Interdigitated back contact solar cell with p-type conductivity
By using a patterned stack of tunnel oxide layer and n-type polycrystalline silicon layer on the back surface of p-type IBC solar cells, combined with a hydrogenated dielectric layer, the problem of high recombination rate caused by surface charge of the dielectric layer is solved, thereby improving cell efficiency and stability.
Patent Information
- Application Number
- CN202411105589.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-05-24
- Filing Date
- 2018-09-20
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the selection of passivation dielectric layer on the rear side of conventional p-type finger-type back contact solar cells is challenging, especially due to the high surface recombination rate caused by the surface charge of the dielectric layer, which affects the cell efficiency.
A patterned stack of tunnel oxide layer and n-type conductive doped polysilicon layer is used, combined with a hydrogenated dielectric layer. By forming gaps on the back surface and arranging Al-Si contacts and Ag contacts therein, the surface recombination is reduced by utilizing the silicon oxide surface passivation properties of the tunnel oxide layer and the hydrogen atom passivation of dangling bonds.
It effectively reduces the surface recombination rate of solar cells, improves open-circuit voltage and cell efficiency, avoids dielectric layer instability issues, and is suitable for high-temperature firing processes.
Smart Images

Figure CN119008722A_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese patent application No. 201880061080.8. Field of the Invention
[0002] The invention relates to a back-contacted p-type solar cell. In addition, the invention relates to a solar panel or photovoltaic module comprising at least one such solar cell. background
[0004] Conventional p-type interdigitated back-contacted (IBC) solar cells have either a p-type base or a diffused n-type emitter on their backside region. Choosing a dielectric layer that can passivate both regions equally well is a challenge. Most dielectric layers have a surface charge. Well-known passivating dielectric layers are aluminum oxide (aluminum oxide, Al2O3) with a negative surface charge and hydrogenated amorphous silicon nitride (a-SiN) with a positive surface charge. x :H).
[0005] If Al2O3 is applied over the entire rear surface of a p-type IBC solar cell, it has a beneficial effect on surface recombination at the p-type base region. In this case, electrons (minority carriers) are repelled while holes (majority carriers) are attracted, which is expressed as "accumulation". Since the minority carrier concentration is the limiting factor, it determines the surface recombination rate. In this way, the surface recombination rate at the p-type base surface can be reduced, which contributes to a high open circuit voltage. However, at the n-type region (emitter), the mechanism works in the opposite direction. Here, holes (minority carriers) are attracted and electrons (majority carriers) are repelled. This increases the surface recombination, also because the minority carrier concentration (holes) in this region now sets the recombination rate.
[0006] The effect becomes stronger if the doping concentration of the n-type emitter is reduced, which is generally beneficial to reduce surface recombination. e Concentration and electron capture cross section σ e The product of these parameters is equal to the hole N h , σ h (i.e. N e σ e =N h σ h ), the worst case occurs.
[0007] This situation is denoted "depleted" because the sum of the concentrations of electrons and holes is at such an extremely low level.
[0008] Hoex et al., “Surface passivation of phosphorus-diffused n+-type emitters by plasma-assisted atomic-layer deposited Al2O3”, Phys. Status SolidiRRL 6, No. 1, 4–6 (2012) / DOI 10.1002 / pssr.201105445, show the implicit V of non-metallized solar cells that illustrate this situation. oc The minimum value of ( Figure 3 , source as above).
[0009] Further reduction of the doping concentration causes a "reversal" of the emitter, meaning that the electron concentration becomes lower than the hole concentration. This may be beneficial in terms of reduced surface recombination, but will result in a non-functional solar cell.
[0010] On the contrary, dielectrics with positive surface charge (such as a-SiN x :H) is deposited on the p / n+ rear surface of a conventional p-type cell, the physics works in the opposite way. The positive surface charge has a beneficial effect on emitter surface recombination, and in general, the surface recombination current j0 decreases as the doped surface concentration decreases (which effectively means that the emitter sheet resistance increases).
