Preparation method of three-dimensional bimetallic nanowire electrode material and application of three-dimensional bimetallic nanowire electrode material in electrocatalytic synthesis of amino acid
The preparation of three-dimensional bimetallic nanowire electrode materials through in-situ growth and annealing technology has solved the problems of high synthesis cost of bimetallic nanostructures and uneven component distribution in the prior art, and achieved efficient amino acid electrocatalytic synthesis.
Patent Information
- Application Number
- CN202411165261.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-22
AI Technical Summary
The existing bimetal nanostructure synthesis methods have problems such as high cost, high complexity, and uneven component distribution, making it difficult to accurately control the structure and component distribution of nanomaterials.
By growing Cu nanowires in situ and annealing in a reducing atmosphere, silver nanoparticles were then uniformly grown on Cu nanowires to form a three-dimensional bimetallic nanowire electrode material for electrocatalyzing the reduction of α-ketoacid amine synthesis of α-amino acid .
It realizes low-cost, simple and efficient preparation of bimetallic nanowire electrode materials, with high catalytic efficiency and selectivity, and can efficiently synthesize amino acids.
Smart Images

Figure BDA0005007688210000081 
Figure BDA0005007688210000091 
Figure BDA0005007688210000092
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of a three-dimensional bimetallic nanowire electrode material and application of the same in electrocatalytic synthesis of amino acids, belonging to the technical field of electrochemistry. Background Art
[0002] As the basic components of proteins, amino acids play an indispensable role in the fields of biomedicine and life sciences. Traditional amino acid synthesis methods, such as the Strecker synthesis method, usually require the use of toxic substances (such as hydrogen cyanide) and harsh reaction conditions, and are prone to produce harmful by-products; although the microbial fermentation method has mild reaction conditions, the conversion efficiency is low. In contrast, electrosynthesized amino acids have many advantages such as mild reaction conditions, high conversion efficiency, and less environmental pollution, providing a new green synthesis method for the sustainable development of the chemical industry and biotechnology. α-Keto acids react with nitrogen-containing compounds (such as nitrogen (N2), nitrogen oxides (NO x The reductive amination reaction of α-keto acids (e.g., lactic acid, glycolic acid, α-hydroxyglutaric acid) and hydroxylamine (NH2OH) is considered to be a new process for the electrosynthesis of amino acids. α-Keto acids can be obtained from the oxidation of α-hydroxy acids (e.g., lactic acid, glycolic acid, α-hydroxyglutaric acid) or the reduction of dicarboxylic acids (e.g., oxalic acid, malonic acid). Therefore, the synthesis of amino acids by electrochemical reductive amination using cheap and abundant α-keto acids as raw materials provides a green, simple and efficient method for the production of amino acids, which has important theoretical and practical significance.
[0003] With the in-depth study of electrocatalyst design and optimization of reaction conditions, the electrocatalytic research of α-keto acid reduction to amino acids has made significant progress. Silver (Ag) and copper (Cu) each have unique advantages in the field of electrocatalysis. Silver has good conductivity and selectivity for specific reactions, and copper is an abundant metal and has high activity for certain reactions. Combining silver and copper to form a bimetallic nanomaterial can achieve the synergistic complementarity of the advantages of both. The unique morphology and interfacial properties of the composite material can show more excellent electrochemical performance, providing stronger catalytic activity and selectivity for the electrocatalytic synthesis of amino acids. Therefore, the synergistic effect of Ag / Cu bimetallic nanostructures is used to improve reaction efficiency and selectivity, providing a new direction for the research and development of catalysts and their application in electrocatalytic reduction amination reactions.
[0004] The current methods for synthesizing bimetallic nanostructures are: 1) coprecipitation method: low cost but there is a problem of uneven composition; 2) sol-gel method: the preparation material has good uniform dispersion but the process is complicated and the cost is high; 3) chemical vapor deposition: highly crystalline nanomaterials can be obtained but the equipment requirements and cost are high and the reaction conditions are harsh; 4) mechanical alloying: the operating conditions are simple but impurities may be introduced and the particle surface energy is high; 5) template method: Ag / Cu nanocomposite structures are synthesized through chemical or physical adsorption of special templates such as polymers or surfactants, and the material selection and removal process of the template may affect the structural properties and cost.
