot into a block or rod-shaped steel by hot working, the impact value may decrease when the cooling rate after hot working is low. This phenomenon becomes obvious when the C content is too high. This is because carbides or carbonitrides precipitate in the austenite grain boundaries during the cooling process after hot working. These precipitates also play the role of "foreign matter" that reduces the impact value, as described in the case of the above-mentioned crystallized product. Therefore, (4) in Table 1 recorded later is necessary. These precipitates cannot be completely dissolved after hot working even after various heat treatments, and ultimately remain in the quenched and tempered structure.

[0046] Although the precipitates are not large and are less than 10 μm, multiple precipitates are spaced apart in a dot array, forming a necklace shape. The "necklace diameter (the maximum length of the area where multiple precipitates are spaced apart in a dot array)" corresponds to the coarse austenite grain size after hot working. Since the size of the coarse original austenite grains becomes the unit of the fracture surface, the impact value and fracture toughness deteriorate.

[0047] Therefore, the C content needs to be 0.39 mass% or less. The C content is preferably 0.38 mass% or less, more preferably 0.37 mass% or less, and even more preferably 0.34 mass% or less.

[0048] (2) 0.03 ≤ V ≤ 0.30 mass %:

[0049] V combines with C and / or N in steel to form carbides, carbonitrides and / or nitrides. All of these substances play a role in pinning particles. See (5) in Table 1 described later. Therefore, when the V content is too low, the amount of pinning particles during the quenching heating process is insufficient.

[0050] In the case where the V content is too low, the degree of secondary hardening during tempering is reduced. Therefore, it is difficult to obtain a hardness of 45HRC or more during tempering at 560°C to 600°C. Since the softening resistance is reduced, even if a hardness of 45HRC or more is obtained after quenching and tempering, the hardness will decrease during use as a mold, and the high-temperature tensile strength may decrease. See (2) in Table 1 described later.

[0051] Therefore, the V content needs to be 0.03% by mass or more. The V content is preferably 0.05% by mass or more, more preferably 0.07% by mass or more, and even more preferably 0.12% by mass or more.

[0052] On the other hand, when the V content is too high, coarse foreign matter increases. As described above, "foreign matter" refers to a crystal product crystallized during casting or a precipitate precipitated during cooling after hot working. Therefore, (4) in Table 1 described later is necessary.

[0053] Therefore, the V content needs to be 0.30% by mass or less. The V content is preferably 0.29% by mass or less, more preferably 0.28% by mass or less, and even more preferably 0.25% by mass or less.

[0054] (3) 6.60 mass% ≤ Mn + Cr ≤ 7.40 mass%:

[0055] Both Mn and Cr affect hardenability. When the content of Mn+Cr is too little, hardenability is insufficient. As a result, the impact value may be significantly reduced, especially inside large molds (areas with low quenching rates). Therefore, the content of Mn+Cr needs to be 6.60% by mass or more. The content of Mn+Cr is preferably 6.65% by mass or more, and more preferably 6.70% by mass or more.

[0056] On the other hand, when the content of Mn+Cr is too much, the thermal conductivity is significantly reduced. As a result, the thermal crack resistance is deteriorated due to the increase in thermal stress. Therefore, the content of Mn+Cr needs to be 7.40 mass% or less. The content of Mn+Cr is preferably 7.35 mass% or less, and more preferably 7.30 mass% or less.

[0057] (4) Mn / Cr≤0.150:

[0058] The ratio of the mass of Mn to the mass of Cr contained in the steel (Mn / Cr) affects the SA performance. When the Mn / Cr ratio is too large, the SA performance deteriorates. Therefore, in order to heat the SA at a temperature exceeding A c3 To soften the steel to below 98HRB at the point, the cooling rate needs to be less than 10°C / hour. As a result, the SA step becomes longer and productivity decreases. In the case of coarse grains and large Mn / Cr, SA failure is likely to occur. SA also has the effect of avoiding austenite memory described later. Therefore, when SA failure occurs, it may be difficult to form fine grains during quenching.

[0059] Therefore, Mn / Cr needs to be 0.150 or less. Mn / Cr is preferably 0.148 or less, and more preferably 0.145 or less.

[0060] (5) Mn ≥ 0.60 mass%:

[0061] Mn affects hardenability. In the case where the Mn content is too little, the hardenability deteriorates. In order to ensure hardenability in the case where the Mn content is low, the Cr content must be increased. However, when the Cr content is too much, the problems described later may become apparent.

[0062] Therefore, the Mn content needs to be 0.60 mass% or more. The Mn content is preferably 0.62 mass% or more, more preferably 0.65 mass% or more, and even more preferably 0.69 mass% or more. The Mn content is preferably 0.90 mass% or less.

[0063] (6) Cr≤6.60 mass%:

[0064] In the case where the Cr content is too much, the softening resistance is reduced. That is, when the mold surface in contact with the molten metal is heated to a high temperature during use as a die casting mold, the mold surface heated to a high temperature may soften. In the case where the high temperature strength is reduced due to softening, the heat crack resistance will also deteriorate. The softening of the area where the hardness exceeds the maximum value is significant, and it is difficult to adjust the tempering hardness. This is because the hardness is sensitive to changes in the furnace temperature.

[0065] In the case where the Cr content is too much, thermal conductivity decreases. As a result, thermal stress increases and thermal crack resistance deteriorates. In addition, in the case where the Si content is 0.50 mass % or less, when the Cr content increases, machinability decreases significantly.

[0066] Therefore, the Cr content needs to be 6.60 mass% or less. The Cr content is preferably 6.55 mass% or less, more preferably 6.50 mass% or less, and even more preferably 6.40 mass% or less. The Cr content is preferably 6.00 mass% or more.

[0067] As described above, by optimizing the content of Mn+Cr, Mn / Cr, Mn content and Cr content, a finer structure can be obtained. Figure 2 .

[0068] (7) Cu+Ni≤0.84 mass%:

[0069] As described above, in the present invention, SA performance, hardenability and softening resistance are ensured by the balance between Cr and Mn (Cr content, Mn content, Mn+Cr content and Mn / Cr ratio). On the other hand, Cu and Ni both have the effect of improving hardenability, but will deteriorate SA performance. In addition, Cu and Ni have no significant effect on softening resistance, but have a significant negative impact on SA performance. When the Cu content is greater than the Ni content, hot workability deteriorates. Therefore, the total content of Cu and Ni is limited, and the upper limit of the total content is limited to a range with a small impact on hardenability or SA performance.

[0070] Therefore, the content of Cu+Ni needs to be below 0.84 mass %. Since the content of Mn+Cr for ensuring hardenability is above 6.60 mass %, it is obvious that when the content of Cu+Ni is below 0.84 mass %, hardenability will not be significantly affected. The content of Cu+Ni is preferably below 0.78 mass %, and more preferably below 0.72 mass %. The content of Cu+Ni is preferably above 0.10 mass %.

[0071] (8) 0.01 mass%≤Si≤0.40 mass%:

[0072] In the case where the Si content is too small, the machinability is reduced, and it is difficult to stably process large molds industrially. In particular, since the steel material of the present invention is intended for use in manufacturing large molds, the amount to be cut is large, and good machinability is required. Therefore, the Si content needs to be 0.01 mass% or more. The Si content is preferably 0.03 mass% or more, more preferably 0.05 mass% or more, and even more preferably 0.15 mass% or more.

[0073] On the other hand, when the Si content is too much, coarse foreign matter may increase. This tendency is obvious when the C content, V content and N content are large. Pearlite is easily precipitated during quenching cooling. In addition, when the Si content is too much, the thermal conductivity is significantly reduced. Therefore, the Si content needs to be 0.40 mass % or less. The Si content is preferably 0.37 mass % or less, more preferably 0.35 mass % or less, and even more preferably 0.33 mass % or less.

[0074] (9) 2.00 mass% ≤ Mo ≤ 3.50 mass%:

[0075] When the Mo content is too little, pearlite is easily precipitated during the quenching cooling process. The degree of secondary hardening during the tempering process will also be reduced. Therefore, when the Mo content is too little, it is difficult to obtain a hardness of 45HRC or more during the tempering process of 560°C to 600°C. In addition, softening resistance and high temperature strength may be insufficient, and thermal crack resistance may deteriorate. In addition, when the quenching rate is low, the amount of retained austenite increases. When the Mo content is too little, the creep strength is also reduced. Therefore, the Mo content needs to be 2.00% by mass or more. The Mo content is preferably 2.05% by mass or more, more preferably 2.10% by mass or more, and even more preferably 2.30% by mass or more.

[0076] On the other hand, when the Mo content is too much, the machinability is reduced. In particular, when the Si content is small, when the Mo content is too much, the machinability is significantly reduced. When the Mo content is too much, the fracture toughness may be reduced. This tendency is obvious when the Si content is large. Therefore, the Mo content needs to be 3.50 mass% or less. The Mo content is preferably 3.40 mass% or less, more preferably 3.25 mass% or less, and even more preferably 3.10 mass% or less.

[0077] (10) 0.001 mass% ≤ Al ≤ 0.080 mass%:

[0078] In the steel material according to the present invention, the C content and the V content are much less than those in the hot working die steel (SKD61 according to JIS G4404:2015) in the prior art. Therefore, the contents of V-based carbides, carbonitrides, and nitrides that serve as pinning particles during quenching heating are less than those in SKD61. Therefore, in the present invention, AlN particles are also used to prevent the growth of austenite grains. See (5) in Table 1 shown later.

[0079] When the Al content is too little, it is difficult to reduce oxygen during the refining process, and the amount of oxide increases, which may reduce the impact value. When the Al content is too little, the amount of AlN used as pinning particles is insufficient. As a result, the austenite grains may coarsen during the quenching heating process, and the impact value, fracture toughness and / or ductility may decrease. Therefore, the Al content needs to be 0.001% by mass or more. The Al content is preferably 0.002% by mass or more, and more preferably 0.003% by mass or more.

[0080] On the other hand, in the case where the Al content is too much, coarse alumina particles may increase, whereby the impact value and fatigue strength may decrease. Thermal conductivity may decrease, and thermal crack resistance may deteriorate. Therefore, the Al content needs to be 0.080 mass % or less. The Al content is preferably 0.070 mass % or less, and more preferably 0.060 mass % or less.

[0081] Note that in the case of Ca addition to improve machinability, the Al content is extremely important to optimize the form of the compound.

[0082] (11) 0.003 mass% ≤ N ≤ 0.040 mass%:

[0083] In the steel material according to the present invention, the C content and the V content are much less than those in the hot working die steel (SKD61) in the prior art. Therefore, the content of V-based carbides used as pinning particles during quenching heating is less than that in SKD61. Therefore, in the present invention, N is added to increase the content of V-based carbides, carbonitrides and nitrides used as pinning particles, thereby preventing the growth of austenite grains. By adding N, AlN can also be used as pinning particles. See (5) in Table 1 shown later.

