Device and method for optimizing grain growth direction of single crystal casting

By using a device and method for selecting crystal structures and refining agent coatings during the growth of single crystal castings, the dendrite orientation was optimized, the problem of deviation between the growth direction and the heat flow direction of single crystal blades was solved, and the integrity and yield of single crystal castings were improved.

CN118996599APending Publication Date: 2024-11-22SUZHOU GAOJING NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411106175.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the existing technology, there is a large angular deviation between the growth direction and the heat flow direction of single crystal blades, which affects performance and easily leads to impurity crystal defects, making it difficult to guarantee the integrity and pass rate of single crystal castings.

Method used

An apparatus and method for optimizing the grain growth direction of single-crystal castings are employed, including a pouring cup, a single-crystal mold shell, a crystal selector, a water-cooling plate, and a pull rod. By setting a crystal selection structure and nickel foil in the crystal selector, combined with a refining agent coating, the dendrite orientation is optimized by utilizing temperature gradient and the pulling process, and single crystals with small orientation deviations are selected.

Benefits of technology

It improves the crystal selection efficiency of single crystal castings, reduces the probability of impurity crystal formation, obtains single crystals with smaller orientation deviations, and improves the integrity and yield of single crystal castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996599A_ABST
    Figure CN118996599A_ABST
Patent Text Reader

Abstract

The invention discloses a device for optimizing the grain growth direction of a single-crystal casting and an optimization method, and relates to the technical field of high-temperature alloy directional solidification. A pouring cup can be communicated with a single-crystal mold shell, a crystal selection structure is arranged in a crystal selector, a plurality of crystal selection channels are arranged in the crystal selection structure, and the single-crystal mold shell is communicated with the crystal selector. The lower end of the crystal selector is connected with the water cooling disc. The grain growth direction optimization method comprises the following steps that 1, a refiner is sprayed on the surface of nickel foil to form a refiner coating, and the nickel foil is arranged between a water cooling disc and a crystal selector; and 2, vacuumizing, pouring the smelted alloy, enabling the smelted alloy to enter a crystal selector from the single crystal mold shell, preserving heat, drawing the single crystal mold shell and the crystal selector, cooling after drawing is finished, taking out the single crystal mold shell, and finishing the pouring process to obtain the single crystal casting. According to the method, the dendritic crystal orientation finally entering the crystal selection section can be optimized, the single crystal with small orientation deviation is obtained, and the integrity of a single crystal casting is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of directional solidification of high-temperature alloys, and in particular to a device and an optimization method for optimizing the growth direction of grains of a single crystal casting. Background Art

[0002] Gas turbines and aircraft engines are known as the jewels in the crown of modern industry. They are the concentrated embodiment of a country's industrial foundation, scientific and technological level and comprehensive national strength. One of the main factors that determine the performance of aircraft engines and gas turbines is the temperature of the turbine inlet. As the temperature of the turbine inlet continues to increase, the organization of the turbine blade gradually develops from an equiaxed crystal organization of multiple grains to a single crystal organization of a single grain. Single crystal blades are composed of a single grain and have anisotropic characteristics. Their optimal performance direction is the

[001] orientation. In the actual growth process of the blade, due to the difference in temperature field, the

[001] orientation of the single crystal blade is at a certain angle to the heat flow direction, which has a great influence on the performance of the blade. Therefore, in order to ensure that the high-temperature mechanical properties of the blade are not affected, the

[001] growth direction of the single crystal blade is parallel to the heat flow direction as much as possible during the preparation process of the single crystal blade. In the prior art, the actual growth direction is generally about 10° from the heat flow direction, or even larger, and in this case, solidification defects such as impurities are also prone to occur. Summary of the invention

[0003] The purpose of the present invention is to provide a device and an optimization method for optimizing the grain growth direction of a single crystal casting, which can optimize the orientation of the dendrites that finally enter the crystal selection stage, obtain single crystals with smaller orientation deviation, and improve the integrity of the single crystal casting.

