Preparation method of gate-all-around stacked nanosheet field effect transistor

By using high etching selection ratio material as the sacrificial layer, the problem of channel material removal difficulties in the prior art is solved, and the preparation of stacked nanosheet ring gate field effect transistors is realized, which improves device performance and process compatibility and promotes Its industrial application.

CN119008531APending Publication Date: 2024-11-22BEIJING ZHICUN (WITIN) TECH CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411121502.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Prior Art When preparing stacked nanosheet ring-gate field effect transistors, the lack of a high selection ratio etching process makes it difficult to remove the sacrificial layer of the channel material, damages the oxide semiconductor channel, and limits the performance of the device and process compatibility. .

Method used

Using high etching selection ratio material as the sacrificial layer, etching is carried out through an etching solution that does not damage the channel material to form a suspended space, achieving the formation of multi-layer vertical nanosheet structures, and building a ring-gate stacked nanosheet field effect on it transistor.

Benefits of technology

The channel material is suspended, the process complexity is reduced, the device performance and compatibility is improved, and the preparation method of high-performance transistors is provided, which is suitable for the construction of high-performance logic circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008531A_ABST
    Figure CN119008531A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a gate-all-around stacked nanosheet field effect transistor, and belongs to the field of semiconductor devices. The preparation method comprises the following steps: cleaning an insulating substrate; depositing a sacrificial layer; depositing an oxide semiconductor channel material; repeatedly depositing a sacrificial layer and a channel material; defining and etching a channel isolation region; defining and depositing a source-drain contact electrode; etching the sacrificial layer at a high selection ratio to form a multi-layer nanosheet structure with a suspension space; defining and depositing a gate oxide layer; and defining and depositing a gate metal electrode, and finally etching the stacked gate to form the ring gate stacked nanosheet field effect transistor. The sacrificial layer is removed through a high-etching-selection-ratio etching process to achieve a suspension space, the device performance and the device density are improved through the vertical stacking structure, and a feasible technical path is provided for industrial application of the gate-all-around stacked nanosheet field effect transistor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a method for preparing a ring-gate stacked nanosheet field effect transistor with a high etching selectivity. Background Art

[0002] The development of integrated circuits has improved the performance, integration density and parallel computing capabilities of silicon complementary metal oxide semiconductor (CMOS) transistors by reducing their size, and reducing power consumption and cost. However, as the size of silicon transistors gradually approaches the physical limit, the short channel effect becomes more and more serious, and it will become increasingly difficult to continue this trend at new technology nodes. In order to suppress the short channel effect, multi-gate structure devices such as double-gate, triple-gate, fin-type gate, and ring-gate have emerged. Among them, stacked nanosheet ring-gate field effect transistors have better gate control capabilities and are compatible with existing fin-type field effect transistor (FinFET) process technology, making them a strong competitor to FinFET. However, stacked nanosheet ring-gate field effect transistors face the difficulties of difficult preparation of channel materials and high process complexity. In the selection of channel materials, wide-bandgap oxide semiconductors such as indium tin oxide and indium gallium zinc oxide can maintain good mobility and switching ratio in ultra-thin bodies, and can significantly suppress the short channel effect. Moreover, the material preparation process of amorphous oxide semiconductors can be achieved through traditional sputtering processes, which is compatible with existing CMOS processes and is an excellent candidate for large-scale preparation of stacked nanosheet ring-gate field effect transistors. In micro-nano processing technology, there is a lack of high-selectivity etching processes to etch the sacrificial layer that supports the channel material. Methods of etching the SiO2 sacrificial layer using hydrofluoric acid vapor and the like can quickly remove the sacrificial layer, but this will damage the oxide semiconductor channel. Therefore, it is necessary to optimize the selection of sacrificial layer materials and the etching process at the same time, thereby providing an excellent method for preparing high-performance transistor devices and applying them to the construction of high-performance logic circuits. Summary of the invention

[0003] The present invention provides a method for realizing channel suspension by using a high etching selectivity ratio material as a sacrificial layer and completing the preparation of a ring-gate stacked nanosheet field effect transistor.