[0084] When the N content is too low, the amount of AlN used as pinning particles is insufficient. As a result, the austenite grains coarsen during the quenching heating process, and the impact value, fracture toughness value and / or ductility may be reduced. When the N content is too low, the content of V-based carbonitrides and nitrides, which are also used as pinning particles, may be insufficient. Therefore, the N content needs to be 0.003 mass % or more. The N content is preferably 0.004 mass % or more, more preferably 0.005 mass % or more, and even more preferably 0.007 mass % or more.

[0085] On the other hand, in order to add N to an amount exceeding the amount that can be adjusted in normal refining, it is necessary to actively add N using special equipment, which increases the material cost. In the case of excessive N content, the crude crystalline product may increase. See (4) in Table 1 described later. This trend is obvious when the C content, Si content and V content are large. In addition, in the case of excessive N content, the amount of coarse AlN may be too large and the impact value may be reduced. Therefore, the N content needs to be less than 0.040 mass %. The N content is preferably less than 0.038 mass %, more preferably less than 0.036 mass %, and even more preferably less than 0.020 mass %.

[0086] (12) Unavoidable impurities:

[0087] The steel according to the present invention may contain inevitable impurities. The elements that can be included as impurities in the steel according to the present invention and their contents are as follows. P ≤ 0.03 mass%, S ≤ 0.006 mass%, O ≤ 0.006 mass%, W ≤ 0.30 mass%, Co ≤ 0.30 mass%, B ≤ 0.0002 mass%, Nb ≤ 0.004 mass%, Ta ≤ 0.004 mass%, Ti ≤ 0.004 mass%, Zr ≤ 0.004 mass%, Ca ≤ 0.0005 mass%, Se ≤ 0.03 mass%, Te ≤ 0.005 mass%, Bi ≤ 0.01 mass%, Pb ≤ 0.03 mass% and Mg ≤ 0.02 mass%.

[0088] In the present invention, "content" means "average element content of the steel", including parts with high segregation, parts with low segregation and parts with average segregation. Examples of methods for evaluating element content include (a) a method of analyzing the steel by dissolving a predetermined mass of the steel in an acid (preferably 1 g or more for each element analysis), and (b) a method of irradiating the surface of the steel with X-rays.

[0089] 1.1.2. Minor constituent elements

[0090] The steel according to the present invention, in addition to containing the above-mentioned main constituent elements and inevitable impurities, may also contain one, two or more of the elements described below. The types of additive elements, their composition ranges and the reasons for the limitations are as follows.

[0091] A. Group A

[0092] (13) 0.30 mass% < W ≤ 2.00 mass%:

[0093] In the steel according to the present invention, the C content and the V content are less than the C content and the V content in the hot working die steel in the prior art, so the strength may be insufficient depending on the application. In this case, it is effective to add W to increase the strength. To obtain such an effect, the W content is preferably more than 0.30 mass%. The W content is more preferably 0.80 mass% or more.

[0094] On the other hand, when the W content is excessive, the material cost increases. The segregation phenomenon may cause deterioration of mechanical properties or an increase in anisotropy. Therefore, the W content is preferably 2.00 mass% or less. The W content is more preferably 1.50 mass% or less.

[0095] (14) 0.30 mass% < Co ≤ 1.00 mass%:

[0096] Like W, Co has the effect of increasing strength. Therefore, when the strength is insufficient, adding Co to increase the strength is effective. To obtain such an effect, the Co content is preferably more than 0.30% by mass. The Co content is more preferably 0.50% by mass or more.

[0097] On the other hand, when the Co content is excessive, the material cost increases. The segregation phenomenon may cause deterioration of mechanical properties or an increase in anisotropy. Therefore, the Co content is preferably 1.00% by mass or less. The Co content is more preferably 0.90% by mass or less.

[0098] Note that the steel according to the present invention may include one or both of Co and W.

[0099] B. Group B

[0100] (15) 0.0002% by mass < B ≤ 0.0080% by mass:

[0101] When the P content in the steel is relatively large, P segregated at the grain boundaries reduces the grain boundary strength and the impact value decreases. Adding B is effective in increasing the grain boundary strength. For the grain boundary strength to increase, B needs to exist alone in the steel (not form a compound). When BN is formed, the effect of adding B disappears. Therefore, in the steel containing N, when adding B to increase the grain boundary strength, N needs to combine with an element other than B.

[0102] Specifically, N is preferably combined with nitride-forming elements such as Ti, Zr, or Nb that easily form nitrides. These elements are effective even at impurity levels, but when the content of these elements is insufficient, it is preferable to add these elements so that their content exceeds the impurity level.

[0103] Note that BN has the effect of improving the machinability of the steel. Therefore, when adding B to improve the machinability, it is not necessary to actively add nitride-forming elements to the steel.

[0104] To obtain the above effects, the B content is preferably greater than 0.0002% by mass. The B content is more preferably 0.0003% by mass or more, and further preferably 0.0004% by mass or more.

[0105] On the other hand, even when adding more B than necessary, there is no difference in the effect and no practical benefit. When the B content is excessive, the cost of the steel increases. Therefore, the B content is preferably 0.0080% by mass or less. The B content is more preferably 0.0075% by mass or less, and further preferably 0.0070% by mass or less.

[0106] C. Group C

[0107] (16) 0.006 mass% < S ≤ 0.180 mass%:

[0108] (17) 0.0005 mass% < Ca ≤ 0.0500 mass%:

[0109] (18) 0.03 mass% < Se ≤ 0.50 mass%:

[0110] (19) 0.005 mass% < Te ≤ 0.100 mass%:

[0111] (20) 0.01 mass% < Bi ≤ 0.50 mass%:

[0112] (21) 0.03 mass% < Pb ≤ 0.50 mass%:

[0113] In the steel according to the present invention, addition of free-cutting elements is effective for improving machinability. Specific examples of free-cutting elements include S, Ca, Se, Te, Bi, and Pb. The steel according to the present invention may contain any one of these free-cutting elements, or may contain two or more of them.

[0114] In order to obtain sufficient free-cutting performance, the content of free-cutting elements is preferably greater than the respective lower limits described above.

[0115] On the other hand, when the content of free-cutting elements is excessive, cracks may occur during hot working. When the content of free-cutting elements is excessive, the impact value, fatigue strength, hot crack resistance, etc. may decrease. Therefore, the content of free-cutting elements is preferably equal to or less than the respective upper limits described above.

[0116] Group D.D

[0117] (22) 0.004 mass% < Nb ≤ 0.100 mass%:

[0118] (23) 0.004 mass% < Ta ≤ 0.100 mass%:

[0119] (24) 0.004 mass% < Ti ≤ 0.100 mass%:

[0120] (25) 0.004 mass% < Zr ≤ 0.100 mass%:

[0121] In the steel according to the present invention, carbide nitride forming elements other than V and Al may be added to increase the amount of carbides, carbonitrides, and / or nitrides. Specific examples of carbide nitride forming elements include Nb, Ta, Ti, and Zr. The steel according to the present invention may contain any one of these carbide nitride forming elements, or may contain two or more of them.

[0122] In order to prevent excessive grain growth of austenite grains, the content of the carbonitride-forming element is preferably greater than the above-mentioned respective lower limits.

[0123] On the other hand, when the content of carbonitride-forming elements is too much, carbides, carbonitrides and / or nitrides are crystallized in a coarse-crystalline state during the casting process. Even during homogenization heat treatment, SA and quenching, coarse crystal particles cannot be eliminated and remain as foreign matter, which leads to a decrease in impact value and fatigue strength. Therefore, the content of carbonitride-forming elements is preferably equal to or less than the above respective upper limits.

[0124] 1.2. Steel properties

[0125] 1.2.1. Quality and size

[0126] In the steel material according to the present invention, the C content and the V content are small, and the Mn content and the Cr content are optimized, so the influence of large foreign matter, low cooling rate after hot working, and low quenching rate is small. That is, in the steel material according to the present invention, even in the case of large mass and size, high levels of five properties of SA performance, machinability, impact value, hot crack resistance, and softening resistance can be obtained.

[0127] For example, when the composition and manufacturing conditions of the steel are optimized, in addition to all five properties reaching a practical level, a steel with a mass of more than 3,000 kg can be obtained. When the composition and manufacturing conditions of the steel are further optimized, a steel with a mass of more than 4,000 kg or more than 5,000 kg can even be manufactured.

[0128] When the composition and manufacturing conditions of the steel material are optimized, a steel sheet having the above-mentioned properties and having the minimum size (L1) in the longitudinal direction, the size (L2) in the transverse direction, and the size (L3) in the height direction can be obtained. min ) is a steel material with a thickness of 300 mm or more. If the composition and manufacturing conditions of the steel material are further optimized, even L min Steel materials with a thickness of 350 mm or more or 400 mm or more.

[0129] Here, “dimension in the longitudinal direction ( L1 )”, “dimension in the transverse direction ( L2 )” and “dimension in the height direction ( L3 )” respectively refer to the lengths of three sides of a rectangular parallelepiped with a minimum volume defining the periphery of the steel material.

[0130] 1.2.2. Hardness

[0131] In the present invention, “hardness of a steel material” refers to the Rockwell B-scale hardness obtained by (a) cutting out a sample from near the center (region where the solidification rate is low) of a cross section of a steel material after SA and (b) measuring the hardness at room temperature using the sample.

[0132] For example, when the steel material is a bulk material of a[mm]×b[mm]×c[mm] (a≤b≤c, a≥300mm), a first material of a[mm]×b[mm]×d[mm] is cut from the end surface in the c-axis direction. The value of d is not particularly limited, but is preferably 30 mm to 70 mm.

[0133] Next, a second material of e [mm] × f [mm] × d [mm] is cut out from the approximate center of the ab surface of the first material. There is no particular limitation on the values ​​of e and f, but preferably e = 90 mm to 120 mm, and f = 130 mm to 160 mm. In addition, a sample for hardness measurement is cut out from the second material, and the hardness is measured using the sample.

[0134] When the steel material according to the present invention is subjected to SA under appropriate conditions, the hardness of the steel material is appropriately reduced and mechanical processing can be performed. When the composition and manufacturing conditions (particularly SA conditions) of the steel material are optimized, the hardness at room temperature is 98 HRB or less. When the composition and / or manufacturing conditions of the steel material are further optimized, the hardness at room temperature is 97 HRB or less or 96 HRB or less.

[0135] 1.2.3. Impact value

[0136] In the present invention, the "impact value of a steel material" refers to an impact value obtained by: (a) cutting a square bar (12 mm × 12 mm × 55 mm) from near the center of a cross section of a steel material after SA (an area with a low solidification rate), (b) tempering the square bar to 44.5 HRC to 45.5 HRC by heat treatment, (c) manufacturing an impact test specimen from the tempered square bar, and (d) conducting an impact test at 15°C to 35°C.