[0004] To achieve the above object, the present invention provides the following solutions:

[0005] The present invention provides a device for optimizing the grain growth direction of a single crystal casting, comprising: a pouring cup, a single crystal mold shell, a crystal selector, a water cooling plate and a pull-out rod, wherein the pouring cup can be connected to the single crystal mold shell, a crystal selection structure is arranged in the crystal selector, a plurality of crystal selection channels are arranged in the crystal selection structure, the single crystal mold shell is connected to the crystal selector, and the connection position between the single crystal mold shell and the crystal selector is located below the crystal selection structure, the lower end of the crystal selector is connected to the water cooling plate, and the water cooling plate is connected to the pull-out rod.

[0006] Preferably, the crystal selector comprises a spiral section and a seeding section arranged from top to bottom, the seeding section is a straight structure, the spiral section is a spiral structure, and the crystal selection structure is located in the seeding section.

[0007] Preferably, there is a gap between the upper end of the crystal selection structure and the upper end of the seeding section, and there is a gap between the lower end of the crystal selection structure and the lower end of the seeding section.

[0008] Preferably, the middle portion of the crystal selection structure is a solid structure, and each of the crystal selection channels is located outside the solid structure.

[0009] Preferably, the size of the crystal selection channel gradually decreases from the lower end to the upper end.

[0010] Preferably, a nickel foil is provided between the water cooling plate and the crystal selector, and a refiner coating is provided on the nickel foil.

[0011] Preferably, it also includes an outer cover, the pouring cup is arranged in the outer cover, the single crystal mold shell and the crystal selector can be located on the inner side of the outer cover, the outer cover includes an insulation layer, a heating body is arranged on the inner side of the insulation layer, and a heating coil is arranged on the outer side of the insulation layer.

[0012] Preferably, a water cooling ring is provided at the lower end of the outer cover, a heat insulation baffle is provided between the water cooling ring and the outer cover, and the water cooling ring is located outside the water cooling disk.

[0013] The present invention provides a method for optimizing the grain growth direction using the device for optimizing the grain growth direction of a single crystal casting, comprising the following steps:

[0014] Step 1, spraying a refiner on the surface of the nickel foil to form a refiner coating, and placing the nickel foil between a water cooling plate and a crystal selector;

[0015] Step 2: Vacuum and pour the molten alloy. The molten alloy enters the crystal selector from the single crystal mold shell, keeps warm, and pulls the single crystal mold shell and the crystal selector. After the pulling is completed, cool down and take out the single crystal mold shell. The pouring process is completed to obtain a single crystal casting.

[0016] Preferably, in the step 2, the molten alloy is heated to a superheated temperature and kept warm before being poured.

[0017] Compared with the prior art, the present invention has achieved the following technical effects:

[0018] The device and optimization method for optimizing the grain growth direction of single crystal castings of the present invention can improve the crystal selection efficiency in the competitive growth stage of single crystal castings and reduce the probability of forming impure crystals; can optimize the orientation of dendrites that finally enter the crystal selection stage and obtain single crystals with smaller orientation deviation; and can improve the integrity and qualified rate of single crystal castings. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 A schematic diagram of a device for optimizing the grain growth direction of a single crystal casting according to the present invention;

[0021] Figure 2 A schematic diagram of a nickel foil sprayed with a refiner coating according to the present invention;

[0022] Figure 3 It is a schematic diagram of the pouring cup, single crystal mold shell, crystal selector and water cooling plate of the present invention;

[0023] Figure 4 It is a front view of the crystal selector of the present invention;

[0024] Figure 5 It is a schematic diagram of the crystal selection structure of the present invention;

[0025] Figure 6 It is a cross-sectional view of the crystal selection structure of the present invention;

[0026] Figure 7 A top view of the crystal selection structure of the present invention;

[0027] Figure 8 A bottom view of the crystal selection structure of the present invention;

[0028] Fig. 9 This is a diagram showing the competitive growth and crystal selection effect of the grains at the lower position of the crystal selection structure of the present invention;