[0005] In summary, the existing methods have the following disadvantages: high cost and complexity, inability to precisely control the structure of nanomaterials, and uneven component distribution; therefore, it remains a challenge to design a low-cost, simple, and precise method for synthesizing bimetallic nanomaterials with uniform component distribution. Summary of the invention
[0006] In view of the deficiencies of existing research, the present invention provides a method for preparing a three-dimensional bimetallic nanowire electrode material and its application in the electrocatalytic synthesis of amino acids.
[0007] The present invention first obtains Cu nanowires by in-situ growth and annealing in a reducing atmosphere, and further uniformly grows silver nanoparticles on the copper nanowires by electrodeposition to obtain three-dimensional bimetallic nanowires, which are used as catalysts for electrocatalytic α-keto acid reductive amination to synthesize α-amino acids, and have high catalytic efficiency and selectivity.
[0008] The technical solution of the present invention is as follows:
[0009] A method for preparing a three-dimensional bimetallic nanowire electrode material comprises the following steps:
[0010] (1) treating the copper foam with acetone, deionized water, and anhydrous ethanol ultrasonic cleaning in sequence to remove impurities on the surface, and then drying to obtain a pretreated copper foam;
[0011] (2) immersing the pretreated copper foam in a mixed aqueous solution of NaOH and (NH4)2S2O8 to react under magnetic stirring, and the surface of the copper foam changes from orange-yellow to dark blue. The copper foam is taken out and washed with deionized water until it is neutral; then it is placed in a vacuum oven and dried to obtain Cu(OH)2 nanowires;
[0012] (3) annealing the Cu(OH)2 nanowires in a reducing atmosphere to obtain Cu nanowires;
[0013] (4) Using Cu nanowires as working electrodes, graphite rods as counter electrodes, and Ag / AgCl as reference electrodes, constant potential deposition was performed in an electrochemical workstation in an electrodeposition solution to deposit a uniform and stable layer of Ag nanoparticle catalyst on the surface of the Cu nanowires to obtain a three-dimensional bimetallic nanowire electrode material.
[0014] Preferably according to the present invention, in step (1), the size of the copper foam is 10×20×1 mm.
[0015] Preferably, according to the present invention, in step (1), the ultrasonic cleaning treatment time is 10-20 minutes.
[0016] Preferably according to the present invention, in step (1), the drying condition is drying under argon.
[0017] Preferably, according to the present invention, in step (2), the concentration of NaOH in the mixed aqueous solution of NaOH and (NH4)2S2O8 is 1-5 mol / L, and the concentration of (NH4)2S2O8 is 0.05-0.5 mol / L.
[0018] Further preferably, in step (2), the concentration of NaOH in the mixed aqueous solution of NaOH and (NH4)2S2O8 is 2.5 mol / L, and the concentration of (NH4)2S2O8 is 0.13 mol / L.
[0019] Preferably, according to the present invention, in step (2), the temperature of the mixed aqueous solution of NaOH and (NH4)2S2O8 is 20-25°C.
[0020] Preferably according to the present invention, in step (2), the magnetic stirring speed is 150-200 rpm.
[0021] Preferably according to the present invention, in step (2), the magnetic stirring reaction time is 10-30 min.
[0022] Preferably according to the present invention, in step (2), washing is performed with deionized water until the pH value is 7.
[0023] Preferably according to the present invention, in step (2), the vacuum drying temperature is 50-70° C. and the drying time is 8-12 h.
[0024] Preferably, according to the present invention, in step (3), the reducing atmosphere is a H2 / Ar mixed gas, and the volume ratio of H2 to Ar is 10%:90%.
[0025] Preferably, according to the present invention, in step (3), the annealing temperature is 100-300° C., the heating rate is 1-5° C. / min, and the annealing time is 1-4 h.
[0026] Preferably, according to the present invention, in step (4), the electrodeposition solution is a mixed aqueous solution of AgNO3, C6H5Na3O7·2H2O and KNO3, the concentration of AgNO3 is 4-6mmol / L, the concentration of C6H5Na3O7·2H2O is 0.1-0.5mmol / L, and the concentration of KNO3 is 0.05-0.2mmol / L.