[0137] The cutting position of the square rod is the same as the cutting position of the sample used for hardness measurement. That is, the square rod is cut out from the second material.

[0138] The "heat treatment" for quenching and tempering the square bar refers to a treatment in which: (a) the square bar is held at 970°C for 2 hours, then cooled from 970°C to 500°C at a cooling rate of 6°C / min, cooled from 500°C to 180°C at a cooling rate of 0.5°C / min, and then cooled from 180°C to below 100°C at an arbitrary cooling rate, and (b) subsequently subjected to the following heat treatment, wherein the process of heating to a temperature range of 560°C to 600°C and cooling to below 100°C is regarded as one cycle, and this cycle is performed one or more times.

[0139] “Impact test specimen” refers to a test specimen that complies with JIS Z2242:2018 (10 mm × 10 mm × 50 mm, arc radius at notch tip: 1 mm, notch depth: 2 mm, lower cross-sectional area at notch bottom of test specimen: 0.8 cm 2 ).

[0140] "Impact value (J / cm 2 )” is the absorption energy [J] divided by the lower cross-sectional area of ​​the notch bottom of the specimen (0.8 [cm 2 ]) and obtain the value.

[0141] "Average impact value (J / cm 2 )” refers to the average impact value of 10 or more (preferably 10 to 20) impact specimens.

[0142] "Low impact value ratio (%)" means that the impact value is less than 20 [J / cm 2 ] is the ratio of the number of impact specimens (n) to the total number of impact specimens subjected to impact test (n0) (=n×100 / n0).

[0143] In the steel material according to the present invention, with optimization of the composition and the manufacturing conditions, a steel material which exhibits a high impact value and a small variation in the impact value despite a large size can be obtained.

[0144] Specifically, under optimized composition and manufacturing conditions, an average impact value of 25 [J / cm 2 ] or above and the low impact value ratio is 30% or less.

[0145] When the composition and manufacturing conditions are further optimized, the average impact value is 26 [J / cm 2 ] or above or 27[J / cm 2 ]above.

[0146] In the case where the composition and manufacturing conditions are further optimized, the low impact value ratio is 20% or less or 10% or less.

[0147] 1.2.4. Original austenite grain size

[0148] The “prior austenite grain size” of a steel material means a value obtained by: (a) preparing an impact test specimen or a test specimen subjected to heat treatment under the same conditions as those for an impact test specimen, (b) etching the test specimen to expose the grain boundaries of prior austenite, or determining the grain boundaries of prior austenite by crystal orientation analysis, and (c) observing the test specimen at a magnification such that 50 or more grains are included in one field of view and calculating the equivalent circle diameter of each prior austenite grain included in the field of view.

[0149] The average value of the original austenite grain size is the average value of the grain size in the total area of ​​0.5 mm 2 The average grain size of all prior austenite grains contained in one or more fields of view.

[0150] Since the steel material according to the present invention contains a relatively large amount of pinning particles, the austenite grains are less likely to coarsen during quenching heating. When the composition and manufacturing conditions of the steel material are optimized, the average value of the original austenite grain size is 150 μm or less. When the composition and manufacturing conditions of the steel material are further optimized, the average value of the original austenite grain size is 135 μm or less or 120 μm or less.

[0151] 2. Mould

[0152] The mold according to the present invention is made of the steel material according to the present invention, and has the following properties.

[0153] 2.1. Quality and size

[0154] The mold of the present invention can have a mass of more than 2000 kg. When the composition and manufacturing conditions of the mold are further optimized, a mold with a mass of more than 3000 kg or more than 4000 kg can be manufactured.

[0155] By optimizing the composition and manufacturing conditions of the mold, it is possible to obtain a mold having the above-mentioned properties and having the minimum size (L'1) in the longitudinal direction, the size (L'2) in the transverse direction, and the size (L'3) in the height direction. min ) is a mold with a diameter of more than 250 mm. In the case of further optimizing the composition and manufacturing conditions of the mold, it is even possible to manufacture L' min The mold is larger than 300 mm or larger than 350 mm.

[0156] Here, "dimension in longitudinal direction (L'1)", "dimension in transverse direction (L'2)" and "dimension in height direction (L'3)" respectively refer to the lengths of three sides of a rectangular parallelepiped with minimum volume defining the periphery of the mold.

[0157] 2.2. Hardness

[0158] In the present invention, the "hardness of a mold" refers to a Rockwell C-scale hardness obtained by (a) cutting out a sample from a mold surface and (b) measuring at room temperature using the sample.

[0159] Alternatively, a portable hardness tester (durometer) may be used to evaluate the surface of the mold according to the Rockwell C scale. Furthermore, the hardness (eg, Shore hardness) evaluated by the portable hardness tester (durometer) may be converted into Rockwell C hardness.

[0160] The mold according to the present invention can achieve high hardness even when the mass and size are relatively large. When the composition and manufacturing conditions of the mold are optimized, the hardness at room temperature is 38HRC to 48HRC by the HT method. When the composition and manufacturing conditions of the mold are further optimized, the hardness at room temperature is 39HRC to 49HRC or 40HRC to 50HRC.

[0161] By PH method, the hardness at room temperature is 35HRC to 45HRC. When the composition and manufacturing conditions of the mold are further optimized, the hardness at room temperature is 34HRC to 44HRC or 33HRC to 43HRC.

[0162] 3. Steel manufacturing method

[0163] The method for manufacturing a steel material according to the present invention comprises (a) a first step of melting raw materials mixed into a predetermined composition, refining the molten metal and pouring the molten metal into a mold, (b) a second step of subjecting the ingot to homogenization heat treatment, and (c) a third step of hot working the ingot after the homogenization heat treatment.

[0164] In the case of a steel material for the HT method, the method further includes: after the third step, (d) a fourth step of normalizing the substantially shaped material after hot working as required, (e) a fifth step of tempering the substantially shaped material as required, and (f) a sixth step of spheroidizing annealing (SA) the substantially shaped material.

[0165] On the other hand, in the case of a steel material for the PH method, the method further includes: after the third step, (d) a fourth step of normalizing the substantially formed material after hot working as required, (e) a fifth step of tempering the substantially formed material as required, (f) a sixth step of spheroidizing annealing (SA) the substantially formed material as required, and (g) a seventh step of quenching and tempering the substantially formed material as required.

[0166] In the case of steel for HT method, the sixth step is indispensable. Through SA treatment, the steel is tempered to a hardness that can be machined. On the other hand, in the case of steel for PH method, SA treatment is performed as needed.

[0167] In the present invention, "spheroidizing annealing (SA)" refers to a process in which: (a) the steel is heated in a furnace to [A c3 point -10℃] to [A c3 point + 50°C] (hereinafter also referred to as "SA treatment temperature") to form "a structure having dispersed carbides in the austenite phase and almost no or no ferrite phase", and (b) applying a slow cooling method or a constant temperature holding method to the steel having the above structure.

[0168] The SA treatment temperature is usually 830°C to 950°C, depending on the composition of the steel. Regardless of whether the slow cooling method or the constant temperature holding method is used, the hardness of the steel after SA is about 98HRB or less (about 240Hv or less), and it is in a relatively soft state that is convenient for rough processing (processing into a rough mold shape through machining).

[0169] 4. Effect

[0170] 4.1. Background

[0171] In recent years, as the size of cast products has increased, the size of die-casting molds used to manufacture cast products has also increased. The background of the increase in the size of cast products is that: (a) the size of each cast product has increased, or (b) a part manufactured by assembling a plurality of cast products in the prior art is cast in an integrated state.

[0172] In the case of a large die casting mold, the weight of the mold is more than 2000kg, and the weight of the material used to make the mold is more than 3000kg. The steel used for large die casting molds is required to be easy to cut (high machinability), have almost no cracks (thermal cracks) on the mold surface, and have almost no large cracks.

[0173] Large cracks are cracks that reach deep into the mold. The time when large cracks appear is the service life of the mold. Thermal cracks on the mold surface may cause large cracks, so large cracks and thermal cracks need to be prevented.

[0174] In the present invention, in order to prevent large cracks, the contents of C and V are reduced, and the contents of Mn and Cr are increased compared to the steel in the prior art. Then, the composition is further optimized based on the following three new viewpoints: (a) reducing retained austenite by high Mo content, (b) extending creep rupture time by high Mo content, and (c) preventing transformation heat generation by low Si content.

[0175] The above three points are important in large molds above 2000 kg, but are not considered problematic in molds of the prior art because most of these molds are less than 2000 kg.

[0176] Figure 1 A schematic diagram showing the effects obtained by increasing the Mo content and decreasing the Si content.

[0177] 4.2. Methods to prevent large cracks

[0178] 4.2.1. Reduction of retained austenite

[0179] The retained austenite in the quenched structure is transformed into martensite by sub-zero treatment. However, when the steel containing retained austenite is tempered, the retained austenite is transformed into bainite at high temperature (>Ms point + 120°C). The coarse bainite structure transformed at high temperature has a negative impact on the impact value and fracture toughness.

[0180] In the prior art, it is believed that retained austenite is transformed into martensite by tempering. Therefore, it is recognized that even if retained austenite exists, there is no problem with properties such as toughness by tempering. In contrast, in the present invention, it has been found that tempered retained austenite is transformed into bainite at high temperatures, and it has been concluded that controlling the amount of retained austenite is important for preventing large cracks.

[0181] The amount of retained austenite increases as the quenching rate decreases. Therefore, as the size of the die casting die increases, the amount of retained austenite increases. With the recent increase in the size of the die casting die, it is expected that it will be important to reduce the retained austenite as much as possible.

[0182] The steel material according to the present invention is characterized in that the Mo content is increased compared to the steel in the prior art, thereby reducing the amount of retained austenite.

[0183] 4.2.2. Prolonging creep rupture time

[0184] In large die casting dies, creep strength is expected to be important in addition to impact value and fracture toughness. In die casting, solidification of large cast products takes a long time, so the mold closing time becomes longer. During mold closing, high loads continue to act on the mold at high temperatures in a state of small fluctuations. This load may cause creep deformation and may cause large cracks in the mold.

[0185] The steel material according to the present invention is characterized in that the Mo content is increased compared to the steel in the prior art, thereby prolonging the creep rupture time.

[0186] 4.2.3. Preventing heat generation from transformation

[0187] When austenite transforms into another phase, heat is generated due to changes in the crystal structure or the value of thermophysical properties. This is transformation heat generation. Due to transformation heat generation, the temperature of the steel will hardly decrease during quenching. Even during quenching cooling, temperature rise or stagnation may occur. This tendency is obvious on the inside of large die casting molds.