[0029] Fig.10 This is a diagram showing the competitive growth and crystal selection effect of the grains in the middle of the crystal selection structure of the present invention;

[0030] Fig.11 This is a diagram showing the competitive growth and crystal selection effect of the grains at the upper position of the crystal selection structure of the present invention;

[0031] Fig.12 A diagram showing competitive growth of grains and crystal selection effects during crystal selection of a single crystal casting using the method for optimizing the dendrite growth direction of a single crystal casting of the present invention (Comparative Example 1);

[0032] Fig.13 This is a diagram showing the competitive growth of grains and the effect of crystal selection during the crystal selection process of the single crystal casting of Comparative Example 2;

[0033] Fig.14 This is a diagram showing the competitive growth of grains and the effect of crystal selection during the crystal selection process of the single crystal casting of Comparative Example 3;

[0034] Fig.15 It is a diagram showing the competitive growth of grains and the effect of crystal selection during the crystal selection process of the single crystal casting of Comparative Example 4;

[0035] In the figure: 1-heating coil, 2-insulation layer, 3-heating body, 4-insulation baffle, 5-water cooling ring, 6-pouring cup, 7-single crystal mold shell, 8-nickel foil, 9-water cooling plate, 10-pull rod, 11-refining agent coating, 12-crystal selector, 13-crystal selection structure, 14-crystal selection channel, 15-solid structure, 16-casting, 17-spiral section, 18-seedling section, 19-center injection pipe, 20-pouring channel. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The purpose of the present invention is to provide a device and an optimization method for optimizing the grain growth direction of a single crystal casting, which can optimize the orientation of the dendrites that finally enter the crystal selection stage, obtain single crystals with smaller orientation deviation, and improve the integrity of the single crystal casting.

[0038] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0039] Embodiment 1

[0040] like Figures 1 to 8 As shown, this embodiment provides a device for optimizing the grain growth direction of a single crystal casting, including: a pouring cup 6, a single crystal mold shell 7, a crystal selector 12, a water-cooled plate 9 and a pull-out rod, the pouring cup 6 can be connected to the single crystal mold shell 7, a crystal selection structure 13 is arranged in the crystal selector 12, and a plurality of crystal selection channels 14 are arranged in the crystal selection structure 13, the center injection pipe 19 of the single crystal mold shell 7 is connected to the crystal selector 12 through a pouring channel 20, and the connection position of the pouring channel 20 of the single crystal mold shell 7 and the crystal selector 12 is located below the crystal selection structure 13, the lower end of the crystal selector 12 is connected to the water-cooled plate 9, and the water-cooled plate 9 is connected to the pull-out rod 10.

[0041] Specifically, in this embodiment, the crystal selector 12 includes a spiral section 17 and a seeding section 18 arranged from top to bottom, the casting 16 , the spiral section 17 and the seeding section 18 are all on a coaxial line, and the crystal selection structure 13 is located in the seeding section 18 .

[0042] In this embodiment, there is a gap between the upper end of the crystal selection structure 13 and the upper end of the seeding section 18, and there is a gap between the lower end of the crystal selection structure 13 and the lower end of the seeding section 18, preferably 30mm-50mm, which is conducive to the competitive growth of grains and the selection of grains with better orientation. The pouring channel 20 is connected to the seeding section 18, and the connection position of the pouring channel 20 and the seeding section 18 is 10mm away from the lower end of the crystal selection structure 13.

[0043] In this embodiment, the crystal selection structure 13 is an alumina porous ceramic cylinder obtained by 3D printing technology. The middle part of the crystal selection structure 13 is a solid structure 15. The diameter of the solid structure 15 matches the inner diameter of the spiral section 17 of the crystal selector 12. The diameter of the solid structure 15 is preferably 5 mm. The solid structure 15 can block the poorly oriented grains below the area from directly entering the crystal selector 12. Each crystal selection channel 14 is located on the outside of the solid structure 15. The size of the crystal selection channel 14 gradually decreases from the lower end to the upper end, that is, the crystal selection channel 14 is conical.