[0027] Preferably according to the present invention, in step (4), the electrodeposition voltage is -0.1 to -0.4 V vs. RHE, and the electrodeposition time is 1 to 600 s.
[0028] Further preferably, in step (4), the electrodeposition voltage is -0.35 V vs. RHE, and the electrodeposition time is 100-400 s.
[0029] A three-dimensional bimetallic nanowire electrode material is prepared by the method.
[0030] The three-dimensional bimetallic nanowire electrode material is used for cathode electrocatalytic reduction reaction of α-keto acid and hydroxylamine.
[0031] According to the preferred embodiment of the present invention, the specific application method is as follows:
[0032] A three-electrode system was composed of a three-dimensional bimetallic nanowire electrode material as a working electrode, a Pt sheet electrode as a counter electrode, and a saturated calomel electrode as a reference electrode, and the electrocatalytic reduction reaction of α-keto acid and hydroxylamine was carried out in an electrolyte.
[0033] Preferably according to the present invention, the electrolyte includes a cathode electrolyte and an anode electrolyte, the working electrode and the reference electrode are placed in the cathode electrolyte, and the counter electrode is placed in the anode electrolyte, the cathode electrolyte is an aqueous solution of α-keto acid, hydroxylamine sulfate and H2SO4, wherein the concentration of α-keto acid is 0.16 mol / L, the concentration of hydroxylamine sulfate is 0.096 mol / L, the concentration of H2SO4 is 0.2 mol / L, and the anode electrolyte is a 0.2 mol / L H2SO4 solution.
[0034] Preferably, according to the present invention, the electrolytic cell used is an H-type two-chamber glass electrolytic cell, and the cathode chamber and the anode chamber are separated by a Nafion 211 membrane.
[0035] Preferably according to the present invention, in order to eliminate interference from other reactions, the cathode chamber is thoroughly purged with Ar gas for 10 minutes before the reduction reaction to remove residual air in the solution. During the reduction reaction, argon gas is continuously introduced into the cathode chamber at a flow rate of 100 sccm to maintain an inert atmosphere.
[0036] According to the preferred embodiment of the present invention, when the electrocatalytic reduction reaction of α-keto acid and hydroxylamine sulfate is carried out, the potential is from 0V to -0.6V relative to the reversible hydrogen electrode ERHE , the scan rate is 5 mV s -1 , the reduction reaction time is 0.5-2h.
[0037] Reversible hydrogen electrode conversion formula: E RHE =E SCE +0.24+0.059×pH.
[0038] The technical features and excellent effects of the present invention are as follows:
[0039] 1. The present invention soaks the foam copper in a mixed aqueous solution of NaOH and (NH4)2S2O8 to grow Cu(OH)2 nanowires in situ by chemical oxidation. 2- A redox reaction occurs with Cu atoms, and Cu atoms are oxidized to Cu 2+ , with OH - The Cu(OH)2 nanowires are combined and finally a uniform and stable nanowire structure is obtained through mild oxidation conditions, specific concentration of the mixed aqueous solution, temperature, and stirring speed; annealing in a reducing atmosphere is performed to achieve uniform reduction while maintaining the morphology and size of the nanowires, avoiding sintering and aggregation, thereby obtaining Cu nanowires with good dispersion, which gives the catalyst a larger specific surface area.
[0040] 2. The present invention uses Cu nanowires as working electrodes for electrodeposition to achieve uniform deposition of silver nanoparticles on copper nanowires, and regulates the coverage of silver nanoparticles so that the prepared silver nanoparticles have good dispersibility. The cost requirement is low, the method is simple, and the morphology of copper nanowires modified with silver nanoparticles can be precisely controlled.