[0004] The technical solution of the present invention is as follows:

[0005] A method for preparing a ring-gate stacked nanosheet field effect transistor, wherein the field effect transistor is a vertical ring-gate structure, characterized in that a high etching selectivity material is used as a sacrificial layer to form a multi-layer vertical ring-gate nanosheet channel material interconnected together, and the specific preparation includes the following steps:

[0006] 1) Cleaning the insulating substrate;

[0007] 2) depositing a sacrificial layer, wherein the thickness of the sacrificial layer is in the range of 10-30 nm;

[0008] 3) depositing an oxide semiconductor channel material, wherein the thickness of the oxide semiconductor channel material is in a range of 2 nm to 20 nm;

[0009] 4) Repeat steps 2) to 3);

[0010] 5) Trench isolation region definition and etching:

[0011] 6) Definition and deposition of source and drain contact electrodes;

[0012] 7) using an etching solution that does not damage the channel material to etch the sacrificial layer with a high selectivity ratio to form a multi-layer vertical nanosheet structure with suspended spaces;

[0013] 8) depositing a gate oxide layer around the suspended space and on the source and drain contact electrodes;

[0014] 9) filling a gate metal electrode in the suspended space, and depositing a gate metal electrode on the gate oxide layer on the source and drain contact electrodes;

[0015] 10) Etching the stacked gate to form a ring-gate stacked nanosheet field effect transistor.

[0016] Furthermore, the insulating substrate in step 1) is a high-resistance silicon with a surface thermally oxidized silicon dioxide layer, or a high-resistance silicon, diamond, silicon carbide, or sapphire insulating substrate.

[0017] Furthermore, in step 2), a sacrificial layer is prepared by magnetron sputtering, thermal evaporation, atomic layer deposition or electron beam evaporation, and the sacrificial layer is LiF, GaF2, Ge, AlN or Au.

[0018] Furthermore, in step 3), a magnetron sputtering process or an atomic layer deposition process is used to deposit an oxide semiconductor channel material, and the channel material is indium tin oxide, indium gallium zinc oxide, indium oxide or indium tungsten oxide.

[0019] Furthermore, in step 5), the etching process adopts inductively coupled plasma etching or ion beam etching.

[0020] Furthermore, in step 6), the source and drain electrodes are made of W, Pt, Pd, Ni, Au, Ti or TiN, and the source and drain contact electrode deposition process is an electron beam evaporation process.

[0021] Furthermore, in step 7), the etching solution is deionized water, ammonia / hydrogen peroxide solution or potassium iodide solution.

[0022] Further, in step 8), the gate oxide layer is HfO2, Al2O3, ZrO2, HfSiO, HfZrO, HfLaO, SiN xHigh-κ dielectric material, the oxide layer dielectric deposition process adopts atomic layer deposition process;

[0023] Furthermore, in step 9), the gate metal electrode is TiAl, TiAlN, TiN, AlN, TaC, TaSi or TaSiN, and the gate metal electrode deposition process adopts an atomic layer deposition process.

[0024] Furthermore, in step 10), the stacked gate etching process adopts inductively coupled plasma etching or ion beam etching.

[0025] The beneficial effects of the present invention are as follows:

[0026] 1) The etching process based on high etching selectivity and the growth and device preparation process of oxide semiconductor materials are compatible with the existing silicon-based CMOS process, which can realize back-end process integration and has the potential for mass production.

[0027] 2) Through the high etching selectivity ratio etching process such as water-soluble and alkali-soluble etching processes that can completely remove the sacrificial layer without damaging the channel material, it is easier to achieve the suspension of the channel material, providing a feasible technical path for the industrial application of ring-gate stacked nanosheet field-effect transistors. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 — Fig.10 Schematic diagram of the process flow for preparing a ring-gate stacked nanosheet field effect transistor with high etching selectivity in a specific embodiment of the present invention, wherein (a) is a cross-sectional view and (b) is a corresponding top view.

[0029] Fig.11 for Figure 1 — Fig.10 The legend in . DETAILED DESCRIPTION

[0030] In order to make the purpose, features and advantages of the present invention clearer, the specific implementation of the present invention is described in more detail below in combination with the specific process steps and specific parameters of the embodiments. In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention can be implemented in many other ways different from the description. Therefore, the present invention is not limited to the specific implementation disclosed below.

[0031] Step 1: Cleaning of insulating substrate, such as Figure 1 shown.