[0044] Figures 9 to 11 It shows the process of competitive growth of grains inside the crystal selection structure 13. From the lower end surface to the upper end surface of the crystal selection structure 13, the grains interact with each other and eliminate each other.

[0045] In this embodiment, the manufacturing process of the crystal selector 12 is as follows: the crystal selection structure 13 is placed inside the wax mold of the crystal selector 12, and wax is injected into the wax mold by adjusting the wax pressing parameters to obtain the crystal selector 12 with the crystal selection structure 13, and the residual wax around the crystal selection structure 13 and within 2 mm of the upper and lower edges is removed, which helps the mold shell to tightly fix the crystal selection structure 13 during the shell making process, so that <001> The grains with a relatively small deviation angle between the orientation and the heat flow direction pass through the conical crystal selection channel 14 to achieve the purpose of primary crystal grain screening; the crystal selector 12 with the crystal selection structure 13 is connected to the bottom of the wax mold to ensure that the axis of the crystal selector 12 is in a straight line with the axis of the wax mold. After trimming the wax mold, the wax mold is combined together by bottom injection to ensure that the crystal selector 12 and the wax mold are perpendicular to the wax mold chassis;

[0046] The shell making process of the crystal selector 12: the number of shell making layers is 6; the assembled wax mold is sent to the shell making process, the first surface layer uses 320 mesh zircon powder slurry and 100 mesh corundum sand; the second surface layer is 200 mesh zircon powder slurry and 70 mesh corundum sand; the third to sixth surface layers are 200 mesh zircon powder slurry and 14-28 mesh corundum sand; the drying time of each layer is controlled at 8h-10h.

[0047] In this embodiment, a nickel foil 8 is arranged between the water cooling plate 9 and the crystal selector 12, and a refiner coating 11 is arranged on the nickel foil 8. In this embodiment, the refiner coating 11 is added, so that a large number of nucleation particles are added to the contact surface between the molten alloy and the nickel foil 8. After the molten alloy is overheated, its nucleation supercooling degree increases. When the molten alloy contacts the nickel foil 8 with the refiner coating 11, a large number of nuclei will be formed on the surface of the refiner coating 11, increasing the nucleation rate in the molten alloy. Therefore, in the crystallization stage, the competitive growth effect of the grains is increased, and more grains with large growth orientation deviations are eliminated, thereby achieving the effect of optimizing the dendrite growth orientation of the grains.

[0048] This embodiment also includes an outer cover, a pouring cup 6 is arranged in the outer cover, a single crystal mold shell 7 and a crystal selector 12 can be located on the inner side of the outer cover, the outer cover includes an insulation layer 2, a heating body 3 is arranged on the inner side of the insulation layer 2, a heating coil 1 is arranged on the outer side of the insulation layer 2, a water cooling ring 5 is arranged at the lower end of the outer cover, an insulation baffle 4 is arranged between the water cooling ring 5 and the outer cover, and the water cooling ring 5 is located on the outer side of the water cooling plate 9.

[0049] During the directional solidification process, the single crystal mold shell 7 and the crystal selector 12 are pulled from the hot zone to the cold zone by the pulling rod 10. A temperature difference is formed between the hot zone and the cold zone in the pulling direction of the pulling rod 10, and there is a temperature gradient per unit length. Directional solidification is to pull the casting from the hot zone to the cold zone, and a positive temperature gradient from the solid phase to the liquid phase is generated at the interface front.