[0188] Transformation heat generation has a negative impact on the structure and performance. This is because the diffusion type transformation continues even when the temperature rises or stagnates due to transformation heat generation. For example, in bainite transformation, the transformation heat generation is large compared to the case where the transformation heat generation is small, and the transformation proceeds at a high temperature. Therefore, it is difficult to obtain a fine structure.

[0189] The steel material according to the present invention is characterized in that the Si content is reduced compared to the steel in the prior art to prevent the transition heat generation.

[0190] 4.2.4. Effect of low V content and high Mo content

[0191] In order to obtain a hardness of 45HRC or more, steel in the prior art (such as SKD61) generally satisfies 0.50 mass% ≤ V ≤ 1.20 mass% and 1.00 mass% ≤ Mo ≤ 2.00 mass%. When hot cracks in a mold are repaired by welding with a bar or wire made of such steel, V-based carbides or carbonitrides crystallize in the welded portion. This is caused by the solidification of the weld repair material from a molten state, which is a phenomenon similar to crystallization during casting. The crystallized product crystallized during welding is smaller than that crystallized during casting, but may cause large cracks.

[0192] In contrast, the steel material according to the present invention has a low V content and a high Mo content (V≤0.30 mass%, 2.00 mass%≤Mo). Therefore, when the steel material is used as a rod, wire or powder for welding repair or additive manufacturing, the above-mentioned problem does not occur. This is because the V content is small. In addition, due to the large Mo content, a hardness of 45HRC or more can be stably obtained.

[0193] 4.3. Optimization of composition

[0194] Hereinafter, optimization of the compositional components to achieve hot crack prevention, macrocrack prevention, SA performance improvement, and machinability improvement will be described in detail. Table 1 shows the effects obtained by adjusting the elements related to hot crack prevention and macrocrack prevention.

[0195] [Table 1]

[0196]

[0197] 4.3.1.Preventing thermal cracks

[0198] Preventing thermal cracks is an effect achieved by reducing thermal fatigue. To reduce thermal fatigue, it is necessary to reduce the thermal stress generated in the mold and improve the mold's resistance to thermal stress.

[0199] In order to reduce thermal stress, it is effective to improve the thermal conductivity of steel. In the present invention, the thermal conductivity is improved by the following methods: (a) Reducing the Si content. (b) Not excessively increasing the Mn content and the Cr content.

[0200] In order to improve the resistance, it is effective to improve the high temperature tensile strength and softening resistance. In the present invention, the high temperature tensile strength and softening resistance are improved by the following methods: (a) Reducing the Si content. (b) Increasing the Mo content. (c) Not excessively increasing the Cr content.

[0201] 4.3.2. Preventing large cracks

[0202] Preventing large cracks is an effect achieved by preventing the generation and development of cracks. In order to prevent the generation and development of cracks, it is necessary to improve the impact value, fracture toughness, and load resistance under long-term high temperature. In order to improve the impact value and fracture toughness, it is effective to reduce coarse foreign matter and make the structure finer.

[0203] Note that the coarse foreign matter referred to in the present invention is a large particle with a size exceeding 0.5 μm, which is detrimental to the impact value and fracture toughness. Coarse foreign matter is roughly divided into the following two types according to its source: (4a) a crystallized product with a size of about 5 μm to 150 μm produced during the solidification of the ingot, and (4b) a precipitate with a size of about 0.5 μm to 10 μm formed after hot working.

[0204] In the present invention, the coarse foreign matter is reduced by the following methods: (a) reducing the C content and the V content. (b) not excessively increasing the Si content and the N content.

[0205] The reason for adjusting the C content and the V content is that most foreign matter contains C and V. The reason for adjusting the Si content and the N content is that they affect the amount of foreign matter and become constituent elements of the foreign matter.

[0206] The organization is refined by optimizing the following six items (a) to (f).

[0207] Note that (a) and (b) involve the refinement of austenite grains during quench heating, (c), (d) and (e) involve the prevention of phase transformation behavior during quench cooling, and (f) involves the structure after quenching is completed.

[0208] (a) Austenite memory during quenching heating:

[0209] "Austenite memory" refers to the quenching heating (>A c3The position of austenite grain boundary at the time of heating is different from that before heating ( c1 The phenomenon that the original austenite grain boundary position of the steel sheet (the original austenite grain boundary position) is almost the same as that of the steel sheet (the original austenite grain boundary position) before quenching. That is, the original austenite grain size hardly changes before and after quenching. When the original austenite grains before quenching are coarse, the original austenite grains are difficult to be refined by quenching heating, so the quenched material retains the same coarse original austenite grains as before quenching.

[0210] Austenite memory may occur when bainite or martensite is present in SA materials. For example, austenite memory may occur when the untransformed austenite remaining during removal from the furnace by the slow cooling method or the constant temperature holding method may become bainite or martensite due to rapid cooling after removal from the furnace. That is, austenite memory is likely to occur in steels with "high hardenability but poor SA performance". In order to avoid austenite memory, the Mn / Cr ratio, Ni content and Cu content are mainly optimized to ensure SA performance while maintaining high hardenability.

[0211] (b) Pinning particles dispersed in austenite during quenching:

[0212] The fine austenite grains obtained by avoiding austenite memory during the quenching heating process tend to coarsen during the period of being kept at the heating temperature. The pinning particles present during the quenching process prevent the austenite grains from coarsening. In the present invention, in order to optimize the amount of pinning particles, the C content, V content, Al content and N content are mainly optimized.

[0213] The particles dispersed in the quenched structure are preferably small particles with a size of 0.5 μm or less and at most 1 μm. The size is the length measured in the direction in which the particle length is maximized.

[0214] (c) Pearlite precipitation during quenching cooling:

[0215] When pearlite is precipitated during quenching and cooling, the quenched structure becomes a state in which pearlite is dispersed in a bainite or martensite matrix. Pearlite is coarse and has lower strength than the matrix, so large cracks will be generated during the use of the mold. In the present invention, the Si content, Mn content and Mo content are mainly optimized to prevent the precipitation of pearlite.

[0216] (d) Hardenability in the low temperature range capable of forming martensite or bainite transformed at low temperatures:

[0217] With the improvement of hardenability in the low temperature range, the formation of coarse bainite is prevented. In the present invention, in order to improve the hardenability in the low temperature range, the content of Mn+Cr is mainly optimized.

[0218] (e) Heat generation during bainite or martensite transformation

[0219] ​In particular, in large steel materials, as the heat generation due to transformation becomes less, the structure after quenching becomes finer. In the present invention, in order to prevent the heat generation due to transformation, the Si content is mainly optimized.

[0220] (f) The amount of retained austenite in the quenched structure:

[0221] The part containing the retained austenite in the quenched structure is transformed into coarse bainite by tempering at high temperature. In the structure with the coarse bainite area, cracks are easy to develop. In the present invention, in order to reduce the amount of retained austenite, the Mo content is mainly optimized.

[0222] "Load resistance at high temperature for a long time" means that the creep rupture time is prolonged. That is, even when a high load at high temperature continues to act for a long time in a state of small fluctuations, it must be difficult to break. In the present invention, in order to extend the creep rupture time, the Mo content is mainly optimized.

[0223] 4.3.3.SA Performance

[0224] It is preferred that the steel used for the HT method has excellent SA properties. When the hardenability is improved by increasing the contents of Mn, Ni and Cu, the SA properties deteriorate. Since the steel according to the present invention requires high hardenability, good SA properties are ensured by the following methods. (a) Do not excessively increase the Mn content. (b) Optimize the Mn / Cr ratio. (c) Make the upper limits of the Ni content and the Cr content low.

[0225] When SA performance is good, the austenite memory phenomenon during quenching heating can be avoided, so it also contributes to grain refinement.

[0226] 4.3.4. Machinability

[0227] It is preferred that both the steel material for the HT method and the steel material for the PH method have excellent machinability. When the Si content is reduced in order to prevent hot cracks, the machinability deteriorates. Since the steel material according to the present invention also needs to prevent hot cracks, the following method is used to ensure machinability that enables industrial cutting. (a) The Si content is not excessively reduced. (b) The Cr content and the Mo content are not excessively increased.

[0228] Examples

[0229] 1. Various verification tests

[0230] 1.1. Preferred ranges of Mn and Cr contents

[0231] 1.1.1. Overview

[0232] The quenching rate of large die casting molds is low. In particular, the cooling rate from 500°C to 180°C inside the mold may be less than 1.5°C / min. Even in this case, high hardenability is required so that martensitic transformation or bainitic transformation occurs at low temperature (≤Ms point + 120°C) to form a fine structure.

[0233] When the Mn content and the Cr content increase, the hardenability is improved, but when the Mn content increases, the SA performance deteriorates. In particular, the steel used for the HT method requires high SA performance. Therefore, in the present invention, the hardenability is studied by the Mn content and the Mn+Cr content, and the SA performance is studied by the Mn / Cr ratio, so that the hardenability and SA performance are obtained at the same time. In addition, when determining the preferred range, the softening resistance (Cr content) is also considered.

[0234] 1.1.2. Sample preparation and test methods

[0235] The composition (mass %) of the steel material was set to 0.32C-0.34Si-0.08Cu-0.11Ni-2.16Mo-0.18V-0.028Al-0.011N, and the Mn content and Cr content were systematically changed. This steel material was cast into an ingot of 150 kg. The obtained ingot was subjected to homogenization heat treatment, hot working, normalizing, tempering and SA.

[0236] The obtained steel materials were used to evaluate SA performance.

[0237] That is, a 12mm×12mm×20mm test specimen for evaluating SA performance was manufactured from the steel material after SA. The test specimen was subjected to vacuum heat treatment simulating "hot working-normalizing-tempering-spheroidizing annealing" in the manufacturing process of large mold materials, and its SA performance was evaluated. Please note that in this verification, normalizing and tempering were performed, but these treatments can be omitted.

[0238] The details of the vacuum treatment step are as follows.

[0239] That is, the sample was first kept in a vacuum at 1240°C for 0.5 hours. This treatment was to reproduce the coarse grains of the hot-worked material. After being kept at 1240°C for 0.5 hours, nitrogen was introduced into the furnace and pressurized to cause forced convection, thereby cooling the sample to below 100°C.

[0240] Subsequently, the sample was kept in vacuum at 1020°C for 1 hour. This treatment simulates normalizing. After being kept at 1020°C for 1 hour, nitrogen gas was introduced into the furnace and pressurized to cause forced convection, thereby cooling the sample to below 100°C.

[0241] Subsequently, the sample was kept in vacuum at 680°C for 6 hours. This treatment simulates tempering. After keeping at 680°C for 6 hours, nitrogen gas was introduced into the furnace and pressurized to cause forced convection, thereby cooling the sample to below 100°C.