[0032] Select a high-resistance Si (111) substrate with good electrical insulation and a surface thermally oxidized silicon dioxide layer, where the resistivity of the high-resistance silicon substrate is >10 4Ω·cm. Use standard RCA to clean the substrate. First, soak it in RCA-1 (deionized water: ammonia: hydrogen peroxide = 5:1:1) at 65°C for 10 minutes to clean the particles, metal cations, organic matter and other contaminants on the substrate. After cleaning, blow it dry with high-purity nitrogen for later use;

[0033] Step 2: sacrificial layer deposition, e.g. Figure 2 shown.

[0034] Prepare a 10-30nm thick sacrificial layer by magnetron sputtering, thermal evaporation, electron beam evaporation or atomic layer deposition. Different sacrificial layer materials are selected according to different etching processes. In this example, 20nm Ge evaporated by electron beam is used as the sacrificial layer material;

[0035] Step 3: Deposition of oxide semiconductor channel materials, such as Figure 3 shown.

[0036] The 5nm thick semiconductor channel material ITO was prepared by radio frequency magnetron sputtering process;

[0037] Step 4: Repeated deposition of sacrificial layer and channel material, such as Figure 4 shown.

[0038] Repeat steps 2 and 3 to prepare a multi-layer sacrificial layer / semiconductor channel material stack.

[0039] Step 5: Trench isolation region definition and etching, such as Figure 5 shown.

[0040] The specific steps include:

[0041] 1. First, spin-coat the electron beam photoresist AR-P 6200.13 at 2000 rpm for 60 seconds, and bake at 150 °C for 60 seconds after spin coating;

[0042] 2. The trench isolation region is defined using a Raith Voyager electron beam exposure system with an electron beam dose of 200 μC cm -2 , denaturing the electron beam colloid;

[0043] 3. Development: Use developer MIBK for 60 seconds, IPA for 60 seconds, and then blow dry the sample with a high-purity nitrogen gun;

[0044] 4. Dry etching: Use inductively coupled plasma dry etching to remove the multi-layer sacrificial layer / channel layer in the isolation area;

[0045] 5. Remove the mask layer: Use the degumming liquid N-methylpyrrolidone (NMP) to heat bath at 120℃ for 3 hours to remove the AR-P6200.13 electron beam glue, then clean it in IPA for 2 minutes, and then blow dry it with a nitrogen gun.

[0046] Step 6: Source and drain contact electrode definition and deposition, such as Figure 6 shown.

[0047] The source and drain electrodes are prepared by processes such as coating, baking, electron beam lithography, development, electron beam evaporation, and stripping, including:

[0048] 1. First, based on the fifth step, spin-coat the electron beam photoresist PMMA, the spin-coating parameters are 2000rpm, the spin-coating time is 60 seconds, and the spin-coating is baked at 180°C for 90 seconds;

[0049] 2. The source and drain contact areas were defined using a Raith Voyager electron beam exposure system with an electron beam dose of 760 μC cm -2 , denaturing the electron beam colloid;

[0050] 3. Development: Use developer MIBK:IPA=1:3 for 60 seconds, fix with IPA for 60 seconds, and then blow dry the sample with a high-purity nitrogen gun;

[0051] 4. Electron beam evaporation: Use oxide evaporation mode to evaporate metal electrode materials, with an electrode thickness of 100-200nm;

[0052] 5. Stripping: Soak in acetone at 50°C for 60 minutes, rinse the sample surface with a pipette, wash off excess acetone in IPA, and then blow dry with a high-purity nitrogen gun to complete the preparation of source and drain metal electrodes.

[0053] Step 7: Etch the sacrificial layer with high selectivity, such as Figure 7 shown.

[0054] After the sixth step is completed, the sample is placed in a dilute hydrogen peroxide solution and rinsed for 3 minutes to ensure that the Ge sacrificial layer is completely removed, and then blown dry with high-purity nitrogen gas, thus forming a multilayer nanosheet structure with suspended space.

[0055] Step 8: Gate oxide layer definition and deposition, such as Figure 8 shown.

[0056] Atomic layer deposition of 5nm HfO2 is used as the gate dielectric around the suspended space and on the source and drain contact electrodes.

[0057] Step 9: Gate metal electrode definition and deposition, such as Fig. 9 shown.

[0058] Atomic layer deposition technology is used to deposit 15nm TiN as gate metal in the suspended space and on the gate oxide layer on the source and drain contact electrodes.