[0050] The crystal selection principle of the crystal selection structure 13 is as follows: after the molten alloy is poured into the single crystal mold shell 7, the interface where the molten alloy contacts the nickel foil 8 or the water cooling plate 9 rapidly nucleates to form a layer of fine equiaxed grains. Due to the existence of the positive temperature gradient, the equiaxed crystals grow into columnar crystals through the directional pulling of the pulling rod 10. At this time, the columnar crystals have a disordered orientation and there are many grains with large-angle crystal orientations. When these grains pass through the crystal selection structure 13, due to the constraint of the crystal selection structure 13, the grains with a relatively large crystal orientation deviation will be eliminated by the grains with a small crystal orientation deviation angle. After passing through the crystal selection structure 13, the grain orientation is optimized. After entering the spiral section 17 from the upper end of the seeding section 18, a single grain with a small orientation deviation angle can be obtained, and then a casting 16 is obtained.

[0051] Embodiment 2

[0052] This embodiment provides a method for optimizing the grain growth direction using the device for optimizing the grain growth direction of a single crystal casting according to the first embodiment, comprising the following steps:

[0053] Step 1: a wax mold model is obtained by adding a crystal selection structure 13 into the seeding section 18 of the crystal selector 12, a shell is made according to the shell making process, and then the single crystal shell 7 is dewaxed and roasted, and then a refiner is sprayed on the surface of the nickel foil 8 by a spraying process, and then baked at a high temperature to fix the refiner on the nickel foil 8 to form a refiner coating 11, and the nickel foil 8 is placed on a water cooling plate 9, the nickel foil 8 is in contact with the water cooling plate 9, and the single crystal shell 7 is placed on the nickel foil 8;

[0054] Step two, evacuate the single crystal mold shell 7, and before pouring the molten alloy, heat the molten alloy to an overheating temperature to achieve melt purification, and keep it warm, and pour the molten alloy. The molten alloy enters the crystal selector 12 from the single crystal mold shell 7, and the pouring temperature is 1480-1530°C. After keeping warm for 3-5 minutes, the single crystal mold shell 7 and the crystal selector 12 are pulled by the pulling rod 10. After the pulling is completed, wait until the single crystal mold shell 7 drops below a certain temperature, take out the single crystal mold shell 7, and the pouring process is completed to obtain a single crystal casting 16.

[0055] This embodiment improves the nucleation supercooling of the molten alloy through melt purification. When the nickel foil 8 with the refiner coating 11 is added to the water-cooled plate 9, the refiner coating 11 can increase the nucleation rate. The increase in the supercooling of the molten alloy can also increase the nucleation rate. When the two are combined, under the condition of the positive temperature gradient generated by the water-cooled plate 9 and the molten alloy, grains with different orientations compete for growth in the seeding section 18 of the crystal selector 12. At a fast pulling speed, the grains with an advantageous orientation will eliminate the grains with non-preferred orientation, and then when the grains enter the crystal selection structure 13, they will be preferentially selected again, and finally a single grain with a smaller crystal orientation deviation angle will be selected in the spiral section 17.

[0056] The device and optimization method for optimizing the grain growth direction of single crystal castings of the present invention can improve the crystal selection efficiency in the competitive growth stage of single crystal castings and reduce the probability of forming impure crystals; can optimize the orientation of dendrites that finally enter the crystal selection stage and obtain single crystals with smaller orientation deviation; and can improve the integrity and qualified rate of single crystal castings.

[0057] Comparative Example 1

[0058] The grain growth direction optimization method of the second embodiment includes the following steps:

[0059] Step 1: a wax mold model is obtained by adding a crystal selection structure 13 in the seeding section 18 of the crystal selector 12, and a shell is made according to the shell making process. Then, after the single crystal shell 7 is dewaxed and roasted, a refiner is sprayed on the surface of the nickel foil 8 by a spraying process, and then baked at a high temperature to fix the refiner on the nickel foil 8 to form a refiner coating 11. The nickel foil 8 is placed on a water cooling plate 9, the nickel foil 8 is in contact with the water cooling plate 9, and the single crystal shell 7 is placed on the nickel foil 8;

[0060] Step 2: evacuate the single crystal mold shell 7, heat the molten alloy to 1650-1730°C before pouring the molten alloy, and keep it warm for 3-5 minutes, pour the molten alloy, and let the molten alloy enter the crystal selector 12 from the single crystal mold shell 7. The pouring temperature is 1480-1530°C. After keeping warm for 3-5 minutes, the single crystal mold shell 7 and the crystal selector 12 are pulled by the pulling rod 10. After the pulling is completed, wait until the single crystal mold shell 7 drops below 100°C, take out the single crystal mold shell 7, and the pouring process is completed to obtain a single crystal casting. The dendrite orientation of the obtained casting is as follows: Fig.12 shown.