[0242] Finally, SA was performed. That is, the sample was kept in a vacuum at 900°C for 1 hour. Thereafter, the sample was cooled to 600°C in a vacuum at a cooling rate of 15°C / hour. Thereafter, nitrogen was introduced into the furnace and pressurized to cause forced convection, thereby cooling the sample to below 100°C.

[0243] The hardenability was evaluated using the obtained steel materials.

[0244] That is, 10 square bars of 12 mm × 12 mm × 55 mm were manufactured from the round bars in the SA state. The square bars were kept in a vacuum at 970°C for 2 hours and then quenched. During the quenching process, the cooling rate from 970°C to 500°C was 6°C / min, and the cooling rate from 500°C to 180°C was 0.5°C / min.

[0245] The above quenching step is one of the examples of the inner part with the lowest cooling rate assuming that a large mold of more than 2000 kg is quenched. Since the cooling rate below 180°C does not significantly affect the impact value, the cooling rate from 180°C to below 100°C is not particularly controlled.

[0246] Subsequently, the square bar was subjected to a tempering treatment by holding the square bar at 590° C. for 2 hours and then cooling the square bar to 100° C. or less.

[0247] In addition, a tempering treatment is additionally performed. That is, the square bar is kept at 560°C to 600°C for a predetermined time and then cooled to below 100°C. This treatment is performed once or multiple times, and the square bar is tempered to 44.5HRC to 45.5HRC.

[0248] The impact specimens were made from square bars tempered to 44.5HRC to 45.5HRC. The shape of the impact specimens (10mm×10mm×50mm, arc radius of notch tip: 1mm, notch depth: 2mm, lower cross-sectional area of ​​the notch bottom of the specimen: 0.8cm 2 ) is in compliance with JIS Z2242: 2018. An impact test was performed at a temperature of 15°C to 35°C using the obtained impact test specimen.

[0249] The impact value is used for evaluation. The “impact value [J / cm 2 ]" is calculated by dividing the absorbed energy [J] by the lower cross-sectional area of ​​the notch at the bottom of the specimen, 0.8 cm 2 The values ​​obtained are the average values ​​of ten samples.

[0250] Results

[0251] Figure 2 The following table shows the ranges of Mn content and Cr content for obtaining a steel material having excellent SA properties and hardenability. Figure 2 The shaded area indicates that the hardness after SA is below 98HRB and the impact value after quenching and tempering is 25J / cm 2 and exhibits a high softening resistance.

[0252] 1.2. Preferred Mo content (1): Amount of retained austenite

[0253] 1.2.1. Sample preparation and test methods

[0254] The composition (mass %) of the steel material was set to 0.32C-0.28Si-0.81Mn-0.11Cu-0.23Ni-6.22Cr-0.22V-0.017Al-0.012N, and the Mo content was varied in the range of 0.51 mass % to 3.06 mass %. These steel materials were cast into 150 kg ingots. The obtained ingots were subjected to homogenization heat treatment, hot working, normalizing, tempering and SA.

[0255] Round rods with a diameter of 12 mm and a length of 50 mm were produced from the material after SA (rectangular material with a cross section of 40 mm×65 mm).

[0256] The cooling steps for quenching the round bar at 970°C were divided into two types. The first was heating at 970°C for 2 hours, then cooling to 500°C at a cooling rate of 100°C / min, and cooling from 500°C to 180°C at a cooling rate of 20°C / min. The second was heating at 970°C for 2 hours, then cooling to 500°C at a cooling rate of 6°C / min, and cooling from 500°C to 180°C at a cooling rate of 0.5°C / min.

[0257] The cooling rate below 500°C simulates the center of the mold. The rate of 20°C / min (first step) is assumed when quenching a small mold of about 5 kg. The rate of 0.5°C / min (second step) is assumed when quenching a large mold of more than 2000 kg. Samples were cut from the quenched round bars and the amount of retained austenite was measured.

[0258] Results

[0259] Figure 3 The relationship between the amount of retained austenite and the content of Mo is shown. When the cooling rate is 20° C. / min, the amount of retained austenite is as low as about 5%, and the influence of the Mo content is small.

[0260] On the other hand, when the cooling rate is 0.5°C / min, the amount of retained austenite is large. In particular, when the Mo content is small, the amount of retained austenite reaches 20%. When the Mo content is 2% by mass or more, the amount of retained austenite is significantly reduced even at a cooling rate of 0.5°C / min. That is, it has been found that in the case of a large mold in which the internal quenching rate becomes small, the Mo content can be set to 2.00% by mass or more to reduce the amount of retained austenite.

[0261] 1.3. Preferred Mo content (2): Creep rupture time

[0262] 1.3.1. Sample preparation and test methods

[0263] The material after SA was manufactured in the same manner as in [1.2.1.]. A round bar having a diameter of 18 mm and a length of 100 mm was manufactured from the material after SA. After heating the round bar at 970°C for 2 hours, quenching was performed, wherein the round bar was cooled to 500°C at a cooling rate of 6°C / min, and then cooled from 500°C to 180°C at a cooling rate of 0.5°C / min. In addition, after cooling to below 100°C, the round bar was tempered several times at 560°C to 600°C, thereby being quenched and tempered to 45HRC.

[0264] A creep test specimen having a total length of 70 mm, a parallel portion diameter of 6 mm, and a parallel portion length of 30 mm was prepared from the quenched and tempered round bar. A load of 1000 MPa was applied to the test specimen at 500°C, and the rupture time was evaluated.

[0265] Results

[0266] Figure 4 The relationship between creep rupture time and Mo content is shown. As the Mo content increases, the creep rupture time increases. When the Mo content is about 2.0 mass % or more, a long rupture time can be stably achieved.

[0267] That is, it has been found that, in the case where a high load acts continuously for a long time at a high temperature with a small fluctuation as in a die casting mold used for producing a large cast product, the Mo content can be set to 2.00 mass % or more to prevent fracture.

[0268] 1.4. Preferred Si content (1): Fracture toughness

[0269] 1.4.1. Sample preparation and test methods

[0270] The composition (mass %) of the steel material was set to 0.34C-0.86Mn-6.33Cr-0.22V-0.018Al-0.011N, and the Mo content was 1.21 mass % or 2.83 mass %. The Si content varied in the range of 0.05 mass % to 0.96 mass %. These steel materials were cast into 150 kg ingots. The obtained ingots were subjected to homogenization heat treatment, hot working, normalizing, tempering and SA.

[0271] A plate having a height of 13 mm, a width of 62 mm, and a length of 65 mm was manufactured from the material after SA (a rectangular material having a cross section of 40 mm×65 mm). After heating the plate at 970°C for 2 hours, quenching was performed, wherein the plate was cooled to 500°C at a cooling rate of 6°C / min, and from 500°C to 180°C at a cooling rate of 0.5°C / min. In addition, after cooling to below 100°C, the plate was tempered multiple times at 560°C to 600°C, thereby tempering to 43HRC.

[0272] A fracture toughness test specimen with a thickness of 12.5 mm, a width of 61 mm, and a length of 64 mm was prepared from the quenched and tempered plate, and the fracture toughness was measured at room temperature using the test specimen.

[0273] Results

[0274] Figure 5 The relationship between fracture toughness and Si content is shown. When the Si content is 0.96 mass%, the fracture toughness decreases when the Mo content increases from 1.21 mass% to 2.83 mass%. Although not shown in the figure, it has been found that the fracture toughness becomes very low, especially when the Mo content is 3.5 mass% or more.

[0275] On the other hand, even when the Mo content is 2.83 mass%, the fracture toughness increases when the Si content decreases. In particular, when the Mo content is 2.83 mass%, when the Si content is 0.40 mass% or less, the fracture toughness value is equivalent to the fracture toughness value of the sample with a Mo content of 1.21 mass%.

[0276] That is, it has been found that, for a large die in which the internal quenching rate becomes small, when the Mo content is increased from the viewpoint of the amount of retained austenite and creep strength, fracture toughness can be ensured by setting the Si content to 0.40 mass % or less.

[0277] 1.5. Preferred Si content (2): High temperature tensile strength

[0278] 1.5.1. Sample preparation and test methods

[0279] The material after SA was manufactured in the same manner as in [1.4.1.]. A round bar having a diameter of 18 mm and a length of 105 mm was manufactured from the material after SA. After heating the round bar at 970°C for 2 hours, quenching was performed, wherein the round bar was cooled to 500°C at a cooling rate of 6°C / min and from 500°C to 180°C at 0.5°C / min. In addition, after cooling to below 100°C, the round bar was tempered several times at 560°C to 600°C to be quenched and tempered to 45HRC.

[0280] A tensile test piece having a total length of 100 mm, a parallel portion diameter of 8 mm, and a parallel portion length of 40 mm was prepared from the quenched and tempered round bar, and a tensile test was performed at 600°C using the test piece.

[0281] Results

[0282] Figure 6 The relationship between high temperature tensile strength and Si content is shown. It has been found that the lower the Si content, the higher the high temperature tensile strength. It has been found that when the Si content is about 0.4 mass % or less, high high temperature tensile strength can be stably achieved. In addition, it has been found that even when the Mo content is large, the high temperature tensile strength is improved by reducing the Si content. That is, it has been found that when the Mo content is increased, the high temperature tensile strength can be effectively improved by simultaneously reducing the Si content (Si≤0.40 mass %).

[0283] 1.6. Preferred Si content (3): Softening resistance

[0284] 1.6.1. Sample preparation and test methods

[0285] The material after SA was manufactured in the same manner as in [1.4.1.]. A block material having a height of 11 mm, a width of 12 mm, and a length of 20 mm was manufactured from the material after SA. After heating the block material at 970°C for 2 hours, quenching was performed, wherein the block material was cooled to 500°C at a cooling rate of 6°C / min, and from 500°C to 180°C at a cooling rate of 3°C / min. In addition, after cooling to below 100°C, the block material was tempered multiple times at 560°C to 600°C, thereby being quenched and tempered to 45HRC.

[0286] Note that the cooling rate of 3°C / min below 500°C is the cooling rate assumed in the surface portion of a large mold of 2000 kg or more. Since the portion where softening becomes a problem is the surface of the mold, quenching of the surface portion was simulated.

[0287] The quenched and tempered bulk material was heated to 580°C in a vacuum furnace, maintained at 580°C for 10 hours, and then cooled to room temperature. Cooling was performed for about 1 hour, reducing the temperature from 580°C to 150°C.

[0288] At room temperature, the initial HRC hardness and the HRC hardness after heat treatment (H) were measured. The difference ΔHRC (=H-45) between the HRC hardness after heat treatment (H) and the initial HRC hardness (45HRC) was calculated and used as an indicator of softening resistance.