[0041] 3. The present invention can efficiently, controllably and stably prepare three-dimensional bimetallic nanowires of silver nanoparticle-coated copper nanowires through chemical oxidation, reducing atmosphere annealing reduction and electrodeposition. The three-dimensional bimetallic nanowires have bimetallic active sites. This structure can greatly improve the catalytic efficiency and selectivity of the electrocatalytic reduction of α-keto acids and hydroxylamine to produce α-amino acids. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a scanning electron microscope image of the Cu(OH)2 nanowires prepared in Example 1 of the present invention;
[0043] Figure 2 This is the X-ray diffraction pattern of the Cu(OH)2 nanowires prepared in Example 1 of the present invention;
[0044] Figure 3 This is a scanning electron microscope image of the Cu nanowires prepared in Example 1 after annealing and reduction in an Ar / H2 atmosphere;
[0045] Figure 4This is the X-ray diffraction pattern of the Cu nanowires prepared in Example 1 after annealing and reduction in an Ar / H2 atmosphere;
[0046] Figure 5 This is a scanning electron microscope image of the three-dimensional bimetallic nanowire of Example 1;
[0047] Figure 6 is an X-ray diffraction pattern of the three-dimensional bimetallic nanowire of Example 1;
[0048] Figure 7 This is a scanning electron microscope image of the Cu(OH)2 nanowires (18°C, 200rpm) prepared in Comparative Example 1;
[0049] Figure 8 This is a scanning electron microscope image of the Cu(OH)2 nanowires (5°C, 200rpm) prepared in Comparative Example 2;
[0050] Fig. 9 This is a scanning electron microscope image of the Cu(OH)2 nanowires (25°C, 500rpm) prepared in Comparative Example 3;
[0051] Fig.10 This is a scanning electron microscope image of the Cu(OH)2 nanowires (25°C, 400rpm) prepared in Comparative Example 4;
[0052] Fig.11 This is a scanning electron microscope image of the Cu(OH)2 nanowires (25°C, 100 rpm) prepared in Comparative Example 5;
[0053] Fig.12 This is a scanning electron microscope image of the silver nanoparticle-modified copper nanowire catalyst prepared in Comparative Example 6 after electrodeposition for 1000 s. DETAILED DESCRIPTION
[0054] The present invention is further described in detail below with reference to the embodiments, but the contents of the present invention are not limited thereto.
[0055] In the embodiment: foam copper (Cu, Suzhou Willtech Optoelectronic Materials Co., Ltd., 99.99%), silver nitrate (AgNO3, Chinese medicine, 99.8%), sulfuric acid (H2SO4, Chinese medicine, 95.0% to 98.0%), anhydrous ethanol (C2H5OH, Chinese medicine, 95%), potassium nitrate (KNO3, Chinese medicine, 99.0%), sodium hydroxide (NaOH, Chinese medicine, 95%), ammonium persulfate ((NH4)2S2O8, Chinese medicine, 98.5%), sodium citrate, dihydrate (C6H5Na3O7·2H2O, Aladdin, 99.0%), high purity argon (Ar, Deyang Gas, 99.99%), 10% argon hydrogen mixed gas (10% H2 / Ar, Deyang Gas, 99.99%), deuterium oxide (D2O, Macklin, 99.9%), maleic acid (C4H4O4, Macklin, 99.0%), pyruvic acid (C3H4O3, Macklin, 98%), hydroxylamine sulfate (2NH2OH·H2SO4, Macklin, 99.0%). All are commercially available products.
[0056] Embodiment 1:
[0057] The preparation method of the three-dimensional bimetallic nanowire electrode material comprises the following steps:
[0058] (1) A 10×20×1 mm copper foam was cleaned with acetone, deionized water, and anhydrous ethanol, respectively, and ultrasonically treated for 15 min to remove surface impurities, and then dried under argon;
[0059] (2) The copper foam dried in (1) was immersed in 100 mL of a mixed aqueous solution of NaOH and (NH4)2S2O8 at 25°C, wherein the concentration of NaOH was 2.5 mol / L and the concentration of (NH4)2S2O8 was 0.13 mol / L. The mixture was stirred at 25°C and 200 rpm for 15 min under the action of magnetic stirring, and the surface of the copper foam changed from orange-yellow to dark blue.