[0061] Comparative Example 2

[0062] The following steps are involved:

[0063] Step 1: a wax mold model is obtained by adding a crystal selection structure 13 in the seeding section 18 of the crystal selector 12, and a shell is made according to the shell making process. Then, the single crystal shell 7 is dewaxed and roasted, and then the single crystal shell 7 is placed on the water cooling plate 9, and no nickel foil 8 is arranged between the crystal selector 12 and the water cooling plate 9;

[0064] Step 2: Vacuum the single crystal mold shell 7. Before pouring the molten alloy, heat the molten alloy to 1610-1680°C and keep it warm for 3-5 minutes. Pour the molten alloy. The molten alloy enters the crystal selector 12 from the single crystal mold shell 7. The pouring temperature is 1480-1530°C. After keeping it warm for 3-5 minutes, the single crystal mold shell 7 and the crystal selector 12 are pulled by the pulling rod 10. After the pulling is completed, wait until the single crystal mold shell 7 drops below 100°C, take out the single crystal mold shell 7, and the pouring process is completed to obtain a single crystal casting. The dendrite orientation of the obtained casting is as follows: Fig.13 shown.

[0065] Comparative Example 3

[0066] The following steps are involved:

[0067] Step 1: a wax mold model is obtained by adding a crystal selection structure 13 in the seeding section 18 of the crystal selector 12, and a shell is made according to the shell making process. Then, the single crystal shell 7 is dewaxed and roasted, and then the single crystal shell 7 is placed on the water cooling plate 9, and no nickel foil 8 is arranged between the crystal selector 12 and the water cooling plate 9;

[0068] Step 2: evacuate the single crystal mold shell 7, heat the molten alloy to 1550-1560°C before pouring the molten alloy, and keep it warm for 3-5 minutes, pour the molten alloy, and let the molten alloy enter the crystal selector 12 from the single crystal mold shell 7. The pouring temperature is 1480-1530°C. After keeping warm for 3-5 minutes, the single crystal mold shell 7 and the crystal selector 12 are pulled by the pulling rod 10. After the pulling is completed, wait until the single crystal mold shell 7 drops below 100°C, take out the single crystal mold shell 7, and the pouring process is completed to obtain a single crystal casting. The dendrite orientation of the obtained casting is as follows: Fig.14 shown.

[0069] Comparative Example 4

[0070] The following steps are involved:

[0071] Step 1: without adding the crystal selection structure 13, a wax mold model is conventionally prepared, and the shell is made according to the same shell making process. After the shell is dewaxed and roasted, the single crystal shell 7 is placed on the water cooling plate 9, and no nickel foil 8 is set between the crystal selector 12 and the water cooling plate 9;

[0072] Step 2: Vacuum the single crystal mold shell 7 and pour the molten alloy. The molten alloy enters the crystal selector 12 from the single crystal mold shell 7. The pouring temperature is 1480-1530°C. After keeping warm for 3-5 minutes, the single crystal mold shell 7 and the crystal selector 12 are pulled by the pulling rod 10. After the pulling is completed, the single crystal mold shell 7 is removed when the temperature drops below 100°C. The pouring process is completed to obtain a single crystal casting. The dendrite orientation of the obtained casting is as follows: Fig.15 shown.