[0011] However, on a low-doped p-type substrate, which typically has a resistivity of 1 Ω·cm to 3 Ω·cm, the strong positive surface charge causes a reversal. This implies that the base surface region becomes a surface charge-induced (i.e. non-diffusing) emitter extending toward the base contact. This is known to cause shunting, leading to extremely poor cell performance.
[0012] A possible solution to the above problem is to produce dielectric layers with (almost) zero surface charge. However, it has been shown that processing these dielectric layers is rather difficult. In addition, the passivation quality no longer depends on the field effect, but only on the so-called "chemical passivation", which is generally more difficult to achieve. An example of such a layer is intrinsic amorphous silicon, whose chemical surface recombination is very good under the restriction that the wet chemical pretreatment has very high standards. However, it is known that such layers are unstable at high temperatures and are therefore not suitable for combination with the mainstream firing process of screen-printed metal contacts.
[0013] It is an object of the present invention to overcome or reduce one or more of the problems of the prior art. SUMMARY OF THE INVENTION
[0015] The object is achieved by a back-contact solar cell based on a silicon substrate with p-type conductivity, the back-contact solar cell having a front surface for receiving radiation, and a back surface; wherein the back surface has a tunnel oxide layer and a doped polysilicon layer of n-type conductivity; the tunnel oxide layer and the doped polysilicon layer of n-type conductivity form a patterned layer stack having gaps therein; an Al-Si contact is arranged in each of the gaps in electrical contact with a base layer of the silicon substrate; and one or more Ag contacts are arranged on the patterned doped polysilicon layer and in electrical contact with the patterned doped polysilicon layer.
[0016] According to the present invention, a p-type IBC solar cell is provided having a patterned stack layer of a tunnel oxide and an n-type polysilicon emitter region. The tunnel oxide is typically 0.5 nm to 2 nanometers thick and can be prepared by wet chemical oxidation (e.g., using HNO3 solution) at high temperature or by gas-based oxidation.
[0017] In such solar cells, the passivation properties are determined by the silicon oxide surface of the tunnel oxide layer. In addition, the passivation of dangling bonds on the silicon substrate surface by hydrogen atoms plays a key role.
[0018] In one embodiment where the rear surface of a p-type IBC solar cell has an alternating structure of n-type polysilicon emitter regions and base regions, a dielectric having a negative surface charge, such as Al2O3 (or a dielectric layer including Al2O3 layers and a-SiN x : stack of H layers). The presence of the dielectric layer then causes the desired accumulation at the surface of the base region, while the tendency towards depletion is not disadvantageous, because firstly, the doping concentration in n-type polysilicon is quite high, and secondly, since the polysilicon layer is usually an order of magnitude thicker, the tendency towards depletion occurs at a distance of typically 10nm to 20nm and therefore does not affect the surface recombination at the tunnel oxide. In the case of n-type polysilicon, an important function of the dielectric layer is to provide hydrogen, which will migrate towards the tunnel oxide during the high temperature step (usually occurring during the firing of the contacts of the solar cell) and thereby greatly reduce the surface recombination.
[0019] In another embodiment, the back surface of the solar cell has an interdigitated electrode pattern including alternating regions of n-type polysilicon and intrinsic polysilicon. This can usually be prepared by sequentially depositing tunnel oxide and intrinsic polysilicon layers. Thereafter, a diffusion barrier pattern is applied, and diffusion of phosphorus atoms into the wafer surface occurs, for example, by POCl3 diffusion or by ion implantation. The diffusion barrier is subsequently removed. In this embodiment, surface passivation occurs at the tunnel oxide over the entire region. The hydrogenation of the tunnel oxide (wherein hydrogen atoms will be positioned at the dangling bonds on the silicon wafer surface) causes a very high degree of surface passivation. Since a polysilicon layer of about 200nm covers the tunnel oxide and the surface charge of the dielectric only affects the carrier concentration level at 10nm to 20nm of the outer polysilicon surface, the sign of the surface charge is no longer relevant. The only effect of the dielectric is that both intrinsic polysilicon and n-type polysilicon provide hydrogen. Therefore, in this embodiment, the choice of dielectric layer type is free. This means that the dielectric layer can be, for example, Al2O3, a-SiN x :H or a stack of these dielectric layers.