[0060] (3) taking out the copper foam treated in step (2), washing it with deionized water until the surface pH is 7, and then drying it in a vacuum oven at 60° C. for 10 h to obtain Cu(OH)2 nanowires;
[0061] (4) placing the Cu(OH)2 nanowires in a tubular furnace in a 10% Ar / H2 reducing atmosphere, heating the furnace to 200°C at a heating rate of 2°C / min, keeping the temperature for 2 hours, and cooling the furnace to room temperature to obtain Cu nanowires;
[0062] (5) Using Cu nanowire as the working electrode, graphite rod as the counter electrode, Ag / AgCl as the reference electrode, and 100mL of 5mmol / L AgNO3+0.2mmol / L C6H5Na3O7·2H2O+0.1mol / L KNO3 electrodeposition solution as the electrolyte, an electrochemical workstation was used to maintain a constant potential deposition of -0.35V vs. RHE for 100s to obtain a silver nanoparticle-modified copper nanowire catalyst.
[0063] Comparative Example 1:
[0064] The same preparation method as described in Example 1, except that:
[0065] In step (2), the temperature of the mixed aqueous solution of NaOH and (NH4)2S2O8 is 18°C, and the reaction temperature is 18°C.
[0066] The rest is carried out according to Example 1.
[0067] Comparative Example 2:
[0068] The same preparation method as described in Example 1, except that:
[0069] In step (2), the temperature of the mixed aqueous solution of NaOH and (NH4)2S2O8 is 5°C, and the reaction temperature is 5°C.
[0070] The rest is carried out according to Example 1.
[0071] Comparative Example 3:
[0072] The same preparation method as described in Example 1, except that:
[0073] In step (2), the stirring speed is 500 rpm;
[0074] The rest is carried out according to Example 1.
[0075] Comparative Example 4:
[0076] The same preparation method as described in Example 1, except that:
[0077] In step (2), the stirring speed is 400 rpm;
[0078] The rest is carried out according to Example 1.
[0079] Comparative Example 5:
[0080] The same preparation method as described in Example 1, except that:
[0081] In step (2), the stirring speed is 100 rpm;
[0082] The rest is carried out according to Example 1.
[0083] Comparative Example 6:
[0084] The same preparation method as described in Example 1, except that:
[0085] In step (5), the electrodeposition time is 1000 s;
[0086] The rest is carried out according to Example 1.
[0087] Test Example 1
[0088] 1. The scanning electron microscope image of the Cu(OH)2 nanowires prepared in step (3) of Example 1 is as follows: Figure 1 As shown, through Figure 1 It can be seen that the formed Cu(OH)2 nanowires are arranged perpendicular to the surface of the foam copper, are evenly distributed, and have a smooth surface. The X-ray diffraction pattern of the Cu(OH)2 nanowires is shown in Figure 2 As shown in the figure, the peaks at 43.297°, 50.433° and 74.13° correspond to the (111), (200) and (220) crystal planes of Cu respectively; the characteristic peaks at 23.836°, 34.061°, 39.800° and 53.210° are consistent with the (021), (002), (130) and (150) crystal planes of Cu(OH)2. This shows that Cu(OH)2 nanowires have been successfully grown on copper foam.
[0089] 2. The scanning electron microscope image of the Cu nanowires obtained in step (4) of Example 1 is as follows: Figure 3 As shown, it can be observed that the nanowires after 10% Ar / H2 reduction annealing are tightly interlaced and still maintain the shape of the nanowires. Due to the gas discharge, they become slightly curved and the surface is porous and rough. Figure 4 This is the X-ray diffraction pattern of the Cu nanowires prepared in step (4) of Example 1. The peaks of Cu (111), (200) and (220) crystal planes at 43.297°, 50.433° and 74.13° can be clearly seen in the figure, indicating that after reduction in 10% Ar / H2 at 200°C, the Cu(OH)2 nanowires on the surface are completely reduced to Cu nanowires.
[0090] 3. The scanning electron microscope image of the three-dimensional bimetallic nanowire prepared in step (5) of Example 1 is as follows: Figure 5 As shown, it can be observed that a layer of very tiny Ag nanoparticles is evenly distributed on the surface of the rough Cu nanowires. Figure 6 This is the X-ray diffraction pattern of the three-dimensional bimetallic nanowires. Although only the diffraction peak of Cu can be observed in the figure, no obvious characteristic peak of Ag can be observed. This is because the Ag content is low compared to the Cu nanowire substrate.