[0289] Results

[0290] Figure 7 The relationship between softening resistance (ΔHRC) and Si content is shown. It has been found that the smaller the Si content, the smaller the absolute value of ΔHRC, that is, the higher the softening resistance. It has been found that when the Si content is about 0.4 mass % or less, high softening resistance can be stably ensured. In addition, it has been found that even when the Mo content is large, the softening resistance is improved by reducing the Si content. That is, it has been found that when the Mo content is increased, the softening resistance can be effectively improved by simultaneously reducing the Si content (Si≤0.40 mass %).

[0291] Please note, Figure 7 0.96Si-1.21Mo in is SKD61. The steel according to the present invention has a lower C content and a lower V content than SKD61, in particular, the V content is as low as 0.22 mass %, but the softening resistance is improved by having a low Si content and a high Mo content. The effectiveness of a low V content and a high Mo content is confirmed.

[0292] It is known that when the content of Si as a solid solution strengthening element is reduced, the strength at room temperature is reduced. On the other hand, it has been found that when the Si content is reduced, the high temperature tensile strength and softening resistance are improved. This is because the reduction of the Si content prevents the high temperature (above 450°C and less than A) from being affected. c1 The carbide coarsening occurs in the area of ​​the point.

[0293] 1.7. Preferred Si content (4): Preventing pearlite precipitation

[0294] 1.7.1. Sample preparation and test methods

[0295] Prepare the material after SA in the same manner as in [1.4.1.]. Prepare a specimen with a diameter of 4 mm and a length of 10 mm from the material after SA. Cool the specimen from 970°C to below 100°C at a constant rate. Change the cooling rate. Measure the dimensional change of the specimen during cooling, and try to detect the expansion caused by pearlite transformation. After cooling to room temperature, confirm whether pearlite precipitates by microstructure observation.

[0296] According to the above procedure, the critical cooling rate for pearlite precipitation is determined. To prevent pearlite precipitation, the lower the critical cooling rate, the better. Because pearlite is unlikely to precipitate even in slow cooling, it is suitable for large molds with low internal quenching rates.

[0297] Results

[0298] Figure 8 The relationship between the critical cooling rate for pearlite precipitation and the Si content is shown. It has been found that the critical cooling rate decreases as the Si content decreases. It has been found that when the Si content is about 0.4 mass % or less, a low critical cooling rate can be stably ensured. In addition, it has been found that even when the Mo content is large, the critical cooling rate can be reduced by reducing the Si content.

[0299] For such large molds or steel materials for large molds, when the Mo content is increased from the viewpoint of the amount of retained austenite and creep strength, the critical cooling rate can be effectively reduced by simultaneously reducing the Si content (Si≤0.40 mass%), that is, pearlite precipitation can be prevented.

[0300] 1.8. Preferred Si content (5): Transformation heat generation

[0301] 1.8.1. Sample preparation and test methods

[0302] The composition (mass %) of the steel material is set to 0.35C-0.83Mn-0.07Cu-0.12Ni-6.28Cr-2.26Mo-0.24V-0.019Al-0.012N, and the Si content is 0.05 mass % or 1.83 mass %. These steel materials are cast into 10-ton ingots. The obtained ingots are subjected to homogenization heat treatment, hot working, normalizing, tempering and SA.

[0303] A block with a height of 400 mm, a width of 400 mm, a length of 800 mm and a mass of about 1 ton was manufactured from the SA steel. A thermocouple was inserted into the central part of the block and the temperature during vacuum quenching was measured. Vacuum quenching was performed by the following method, wherein the block was heated to 970°C in vacuum and nitrogen was introduced into the furnace, pressurized to 10 bar, so that the nitrogen formed forced convection.

[0304] Results

[0305] Fig. 9 The temperature transition in the center of the block during rapid cooling is shown. The temperature stagnation or increase due to the heat generated by the transition (caused by Fig. 9The smaller the Si content, the smaller the heat generated by the transformation. On the other hand, the average cooling rate from 450°C to 200°C is about 3°C / min, regardless of the Si content contained in the block.

[0306] 1.9. Preferred Si content (6): Effect of transition heat generation on impact value

[0307] 1.9.1. Sample preparation and test methods

[0308] Below 500°C in the quenching cooling process, the impact value and fracture toughness are greatly affected by the cooling rate from temperature Ts to temperature Tf. In the temperature range below 500°C, there is a temperature range in particular that has a great influence on the impact value and fracture toughness. In this specification, the starting temperature of this temperature range is defined as Ts, and the ending temperature of this temperature range is defined as Tf. Ts and Tf vary depending on the type of steel, but in the case of the two steels evaluated, it was known in preliminary studies that Ts = 450°C and Tf = 200°C. Therefore, the average cooling rate from 450°C to 200°C was evaluated. Note that the range from Ts to Tf is the temperature range in which bainite transformation or martensite transformation occurs.

[0309] The block after vacuum quenching produced in [1.8.1.] was tempered multiple times at 560°C to 600°C and quenched to 47HRC. When the structure near the center of the quenched block was confirmed, it was confirmed that pearlite was not precipitated. This is because the cooling rate in the pearlite transformation region of 800°C to 600°C exceeded 5°C / min.

[0310] An impact test specimen was made from the steel material near the center of the quenched and tempered block. The dimensions of the test specimen used were: 10 mm square, 55 mm long, 1 mm notch bottom radius, and 2 mm notch depth. The impact value at room temperature was measured using the obtained impact test specimen.

[0311] Results

[0312] When the Si content is 1.83 mass%, the impact value is 19 J / cm 2 On the other hand, when the Si content is 0.05 mass%, the impact value is 34 J / cm 2 .

[0313] Since the mass of the block is not too large, about 1 ton, and the quenching rate is high due to the powerful cooling at 10 bar pressure. In addition, the steel evaluated has a high hardenability (high content of Mn+Cr). For the above reasons, it is believed that the impact value of the material with a Si content of 0.05% is improved.

[0314] On the other hand, although the quenching rate and hardenability of the material having an Si content of 1.83% are almost the same as those of the material having an Si content of 0.05%, its impact value is reduced.

[0315] From the above results, it has been found that even when the average cooling rate in the bainite transformation region is the same, the impact value of the steel material with a small transformation heat generation is higher than that of the steel material with a large transformation heat generation. It is considered that the influence of transformation heat generation becomes significant in a large mold that is difficult to cool. Therefore, it has been found that in order to stably obtain a high impact value in a large mold, it is necessary not only to improve the hardenability but also to prevent the transformation heat generation.

[0316] 1.10. Simulation of heat generation during large mold transformation

[0317] 1.10.1. Test methods

[0318] In the quenching of large dies in the HT method and the quenching of steel materials for large dies in the PH method, the cooling delay due to the heat generation of transformation becomes significant. A simulation was performed to evaluate this situation which is difficult to test.

[0319] The simulation target is the quenching of large die steel in the PH method. SKD61 is used as the steel. The dimensions of the steel are: thickness 700mm, width 1000mm, length 2300mm, and the mass of the steel is about 12.5 tons. The vacuum quenching (nitrogen pressure: 10 bar) of the steel starting from 1030℃ is simulated.

[0320] 1.10.2. Results

[0321] Fig.10 A quenching simulation of a 12.5 tonne SKD61 block is shown. A significant delay in cooling is foreseen around 400°C due to the heat generation of the transformation. When state-of-the-art steels are used for large moulds, the impact values ​​are expected to be very low due to the low hardenability combined with the high heat generation of the transformation.

[0322] 2. Verification test of the phenomenon actually occurring in the mold: Examples 1 to 16 and Comparative Examples 1 to 6

[0323] 2.1. Overview

[0324] The object of the present invention is to "provide a steel material for a mold having good manufacturability and to provide a mold made of the steel material having a long service life". "Manufacturability" refers to SA performance and machinability. The term "long service life" means that hot cracks are unlikely to occur and large cracks will not occur.

[0325] Another object of the present invention is to "achieve the above objects even when the mass and size of the steel material are large."

[0326] In the following tests, SA performance, machinability, hot cracks, macro cracks, impact values, creep rupture time and the amount of retained austenite were verified. The heat treatment steps simulating large molds of more than 2000 kg were applied to small materials. Without using expensive and time-consuming large materials to manufacture, the phenomena actually occurring in large molds were verified efficiently and accurately.

[0327] 2.2. Sample preparation

[0328] 2.2.1. Preparation of round rod material

[0329] Table 2 shows the composition of 22 kinds of steel (Examples 1 to 16 and Comparative Examples 1 to 6) used for verification.

[0330] Note that Comparative Example 1 is SKD61. Comparative Examples 2 to 4 are commercially available steels that are improved steels of SKD61. Comparative Example 5 is a steel having a lower C content and Mo content than the steel according to the present invention (C=0.17 mass %, Mo=0.51 mass %). Comparative Example 6 is a steel having a higher V content (V=0.48 mass %) than the steel according to the present invention.

[0331] Each of the steels in Table 2 was cast into an ingot of 150 kg, and a round bar material in SA state having a diameter of 82 mm and a length of about 2900 mm was manufactured through the first step of the HT method.

[0332] The SA step was performed under appropriate conditions depending on the composition of the steel. The heating temperature of SA was 920°C in Comparative Example 1, 880°C in Comparative Examples 2 to 4, 900°C in Comparative Examples 5 to 6, and 900°C in Examples 1 to 16. After being kept at the above heating temperature for 2 hours, the material was cooled to 650°C at a cooling rate of 10°C / hour. Thereafter, the material was taken out of the heat treatment furnace and cooled.

[0333] [Table 2]

[0334]

[0335]

[0336] 2.2.2. Sample preparation

[0337] The following test specimens were produced from the above round bars.

[0338] (A) SA performance: The size of sample A is 12mm×12mm×20mm

[0339] (B) Machinability: The size of sample B is 25 mm × 50 mm × 200 mm.

[0340] (C) Thermal cracking and crack growth: The size of sample C is 72 mm (diameter) × 50 mm

[0341] (D) Impact value: The size of sample D is 11mm×11mm×55mm

[0342] (E) Creep rupture time: The size of sample E is 18 mm (diameter) × 100 mm

[0343] (F) Amount of retained austenite: The size of sample F is 10 mm (diameter) × 20 mm

[0344] Samples C, D, and E were tempered to 45HRC by heat treatment, machined into predetermined shapes, and then subjected to various evaluations. The other samples were used directly for various evaluations.

[0345] 2.2.3. Tempering treatment of samples

[0346] The tempering treatment was carried out in a vacuum furnace. Samples C, D and E were quenched after being heated at the quenching temperature for 2 hours, wherein the sample was cooled to 500°C at a cooling rate of 6°C / min and from 500°C to 180°C at a cooling rate of 0.5°C / min. At a temperature below 180°C, samples C, D and E were taken out of the furnace and cooled to below 100°C. In Comparative Examples 1 to 4, the quenching temperature was 1030°C, while in other examples the quenching temperature was 970°C. After quenching, the sample was tempered to 45HRC by multiple tempering at 560°C to 600°C.