[0020] The invention also relates to a solar panel or photovoltaic module comprising one or more of the solar cells as described above.
[0021] According to an aspect, the invention relates to a method for manufacturing a back-contact solar cell based on a silicon substrate of p-type conductivity, the back-contact solar cell having a front surface for receiving radiation, and a back surface; the method comprising:
[0022] providing a layer stack of a tunnel oxide layer and a doped polysilicon layer of n-type conductivity on the rear surface, the tunnel oxide layer being arranged between the rear surface and the doped polysilicon layer; patterning the layer stack to have gaps in the layer stack; arranging an Al-Si alloyed contact within each of the gaps in electrical contact with the base layer of the substrate, and
[0023] One or more Ag contacts or transition metal contacts are disposed on and in electrical contact with the doped polysilicon layer of the patterned layer stack.
[0024] According to an embodiment, the method comprises: patterning the layer stack having gaps in the layer stack comprises depositing or generating a layer comprising SiO2 layers and / or SiN x layer, and locally removing the SiO2 layer and / or SiN x The layer patterns the cover layer by creating openings in the cover layer.
[0025] According to another embodiment, the method as described above includes: removing the patterned capping layer to expose the doped polysilicon layer; depositing a dielectric layer on the rear surface over the gap and the exposed patterned doped polysilicon layer; and creating an opening in the dielectric layer at the location of the gap by a laser beam.
[0026] Furthermore, the invention relates to a method for producing a back-contact solar cell based on a silicon substrate of p-type conductivity, the back-contact solar cell having a front surface for receiving radiation, and a back surface; the method comprising:
[0027] A layer stack of a tunnel oxide layer and an intrinsic polysilicon layer is provided on the rear surface, the tunnel oxide layer being arranged between the rear surface and the intrinsic polysilicon layer; a layer stack of a tunnel oxide layer and / or an intrinsic polysilicon layer is provided on the rear surface; x The cover layer of the layer covers the layer stack and produces a sintered SiO2 layer and / or SiN in the cover layer x Removal of unsintered SiO2 layers and / or SiN x Layer area; the unsintered SiO2 and / or SiN x The intrinsic polysilicon layer covering the patterned region of the layer is exposed to an n-type dopant species to produce an unsintered SiO2 layer and / or SiN x The pattern of the n-type doped polysilicon layer region covered by the layer; removing the patterned sintered SiO2 layer and / or SiN x layer regions so as to expose one or more regions of the intrinsic polysilicon layer; arrange Al-Si alloyed contacts on the one or more regions of the intrinsic polysilicon layer, and each of the Al-Si alloyed contacts is in electrical contact with a respective region of the intrinsic polysilicon layer; and produce a silver contact or a transition metal contact on one or more of the patterned n-type doped polysilicon layer regions and in electrical contact with the patterned n-type doped polysilicon layer regions.
[0028] According to an embodiment, the method comprises: producing a sintered SiO2 layer and / or SiN by using a laser beam as a local heat source for sintering x The pattern of the layer area.
[0029] According to an embodiment, the method as described above further comprises:
[0030] In the removal of the patterned sintered SiO2 layer and / or SiN x After depositing the n-type doped polysilicon region, a dielectric layer is deposited over the region of intrinsic polysilicon and the region of n-type doped polysilicon, and for one or more regions of intrinsic polysilicon, a gap or opening is created at a location in the dielectric layer covering the region of intrinsic polysilicon; wherein the gap or opening in the dielectric layer covering the region of intrinsic polysilicon is created by using a laser beam.