[0059] Step 10: Etch the stacked gate to form a ring-gate stacked nanosheet field effect transistor, such as Fig.10 shown.

[0060] The specific steps include:

[0061] 1. First, based on the ninth step, spin-coat the electron beam photoresist HSQ, the spin-coating parameters are 4000rpm, 60 seconds, and bake at 150℃ for 10 minutes after spin-coating;

[0062] 2. The trench isolation region is defined using a Raith Voyager electron beam exposure system with an electron beam dose of 3000 μC cm -2 , denaturing the electron beam colloid;

[0063] 3. Development: bake on a hot plate at 150°C for 10 minutes, develop with AR 300-44 (2.38% TMAH) for 90 seconds, fix with deionized water for 30 seconds, and then blow dry the sample with a high-purity nitrogen gun;

[0064] 4. Dry etching: Use inductively coupled plasma dry etching to remove the stacked gate and gate oxide layer outside the channel area;

[0065] 5. Remove the mask layer: Use NaOH solution wet etching or F-based gas dry etching to remove the HSQ mask, then rinse with deionized water to remove the residual acid solution, and then blow dry with a nitrogen gun.

[0066] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a gate-all-around stacked nanosheet field effect transistor, wherein the field effect transistor is a vertical gate-all-around structure. It is characterized in that A high etching selectivity material is used as a sacrificial layer to form a multi-layer vertical ring gate nanosheet channel material interconnected together. The specific preparation includes the following steps: 1) Cleaning the insulating substrate; 2) depositing a sacrificial layer, wherein the thickness of the sacrificial layer is in the range of 10-30 nm; 3) depositing an oxide semiconductor channel layer, wherein the thickness of the oxide semiconductor channel layer is in a range of 2 nm to 20 nm; 4) Repeat steps 2) to 3); 5) Trench isolation region definition and etching: 6) Definition and deposition of source and drain contact electrodes; 7) using an etching solution that does not damage the channel material to etch the sacrificial layer with a high selectivity ratio to form a multi-layer vertical nanosheet structure with suspended spaces; 8) depositing a gate oxide dielectric layer around the suspended space and on the source and drain contact electrodes; 9) filling the suspended space with a metal gate electrode, and depositing the metal gate electrode on the gate oxide dielectric layer of the source and drain contact electrodes; 10) Etching the stacked gate to form a ring-gate stacked nanosheet field effect transistor.

2. The preparation method according to claim 1, It is characterized in that The insulating substrate in step 1) is high-resistance silicon with a surface thermally oxidized silicon dioxide layer, or is a high-resistance silicon, diamond, silicon carbide, or sapphire insulating substrate.

3. The preparation method according to claim 1, It is characterized in that In step 2), a sacrificial layer is prepared by magnetron sputtering, thermal evaporation, atomic layer deposition or electron beam evaporation. The sacrificial layer is LiF, GaF 2 , Ge, AlN or Au.

4. The preparation method according to claim 1, It is characterized in that In step 3), a magnetron sputtering process or an atomic layer deposition process is used to deposit an oxide semiconductor channel material, wherein the channel material is indium tin oxide, indium gallium zinc oxide, indium oxide or indium tungsten oxide.

5. The preparation method according to claim 1, It is characterized in that In step 5), the etching process adopts inductively coupled plasma etching or ion beam etching.

6. The preparation method according to claim 1, It is characterized in that In step 6), the source-drain contact electrodes are made of W, Pt, Pd, Ni, Au, Ti or TiN, and the source-drain contact electrode deposition process is an electron beam evaporation process.

7. The preparation method according to claim 1, It is characterized in that In step 7), the etching solution is deionized water, ammonia / hydrogen peroxide solution or potassium iodide solution.

8. The preparation method according to claim 1, It is characterized in that In step 8), the gate oxide dielectric layer is HfO 2 、Al 2 O 3 、ZrO 2 , HfSiO, HfZrO, HfLaO or SiN x The gate oxide dielectric layer deposition process adopts an atomic layer deposition process.

9. The preparation method according to claim 1, It is characterized in that In step 9), the metal gate electrode is TiAl, TiAlN, TiN, AlN, TaC, TaSi or TaSiN, and the metal gate electrode deposition process adopts an atomic layer deposition process.

10. The preparation method according to claim 1, It is characterized in that In step 10), the stacked gate etching process adopts inductively coupled plasma etching or ion beam etching.