[0347] 2.2.4. Machining of specimens

[0348] The specimens tempered to 45HRC were machined into shapes for performance evaluation.

[0349] A cylindrical specimen C2 with a profile of 70 mm (diameter) x 50 mm was manufactured from specimen C. A V-shaped notch was provided on one end face of the cylinder. The depth of the notch was 1 mm, the opening angle of the notch was 120°, and the R of the notch tip was 0.4 mm.

[0350] An impact specimen D2 with a profile of 10 mm×10 mm×55 mm was manufactured from specimen D. A U-shaped notch was provided at the center in the length direction. The depth of the notch was 2.0 mm, and the R at the tip of the notch was 1.0 mm.

[0351] From the sample E, a creep sample E2 having a total length of 70 mm, a diameter of a parallel portion of 6 mm, and a length of a parallel portion of 30 mm was manufactured.

[0352] 2.3. Test methods and results

[0353] 2.3.1 SA performance evaluation

[0354] Sample A in the SA state was subjected to an experiment simulating a manufacturing method starting from the hot working step in the “first step of the HT method”.

[0355] Heat treatment was performed using a vacuum furnace. To simulate the coarse austenite grains during hot working, sample A was heated at 1240°C for 2 hours. To simulate the grain boundary precipitation of carbides or the like during cooling after hot working, the sample was cooled from 1240°C to 650°C at a cooling rate of 1°C / min. At temperatures below 650°C, nitrogen was introduced into the furnace to accelerate cooling.

[0356] Since the phenomena simulated by heat treatment are coarse austenite grains and grain boundary precipitation of carbides, the other conditions may not necessarily correspond to the actual hot working steps.

[0357] After the heat treatment simulating the hot working step, the normalizing step and the tempering step are performed, and SA is performed. The heating temperature of SA is the same as the heating temperature described when manufacturing the round bar material. On the other hand, the cooling rate from the heating temperature of SA is 23°C / hour. Softening to 98HRB or less at such a high cooling rate is industrially indispensable in terms of productivity and cost.

[0358] After being held at a predetermined temperature for 2 hours, the sample was cooled to 650°C at a cooling rate of 23°C / hour, and nitrogen was introduced into the furnace at a temperature below 650°C to accelerate cooling. After SA, the Rockwell B scale hardness was measured in accordance with JIS Z2245:2016. Note that in Comparative Example 4, the Rockwell C scale hardness was also measured in accordance with JIS Z2245:2016.

[0359] The hardness after SA is shown in Table 3. In Table 3, "S" indicates that the hardness after SA is 98 HRB or less (SA performance is good), and "D" indicates that the hardness after SA is greater than 98 HRB (SA performance is poor).

[0360] When the temperature reaches 650°C, with the remaining untransformed austenite, through subsequent accelerated cooling, the austenite transforms into martensite or bainite, and the hardness exceeds 98HRB. Such steel is rated as poor SA performance.

[0361] In Comparative Example 4, the Rockwell B hardness was rated as D, and the Rockwell C hardness was measured as 29 HRC. This is considered to be due to the high Mn / Cr of 0.204. On the other hand, various other steels satisfying Mn / Cr≤0.150 had a Rockwell B hardness of 98 HRB or less and exhibited good SA performance.

[0362] [Table 3]

[0363] HRB HRC Evaluation results Example 1 91 S Example 2 93 S Example 3 92 S Example 4 94 S Example 5 91 S Example 6 89 S Example 7 92 S Example 8 95 S Example 9 88 S Example 10 89 S Embodiment 11 90 S Example 12 90 S Embodiment 13 90 S Embodiment 14 91 S Embodiment 15 90 S Example 16 96 S Comparative Example 1 90 S Comparative Example 2 89 S Comparative Example 3 89 S Comparative Example 4 98< 29 D Comparative Example 5 87 S Comparative Example 6 90 S

[0364] 2.3.2. Machinability evaluation

[0365] Cutting specimen B. The cutting distance until the wear of the cutting tool reaches 0.1 mm is defined as the tool life. The tool life corresponds to the machinability when the die material in the SA state is rough-machined. A long cutting distance indicates a long tool life and good machinability.

[0366] Table 4 shows the cutting distance [m]. Table 4 also shows the ratio of the cutting distance of each steel material to the cutting distance of SKD61 (Comparative Example 1) when the cutting distance of 36.4 m is set as 100% (hereinafter also referred to as "relative cutting distance"). In Table 4, "S" indicates that the relative cutting distance is 90% or more, "A" indicates that the relative cutting distance is 75% or more and less than 90%, "B" indicates that the relative cutting distance is 50% or more and less than 75%, "C" indicates that the relative cutting distance is 33% or more and less than 50%, and "D" indicates that the relative cutting distance is less than 33%.

[0367] The machinability of SKD61 (Comparative Example 1) is very good. On the other hand, in the steel types rated as D, the machinability corresponds to less than 1 / 3 of SDK 61 and is industrially unacceptable.

[0368] Among the 22 steels evaluated, none of them was rated as D. It is known that when the Si content is small, machinability deteriorates. Since there is no steel type with an Si content of less than 0.01 mass% among the 22 steels, none of them was rated as D.

[0369] Examples 6 and 9 were rated as C, but had industrially acceptable machinability. The Si content in Example 6 was 0.01 mass%, and the Si content in Example 9 was 0.02 mass%. In Example 10, the Si content was 0.05 mass%, and the machinability was rated as B. From the above results, it can be said that when the Si content is 0.03 mass% or more, there is almost no problem with machinability. In Examples 15 and 16, since the free-cutting component is contained, the machinability is rated as A or more.

[0370] [Table 4]

[0371]

[0372]

[0373] 2.3.3. Thermal crack evaluation

[0374] Thermal cycles were applied to the specimen C2, and the development of the generated hot cracks was evaluated. The following process was repeated on the end surface provided with a notch: heating to 580°C by high frequency and cooling to 90°C by spraying water. The combination of heating and cooling was defined as one cycle. In this evaluation, the case of heating by molten metal in the die casting mold and cooling by injection of a mold release agent was simulated. The notch was assumed to be a sharp corner portion of a stress concentration portion on the mold surface.

[0375] Sample C2 that had been through 10 to 10,000 thermal cycles was cut in the center portion, and the crack at the bottom of the notch, that is, the depth of the thermal crack, was measured. A graph was created with the horizontal axis being the number of thermal cycles and the vertical axis being the crack depth, and the number of thermal cycles when the crack depth was 0.2 mm was obtained by interpolation.

[0376] A crack depth of 0.2 mm is a condition where the transfer of the crack to the cast product begins to become apparent in die casting and the crack begins to show up in dye penetrant testing. The high number of thermal cycles at a crack depth of 0.2 mm indicates that the generation and development of thermal cracks proceed slowly, and therefore thermal crack resistance is good.

[0377] Table 5 shows the number of cycles when the crack depth is 0.2 mm. Table 5 also shows the ratio of the number of cycles of each steel material compared to 228 cycles of SKD61 (Comparative Example 1) when it is set as 100% (hereinafter also referred to as "relative number of cycles A"). In Table 6, "S" means that the relative number of cycles A is greater than 190%, "A" means that the relative number of cycles A is greater than 160% and is less than 190%, "B" means that the relative number of cycles A is greater than 130% and is less than 160%, "C" means that the relative number of cycles A is greater than 105% and is less than 130%, and "D" means that the relative number of cycles A is less than 105%.

[0378] SKD61 (Comparative Example 1) was poor in hot crack resistance and was rated as D. On the other hand, since the improved steels of SKD61 (Comparative Examples 2 to 4) had improved hot crack resistance, they were rated as B and C. Comparative Example 5 was poor in hot crack resistance and was rated as D. It is considered that this is because the C content of Comparative Example 5 is small and the Mo content is small compared with the steel according to the present invention, and therefore, the degree of softening of the surface of the sample by heating at 580° C. during the application of the thermal cycle is large, and hot cracks are easily generated due to the decrease in strength.

[0379] The thermal crack resistance of Examples 15 and 16 was evaluated as C, and the thermal crack resistance was lower than that of the other Examples. This is considered to be because the compound of the free-cutting component accelerates the generation and growth of cracks.

[0380] In other examples, the hot crack resistance was good and was rated as B or more. In particular, in the three steels of Examples 6, 9 and 10, since the Si content was 0.05 mass% or less, the hot crack resistance was rated as S, and it was found that they stably exhibited hot crack resistance of about two to three times that of SKD61. The examples in which Si = 0.10 mass% to 0.24 mass% were rated as A, and it was found that the hot crack resistance thereof was nearly twice that of SKD61.

[0381] [Table 5]

[0382]

[0383]

[0384] 2.3.4. Large crack evaluation

[0385] In a die-casting mold, when a crack develops to a certain depth, the development speed increases rapidly, resulting in a large crack. The same phenomenon was also confirmed in the above-mentioned thermal cycle test. In the graph with the horizontal axis being the number of thermal cycles and the vertical axis being the crack depth, the slope in the graph changes sharply at a certain number of thermal cycles. This is a phenomenon that causes large cracks in a die-casting mold. The number of thermal cycles when the slope in the graph changes rapidly is obtained by interpolation, and the result is used as an indicator of large cracks. A large number of thermal cycles when the slope in the graph changes rapidly indicates that large cracks rarely occur.

[0386] Table 6 shows the number of thermal cycles when cracks begin to develop rapidly. Table 6 also shows the ratio of the number of cycles of each steel material compared to 284 cycles of SKD61 (Comparative Example 1) when it is set as 100% (hereinafter also referred to as "relative number of cycles B"). In Table 6, "S" means that the relative number of cycles B is greater than 900%, "A" means that the relative number of cycles B is greater than 600% and is less than 900%, "B" means that the relative number of cycles B is greater than 300% and is less than 600%, "C" means that the relative number of cycles B is greater than 150% and is less than 300%, and "D" means that the relative number of cycles B is less than 150%.

[0387] When a large mold is manufactured using SKD61 (Comparative Example 1), the mold may have large cracks. In fact, the number of thermal cycles of SKD61 is as low as 284 times, which is a small increase compared to 228 times in Table 5. This is because the time from the start of the transfer of the generated thermal cracks to the cast product to the appearance of large cracks is short. In Comparative Example 2, the relative number of cycles B is improved by 39% compared to SKD61 (Comparative Example 1), but considering that the change in mold service life due to large cracks is about 50%, it cannot be said that a significant improvement has been made.