[0031] Advantageous embodiments are further defined by the dependent claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Embodiments of the present invention will hereinafter be described in more detail, by way of example only, with reference to the accompanying drawings, which are schematic in nature and are therefore not necessarily drawn to scale. In addition, corresponding reference characters in the drawings refer to corresponding or substantially similar elements.
[0034] In the accompanying drawings, Figure 1 schematically illustrates a cross section of a solar cell according to an embodiment of the present invention;
[0035] Figure 2 schematically shows a cross section of a solar cell according to the present invention;
[0036] Figure 3 schematically illustrates a cross section of a solar cell according to an embodiment of the present invention;
[0037] Figure 4 schematically illustrates a plan view of the rear surface of a solar cell according to an embodiment of the present invention;
[0038] Figure 5 Schematically shows Figure 4 A cross section of a solar cell;
[0039] Figure 6 schematically illustrates a plan view of the rear surface of a solar cell according to an embodiment of the present invention;
[0040] Figure 7 schematically illustrates a plan view of the rear surface of a solar cell according to an embodiment of the present invention;
[0041] Figure 8 shows a cross section of a solar panel comprising at least one solar cell according to an embodiment of the present invention;
[0042] Fig. 9 shows a cross section of a solar cell during various stages of a method according to an embodiment; and
[0043] Fig.10 Shown are cross sections of a solar cell during various stages of a method according to an embodiment. Specific implementation plan
[0044] The solar cell of the present invention is based on a p-type semiconductor substrate, and a positive polarity contact and a negative polarity contact are arranged on the rear surface of the substrate. The positive contact is directly connected to the p-type base layer of the substrate, and the negative contact is connected to the n-type doped region on the rear surface. Usually, the positive contact is implemented as a metal alloy contact, and the negative contact is implemented as a metal or metallic contact.
[0045] Figure 1 A cross section of a solar cell according to an embodiment of the present invention is schematically shown.
[0046] According to an embodiment of the present invention, a solar cell 1 comprises a silicon substrate 10 of p-type conductivity. For example, the silicon substrate is doped with boron as a dopant substance.
[0047] The silicon substrate 10 has a front surface F and a rear surface R.
[0048] A stack of a tunnel oxide layer 12 and a doped polysilicon layer 14 is arranged on the rear surface R. The layer stack 12 is patterned to the surface of the silicon substrate with a gap A. The tunnel oxide layer 12 is typically composed of silicon dioxide and typically has a thickness of about 2 nanometers or less.
[0049] The patterned doped polysilicon layer 14 has n-type conductivity, which is opposite to the p-type conductivity of the silicon substrate. The thickness of the n-type patterned polysilicon layer is about 10 nm to about 300 nm.
[0050] In the pattern of the patterned n-type doped polysilicon layer, there is a gap A. In the gap A, the contact 16 of the first conductivity type is positioned to be connected to the silicon substrate 10, i.e., the base of the solar cell. In this embodiment, the contact of the first conductivity type is a metal alloy contact, typically an Al-Si contact. Optionally, this contact contains boron. Such Al-Si contacts are typically composed of a layered structure including an Al head 160, an Al-Si alloy layer 161, and an Al-doped BSF region 162. Optionally, layer 160, layer 161, and layer 162 contain boron. The BSF region 162 is typically in contact with the silicon matrix of the substrate and encapsulates the Al-Si alloy layer 161. The Al head 160 is positioned on the top of the Al-Si alloy layer at the rear surface R and extends from it. The lateral dimensions of the Al-Si contact at the substrate level are smaller than the lateral dimensions of the gap A to avoid contact with the interface region of the n-type doped polysilicon.