[0091] Test Example 2
[0092] The scanning electron microscope image of the Cu(OH)2 nanowires prepared in step (3) of Comparative Example 1 is as follows: Figure 7 As shown in the figure, it can be observed that the in-situ grown Cu(OH)2 presents a nanowire morphology. Compared with the Cu(OH)2 nanowires in Example 1, the reaction temperature is low, resulting in uneven length and thickness, different growth directions, and a disorderly and sparse distribution.
[0093] Test Example 3
[0094] The scanning electron microscope image of the Cu(OH)2 nanowires prepared in step (3) of Comparative Example 2 is as follows: Figure 8 As shown in the figure, it can be observed that Cu(OH)2 presents a nanowire morphology. Compared with the Cu(OH)2 nanowires in Example 1, the reaction temperature is low, resulting in shorter nanowires and uneven distribution.
[0095] Test Example 4
[0096] The scanning electron microscope image of the Cu(OH)2 nanosheet prepared in step (3) of Comparative Example 3 is as follows: Fig. 9 As shown in the figure, it can be observed that at a stirring speed of 500 rpm, the grown Cu(OH)2 is in the form of nanosheets and distributed on the surface of the foamed Cu, rather than Cu(OH)2 nanowires.
[0097] Test Example 5
[0098] The scanning electron microscopy image of the Cu(OH)2 nanostructure prepared in step (3) of Comparative Example 4 is as follows Fig.10 As shown in the figure, it can be observed that at a stirring speed of 300 rpm, the grown Cu(OH)2 is mainly nanosheets, in which a small amount of nanowires are interspersed and scattered on the surface of the foam Cu.
[0099] Test Example 6
[0100] The scanning electron microscope image of the Cu(OH)2 nanowires prepared in step (3) of Comparative Example 5 is as follows: Fig.11 As shown in the figure, it can be observed that at a stirring speed of 100 rpm, the grown Cu(OH)2 presents the morphology of nanowires, is evenly distributed, and has a smooth surface, but the growth direction is chaotic.
[0101] Embodiment 2:
[0102] The same preparation method as described in Example 1, except that:
[0103] In step (5), the concentration of AgNO3 in the electrodeposition solution is 6 mmol / L, the concentration of C6H5Na3O7·2H2O is 0.4 mmol / L, and the concentration of KNO3 is 0.2 mmol / L.
[0104] Embodiment 3:
[0105] The same preparation method as described in Example 1, except that:
[0106] In step (5), the electrochemical workstation was used to maintain a constant potential of -0.35 V vs. RHE for 200 s.
[0107] Embodiment 4:
[0108] The three-dimensional bimetallic nanowire electrode material described in Example 1 is used for cathode electrocatalysis of α-keto acid and hydroxylamine reduction reaction.
[0109] The specific application methods are as follows:
[0110] The three-dimensional bimetallic nanowire electrode material of Example 1 is used as the working electrode, the Pt sheet electrode is used as the counter electrode, and the saturated calomel electrode is used as the reference electrode to form a three-electrode system, and an electrocatalytic reduction reaction of α-keto acid and hydroxylamine is carried out in an electrolyte, wherein the electrolyte includes a cathode electrolyte and an anode electrolyte, the working electrode and the reference electrode are placed in the cathode electrolyte, and the counter electrode is placed in the anode electrolyte, the cathode electrolyte is an aqueous solution of α-keto acid, hydroxylamine sulfate and H2SO4, wherein the concentration of α-keto acid is 0.16 mol / L, the concentration of hydroxylamine sulfate is 0.096 mol / L, the concentration of H2SO4 is 0.2 mol / L, and the anode electrolyte is a 0.2 mol / L H2SO4 solution. At -0.32 V (relative to the reversible hydrogen electrode E RHE ) voltage for 1 h, with a scan rate of 5 mVs -1 After electrolysis, the cathode electrolyte is collected and dispersed in a solvent (D2O water) for 1 H NMR (400 MHz) analysis was performed to detect the yield of each α-keto acid, α-keto acid oxime and α-amino acid. When performing the NMR quantitative test of the product, 150 μL of the cathode electrolyte was mixed with 450 μL of a D2O solution containing 2 mg of maleic acid, wherein maleic acid was used as an internal standard agent, and the liquid was transferred to a 5 mm NMR tube for testing.