[0388] When the number of thermal cycles when large cracks appear is stably close to two times, that is, when the relative cycle number B is 150% to 300%, it is evaluated that a significant improvement effect is obtained. This case is defined as the evaluation result C. All embodiments 1 to 16 are evaluated as exceeding C and being above B. In addition, only embodiment 15 is evaluated as B. The other embodiments are all evaluated as above A, and the number of thermal cycles when large cracks appear is stably more than six times the number of thermal cycles of SKD61. In particular, the number of thermal cycles of the embodiments evaluated as S exceeds ten times the number of thermal cycles of SKD61. In embodiments 1 to 16, low thermal stress due to high thermal conductivity and microstructure refinement due to high hardenability prevent rapid development of cracks.

[0389] Comparative Example 5, which was rated as D in Table 5, was rated as A in the case of large cracks. This is considered to be because, although the thermal crack resistance was poor due to a large softening degree, the development of cracks was prevented due to high thermal conductivity and high hardenability.

[0390] [Table 6]

[0391]

[0392] 2.3.5. Impact value evaluation

[0393] The impact value is sensitive to the presence of foreign matter and tissue density, and it is easy to determine whether the composition, manufacturing method or heat treatment is appropriate. In fact, the impact value of a mold with a long service life is high. Therefore, the impact value can be specified as an acceptance condition for mold steel or molds.

[0394] The impact test was carried out at room temperature using sample D2. The absorbed energy [J] was divided by 0.8 [cm 2 ]The value obtained by measuring the notch cross-sectional area is the impact value.

[0395] Each steel was evaluated by the average value of 10 samples. The results are shown in Table 7. The absolute value of the impact value is more important than the ratio of the impact value to the impact value of a certain steel. In Table 7, "S" means that the impact value is greater than 30 [J / cm 2 ], "A" means the impact value is greater than 25[J / cm 2 ] and 30[J / cm 2 ] below, "B" means the impact value is greater than 23 [J / cm 2 ] and 25[J / cm 2 ] below, "C" means the impact value is greater than 20 [J / cm 2 ] and 23[J / cm 2 ] or less, and "D" means the impact value is 20[J / cm 2 ]the following.

[0396] When the impact value is 20[J / cm 2 ] or less, the mold may develop large cracks during use. In the large molds targeted by the present invention, the impact value required for the die-casting mold is 25 [J / cm 2 ]. When the impact value is greater than 30[J / cm 2 ], the risk of generating large cracks becomes very low. In each of Examples 1 to 16, the impact value was rated as B or more.

[0397] In Comparative Example 5, the C content and the Mo content are less than those of the steel material according to the present invention, and its impact value is evaluated as C. In the comparative example, since the V content is 0.30 mass % or less, the amount of foreign matter is small, and since the content of Mn+Cr is 6.70 mass % or more, the hardenability is also good. However, in Comparative Example 5, since the C content is small and the transformation point is high, the structure is coarse. Therefore, the impact value of Comparative Example 5 is insufficient.

[0398] In Comparative Example 6, the V content is greater than that of the steel material according to the present invention, and the impact value is rated as D. In Comparative Example 6, the content of Mn+Cr is 6.70 mass % or more, so the hardenability is high. However, in Comparative Example 6, the V content is greater than 0.30 mass %, so the amount of foreign matter is large, and good hardenability cannot be achieved.

[0399] The impact values ​​in Comparative Examples 1 to 4 were rated as D. This is considered to be because: (a) the V content exceeded 0.30 mass % and the amount of foreign matter was large, and (b) the Mn+Cr content was less than 6.70 mass % and the hardenability was poor, and as a result, the structure became coarse.

[0400] In particular, in SKD61 (Comparative Example 1), since the V content is the largest and the Mn+Cr content is also small, the impact value is 10 [J / cm 2 ], which is a very low value.

[0401] [Table 7]

[0402] Shock value Evaluation results Example 1 30 A Example 2 29 A Example 3 30 A Example 4 29 A Example 5 32 S Example 6 31 S Example 7 28 A Example 8 26 A Example 9 27 A Example 10 31 S Embodiment 11 32 S Example 12 32 S Embodiment 13 32 S Embodiment 14 28 A Embodiment 15 25 B Example 16 27 A Comparative Example 1 10 D Comparative Example 2 12 D Comparative Example 3 16 D Comparative Example 4 16 D Comparative Example 5 22 C Comparative Example 6 19 D

[0403] 2.3.6. Creep rupture time evaluation

[0404] Creep test was carried out at 500°C using sample E2. The load was set to 1000 MPa. Each steel was evaluated by the average value of three samples. The results are shown in Table 8. Table 8 also shows the ratio of the creep rupture time of each steel compared to SKD61 (Comparative Example 1) when 1.7 hours is set as 100% (hereinafter also referred to as "relative rupture time"). In Table 8, "S" means that the relative rupture time is greater than 300%, "A" means that the relative rupture time is greater than 250% and less than 300%, "B" means that the relative rupture time is greater than 200% and less than 250%, "C" means that the relative rupture time is greater than 150% and less than 200%, and "D" means that the relative rupture time is less than 150%.

[0405] The fracture time of SKD61 (Comparative Example 1) was as short as 1.7 hours. It can be said that in addition to the problem that cracks may develop quickly (see Table 6) and the impact value is low (see Table 7), large cracks may also be generated from the perspective of creep conditions in large molds.

[0406] Comparative Example 2 is an improved steel of SKD61, but its fracture time is the same as that of SKD61. The fracture time of Comparative Example 5 is only 65% ​​of that of SKD61.

[0407] When the fracture time is stably close to twice that of SKD61, i.e., more than 1.5 times, it is evaluated as having a significant improvement effect. This case is defined as the evaluation result C. Steel materials whose fracture time is stably more than twice that of SKD61 are defined as the evaluation result B. Steel materials whose fracture time is close to three times that of SKD61, i.e., more than 2.5 times, have a significant improvement effect and are defined as the evaluation result A. In addition, steel materials whose fracture time exceeds three times that of SKD61 are evaluated as S.

[0408] All Examples 1 to 16 were rated higher than B and above A. In addition, only Example 13 and Example 16 were rated A. All other Examples were rated S.

[0409] The creep rupture time increases with increasing Mo content. Since there is no steel having a Mo content in the range of 1.25 mass % to 2.00 mass % among the 22 steels evaluated, none of the steels was rated as B or C.

[0410] [Table 8]

[0411]

[0412]

[0413] 2.3.7. Evaluation of retained austenite

[0414] Sample F was heated at the quenching temperature for 15 minutes, cooled to 500°C at a cooling rate of 6°C / min, and cooled from 500°C to 180°C at a cooling rate of 0.5°C / min. Then, it was taken out of the furnace and cooled. In Comparative Examples 1 to 4, the quenching temperature was set to 1030°C, while the quenching temperature of the other examples was set to 970°C. After quenching, Sample F was cut into two halves near the center in the length direction, and the amount of retained austenite was measured at the cut surface with a diameter of 10 mm.

[0415] Table 9 shows the amount of retained austenite. As the hardenability decreases and the Mo content decreases, the amount of retained austenite tends to increase. The amount of retained austenite in Comparative Examples 1 to 5 is 16% or more. In Comparative Example 6, the content of Mn+Cr is 6.70% by mass or more, the hardenability is high, and the Mo content is 2.00% by mass or more, so the amount of retained austenite is as low as 13%. In contrast, the amount of retained austenite in Examples 1 to 16 is 16% or less.

[0416] [Table 9]

[0417]

[0418]

[0419] 2.3.8. Overview of Examples

[0420] Six properties are listed in Table 10. In Comparative Example 1 (SKD61), since the SA property and machinability are very high, the mold manufacturing efficiency is the highest. On the other hand, the properties as a mold (such as heat crack resistance) are insufficient.

[0421] Comparative Examples 2 to 4, which are improved steels of SKD61, are steels with reduced machinability and improved thermal crack resistance compared to SKD61. However, they do not have the property of stably preventing macrocracks. Some elements included in Comparative Examples 5 and 6 are different from those of the steel material according to the present invention. Therefore, sufficient performance in terms of thermal cracks and macrocracks cannot be exhibited.

[0422] In contrast, Examples 1 to 16 are excellent in all properties. The amount of retained austenite that affects the impact value and creep rupture time is also small.

[0423] That is, it has been found that the steel material according to the present invention is easy to manufacture a material for a mold or a mold, and the mold manufactured from the steel has a long service life.

[0424] [Table 10]

[0425]

[0426] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications may be made without departing from the gist of the present invention.

[0427] This application is based on Japanese patent application No. 2023-082279 filed on May 18, 2023, the contents of which are incorporated herein by reference.

[0428] Industrial Applicability

[0429] The steel material according to the present invention can be used as a mold or a part thereof used in various manufacturing methods such as casting, forging, hot stamping, extrusion, injection molding and blow molding.

[0430] In the steel material according to the present invention, since the contents of C and V are small, when the steel material is used as a powder, a rod or a wire material for additive manufacturing or welding repair, cracks of a formed object or a welded portion can be avoided.

Claims

1. A steel material, comprising: 0.23% by mass ≤ C ≤ 0.39% by mass; 0.03% by mass ≤ V ≤ 0.30% by mass; 6.60% by mass ≤ Mn + Cr ≤ 7.40% by mass; Mn / Cr ≤ 0.150; Mn ≥ 0.60% by mass; Cr ≤ 6.60% by mass; Cu + Ni ≤ 0.84% by mass; 0.01% by mass ≤ Si ≤ 0.40% by mass; 2.00% by mass ≤ Mo ≤ 3.50% by mass; 0.001% by mass ≤ Al ≤ 0.080% by mass; and 0.003% by mass ≤ N ≤ 0.040% by mass, with the balance being Fe and unavoidable impurities.

2. The steel material according to claim 1, further comprising: at least one group selected from the following groups A to D: Group A: at least one selected from 0.30% by mass < W ≤ 2.00% by mass and 0.30% by mass < Co ≤ 1.00% by mass, Group B: 0.0002% by mass < B ≤ 0.0080% by mass, Group C: at least one selected from 0.006% by mass < S ≤ 0.180% by mass, 0.0005% by mass < Ca ≤ 0.0500% by mass, 0.03% by mass < Se ≤ 0.50% by mass, 0.005% by mass < Te ≤ 0.100% by mass, 0.01% by mass < Bi ≤ 0.50% by mass, and 0.03% by mass < Pb ≤ 0.50% by mass, Group D: at least one selected from 0.004% by mass < Nb ≤ 0.100% by mass, 0.004% by mass < Ta ≤ 0.100% by mass, 0.004% by mass < Ti ≤ 0.100% by mass, and 0.004% by mass < Zr ≤ 0.100% by mass.

3. The steel material according to claim 1 or 2, characterized in that The steel material has a mass of more than 3000 kg, and a minimum dimension (L1) among a dimension in a longitudinal direction, a dimension in a transverse direction, and a dimension in a height direction (L3) is min ) is 300mm or more.

4. A mold, the mold being made of the steel material according to claim 1 and having a mass of more than 2000 kg.