[0073] from Figures 12 to 15 It can be seen from the figure that if conventional process is used for directional solidification ( Fig.15 ), there is a probability to select a single grain with a large angle crystal growth direction, resulting in an increase in the crystal orientation deviation angle of the casting, which increases the scrap rate. When the crystal selection structure 13 is added to the seeding section of the crystal selector 12 ( Fig.14 ), the grain orientation angle is reduced, and the grain orientation deviation angle is within 15°; at the same time, combined with melt purification ( Fig.13 ), the grain orientation deviation angle is further reduced to about 6°; after adding the nickel foil 8 with the refiner coating 11 ( Fig.12 ), the nucleation rate increased, and the dendrite orientation was 3-4° after the crystal selection was completed, indicating that the addition of the crystal selection structure 13 and the nickel foil 8 with the refiner coating 11, and the melt purification scheme, increased the nucleation rate at the starting end of the seeding section 18, improved the effect of competitive growth, and significantly reduced the orientation deviation angle of the grains, thereby reducing the probability of crystal defects.

[0074] The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A device for optimizing the grain growth direction of a single crystal casting, characterized in that: include: A pouring cup, a single crystal mold shell, a crystal selector, a water cooling plate and a pull-out rod, wherein the pouring cup can be connected to the single crystal mold shell, a crystal selection structure is arranged in the crystal selector, a plurality of crystal selection channels are arranged in the crystal selection structure, the single crystal mold shell is connected to the crystal selector, and the connection position between the single crystal mold shell and the crystal selector is located below the crystal selection structure, the lower end of the crystal selector is connected to the water cooling plate, and the water cooling plate is connected to the pull-out rod.

2. The device for optimizing the grain growth direction of a single crystal casting according to claim 1, characterized in that: The crystal selector comprises a spiral section and a seeding section arranged from top to bottom, the seeding section is a straight structure, the spiral section is a spiral structure, and the crystal selection structure is located in the seeding section.

3. The device for optimizing the grain growth direction of a single crystal casting according to claim 2, characterized in that: There is a gap between the upper end of the crystal selection structure and the upper end of the seeding section, and there is a gap between the lower end of the crystal selection structure and the lower end of the seeding section.

4. The device for optimizing the grain growth direction of a single crystal casting according to claim 1, characterized in that: The middle part of the crystal selection structure is a solid structure, and each of the crystal selection channels is located outside the solid structure.

5. The device for optimizing the grain growth direction of a single crystal casting according to claim 1, characterized in that: The size of the crystal selection channel gradually decreases from the lower end to the upper end.

6. The device for optimizing the grain growth direction of a single crystal casting according to claim 1, characterized in that: A nickel foil is arranged between the water cooling plate and the crystal selector, and a refiner coating is arranged on the nickel foil.

7. The device for optimizing the grain growth direction of a single crystal casting according to claim 1, characterized in that: It also includes an outer cover, the pouring cup is arranged in the outer cover, the single crystal mold shell and the crystal selector can be located on the inner side of the outer cover, the outer cover includes a heat preservation layer, a heating body is arranged on the inner side of the heat preservation layer, and a heating coil is arranged on the outer side of the heat preservation layer.

8. The device for optimizing the grain growth direction of a single crystal casting according to claim 7, characterized in that: A water cooling ring is arranged at the lower end of the outer cover, a heat insulation baffle is arranged between the water cooling ring and the outer cover, and the water cooling ring is located outside the water cooling plate.

9. A method for optimizing the grain growth direction using the device for optimizing the grain growth direction of a single crystal casting according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1, spraying a refiner on the surface of the nickel foil to form a refiner coating, and placing the nickel foil between a water cooling plate and a crystal selector; Step 2: Vacuum and pour the molten alloy. The molten alloy enters the crystal selector from the single crystal mold shell, keeps warm, and pulls the single crystal mold shell and the crystal selector. After the pulling is completed, cool down and take out the single crystal mold shell. The pouring process is completed to obtain a single crystal casting.

10. The method for optimizing grain growth direction according to claim 9, characterized in that: In the step 2, before pouring the molten alloy, the molten alloy is heated to a superheated temperature and kept warm.

Citation Information

Cited By

  • Method for controlling orientation deviation of nickel-based single-crystal superalloy casting