[0111] The performance of three-dimensional bimetallic nanowire electrode materials in the electrocatalytic reduction of α-keto acids and hydroxylamine to synthesize amino acids is shown in Table 1.
[0112] Table 1 Performance of amino acids synthesized by three-dimensional bimetallic nanowire electrode materials
[0113]
[0114] It can be seen from Table 1 that the silver nanoparticle-modified copper nanowire catalyst has excellent reduction performance for various α-keto acids. At a constant potential of -0.32 V vs. RHE, the yield of the silver nanoparticle-modified copper nanowire electrode for all amino acids exceeded 570 μmol h –1 cm –2 , FE was maintained above 70%. These results highlight the versatility of this 3D bimetallic nanowire electrode material in the efficient and highly selective electrosynthesis of various α-amino acids.
[0115] Test Example 7
[0116] Comparative Example 6: The scanning electron microscope image of the copper nanowire material modified with silver nanoparticles prepared by electrodeposition for 1000 s is as follows Fig.12 As shown in the figure, it can be observed that Ag nanoparticles are distributed and aggregated on the surface of Cu nanowires, and even larger Ag nanosheets appear covering the Cu nanowires.
[0117] The silver nanoparticle-modified copper nanowire material prepared by electrodeposition for 1000 s in Comparative Example 6 was used as the working electrode. Other operating methods were the same as those in Example 4. Its performance in electrocatalyzing the reduction of α-keto acid and hydroxylamine to synthesize amino acids is shown in Table 2.
[0118] Table 2 Performance of amino acids synthesized by three-dimensional bimetallic nanowire electrode materials prepared by electrodeposition for 1000 s
[0119]
[0120] It can be seen from Table 2 that as the electrodeposition time is too long, too many Ag nanoparticles are deposited on the surface of the Cu nanowires, and the performance of synthesizing amino acids is greatly reduced. Compared with the performance of synthesizing amino acids of the silver nanoparticle-modified copper nanowire material prepared in Example 1, the silver nanoparticle-modified copper nanowire material prepared by electrodeposition for 1000s exhibits a more negative reduction potential, and the corresponding α-amino acid Faradaic efficiency and yield are also lower, indicating that excessive loading of Ag weakens the ability of the Ag / Cu metal catalyst to reduce α-keto acids and hydroxylamine to synthesize amino acids.
[0121] Test Example 8
[0122] The foamed Cu was used as the working electrode, and other operation methods were the same as those in Example 4. The performance of the foamed Cu in the electrocatalytic reduction of α-keto acid and hydroxylamine to synthesize amino acids is shown in Table 3.
[0123] Table 3 Foam Cu synthetic amino acid properties
[0124]
[0125]
[0126] It can be seen from Table 3 that the performance of the foamed Cu as a catalyst for the electro-reduction of α-keto acids to amino acids is not good. Compared with the performance of the copper nanowire material modified with silver nanoparticles in Example 1, the α-keto acid and hydroxylamine reduction starting potential of the foamed Cu is higher, and the Faraday efficiency and yield of various amino acids are smaller, indicating that the catalyst is not conducive to the electro-reduction of α-keto acids to amino acids. At the same time, it also illustrates the unique advantages of the copper nanowire catalyst modified with silver nanoparticles in the electro-reduction of α-keto acids to synthesize amino acids.
Claims
1. A method for preparing a three-dimensional bimetallic nanowire electrode material, comprising the following steps: (1) treating the copper foam with acetone, deionized water, and anhydrous ethanol ultrasonic cleaning in sequence to remove impurities on the surface, and then drying to obtain a pretreated copper foam; (2) immersing the pretreated copper foam in a mixed aqueous solution of NaOH and (NH4)2S2O8 to react under magnetic stirring, and the surface of the copper foam changes from orange-yellow to dark blue. The copper foam is taken out and washed with deionized water until it is neutral; then it is placed in a vacuum oven and dried to obtain Cu(OH)2 nanowires; (3) annealing the Cu(OH)2 nanowires in a reducing atmosphere to obtain Cu nanowires; (4) Using Cu nanowires as working electrodes, graphite rods as counter electrodes, and Ag / AgCl as reference electrodes, constant potential deposition was performed in an electrochemical workstation in an electrodeposition solution to deposit a uniform and stable layer of Ag nanoparticle catalyst on the surface of the Cu nanowires to obtain a three-dimensional bimetallic nanowire electrode material.
2. The preparation method according to claim 1, characterized in that: In step (1), the ultrasonic cleaning treatment time is 10-20 minutes. In step (1), the drying is carried out under argon gas.
3. The preparation method according to claim 1, characterized in that: In step (2), the concentration of NaOH in the mixed aqueous solution of NaOH and (NH4)2S2O8 is 1-5 mol / L, and the concentration of (NH4)2S2O8 is 0.05-0.5 mol / L.
4. The preparation method according to claim 1, characterized in that: In step (2), the temperature of the mixed aqueous solution of NaOH and (NH4)2S2O8 is 20-25°C.
5. The preparation method according to claim 1, characterized in that: In step (2), the magnetic stirring speed is 150-200 rpm, the magnetic stirring reaction time is 10-30 min, the solution is washed with deionized water until the pH value is 7, the vacuum drying temperature is 50-70° C., and the drying time is 8-12 h.
6. The preparation method according to claim 1, characterized in that: In step (3), the reducing atmosphere is a H2 / Ar mixed gas, the volume ratio of H2 to Ar is 10%:90%, the annealing temperature is 100-300°C, the heating rate is 1-5°C / min, and the annealing time is 1-4h.
7. The preparation method according to claim 1, characterized in that: In step (4), the electrodeposition solution is a mixed aqueous solution of AgNO3, C6H5Na3O7·2H2O and KNO3, the concentration of AgNO3 is 4-6mmol / L, the concentration of C6H5Na3O7·2H2O is 0.1-0.5mmol / L, the concentration of KNO3 is 0.05-0.2mmol / L, the electrodeposition voltage is -0.1~-0.4V vs.RHE, and the electrodeposition time is 1-600s.
8. A three-dimensional bimetallic nanowire electrode material, prepared by the method according to any one of claims 1 to 7.
9. Use of the three-dimensional bimetallic nanowire electrode material according to claim 8 for cathode electrocatalysis of α-keto acid and hydroxylamine reduction reaction, The specific application methods are as follows: A three-electrode system was composed of a three-dimensional bimetallic nanowire electrode material as a working electrode, a Pt sheet electrode as a counter electrode, and a saturated calomel electrode as a reference electrode, and the electrocatalytic reduction reaction of α-keto acid and hydroxylamine was carried out in an electrolyte.
10. The use according to claim 9, characterized in that: The electrolyte includes a cathode electrolyte and an anolyte, the working electrode and the reference electrode are placed in the cathode electrolyte, the counter electrode is placed in the anolyte, the cathode electrolyte is an aqueous solution of α-keto acid, hydroxylamine sulfate and H2SO4, wherein the concentration of α-keto acid is 0.16 mol / L, the concentration of hydroxylamine sulfate is 0.096 mol / L, the concentration of H2SO4 is 0.2 mol / L, and the anolyte is a 0.2 mol / L H2SO4 solution; The electrolytic cell used was an H-type two-chamber glass electrolytic cell, with the cathode chamber and the anode chamber separated by a Nafion 211 membrane; When the electrocatalytic reduction reaction of α-keto acid and hydroxylamine sulfate is carried out, the potential ranges from 0V to -0.6V relative to the reversible hydrogen electrode E RHE , the scan rate is 5 mV s -1 , the reduction reaction time is 0.5-2h.
Citation Information
Cited By
Method for efficiently producing bacterial cellulose by using CO2 electroreduction electrolysis waste liquid
CN121674502A
Ag-FeOOH electrocatalyst, hydrogel enhanced electrocatalytic electrode as well as preparation method and application of Ag-FeOOH electrocatalyst and hydrogel enhanced electrocatalytic electrode
CN121781210A
Continuous cascade production method of alanine under photoelectric cooperative driving