[0051] A contact 18 of a second conductivity type opposite to the first conductivity type is arranged on and electrically contacts the patterned n-type doped polysilicon layer 14. According to the present invention, the contact 18 of the second conductivity type is implemented as a metal contact, in an embodiment, an Ag contact or alternatively a transition metal (e.g., Ni-Cu plated, possibly by photoinduced plating) contact. The lateral dimensions of the Ag contact 18 are smaller than the lateral dimensions of the patch of patterned n-type doped polysilicon on which the Ag contact is positioned.
[0052] The patterned n-type doped polysilicon layer 14 and the opening A are covered by a hydrogenated dielectric layer 20. Such a hydrogenated dielectric layer 20 improves the passivation of the rear surface (i.e., the interface between the tunnel oxide and the surface of the silicon substrate 10) by providing hydrogen to shield the electrically active defects at the rear surface R (e.g., dangling bonds at the silicon surface). The hydrogenated dielectric layer 20 may include hydrogenated silicon nitride SiN x :H layer 24, aluminum oxide (Al2O3) layer 22 or a dielectric layer stack of these layers 22, 24. In such a dielectric layer stack, the aluminum oxide layer 22 is positioned at the rear surface of the substrate and the SiN x :H layer 24 in the middle, because SiN x :H layer can have a positive surface charge.
[0053] The Al—Si contact 16 and the Ag contact 18 both extend through the hydrogenated dielectric layer to make electrical contact with the base of the silicon substrate 10 and the patterned n-type doped polysilicon layer 14 , respectively.
[0054] In an embodiment, the hydrogenated dielectric layer is configured to have a negative surface charge. Such negative surface charge affects the distribution of minority and majority charge carriers in the silicon substrate, which beneficially reduces recombination effects as explained in the introduction.
[0055] In the embodiment, the front surface F receiving the radiation is formed by an Al2O3 layer 30 bordering the silicon substrate 10 of p-type conductivity and a SiN layer on top of the Al2O3 layer. x :H layer 32 coverage.
[0056] In another embodiment, the front surface F that will receive radiation is covered by an intrinsic polysilicon layer 30A and an anti-reflective coating 32A (e.g., silicon nitride). Since intrinsic polysilicon is known to parasitically absorb blue light, a solar cell with such an intrinsic polysilicon layer 30A can be used as a bottom solar cell in a tandem device, where the bottom cell mainly collects near-infrared light and the parasitic absorption of the intrinsic polysilicon is relatively low.
[0057] In case the front surface F is configured with only one anti-reflection coating, the solar cell 1 will suffer less from parasitic blue light absorption.
[0058] Figure 2 A cross section of a solar cell 2 according to an embodiment of the present invention is schematically shown.
[0059] Solar cell 2 according to this embodiment includes silicon substrate 10 of p-type conductivity.
[0060] The tunnel oxide layer 12 is disposed on the rear surface R. The patterned n-type doped polysilicon layer 14 is disposed on the tunnel oxide layer 12 .
[0061] Within the pattern of the patterned n-type doped polysilicon layer, there is a region of intrinsic polysilicon layer 26 that interfaces with n-type doped polysilicon 14. In this embodiment, tunnel oxide layer 12 also exists between intrinsic polysilicon layer 26 and rear surface R of silicon substrate 10.
[0062] In the intrinsic polysilicon region 26, the first conductivity type metal alloy contact 16, the first conductivity type metal alloy contact 160, the first conductivity type metal alloy contact 161, the first conductivity type metal alloy contact 162 (usually Al-Si contacts) are positioned to connect to the silicon substrate 10, i.e., the base of the solar cell. The lateral dimensions of the Al-Si contacts are smaller than the lateral dimensions of the region of the intrinsic polysilicon layer 26.
[0063] A metal contact 18 of the second conductivity type (eg, an Ag contact) is disposed on and electrically contacts the patterned n-type doped polysilicon layer 14, as described above with reference to Figure 1 described.
[0064] In this embodiment of the solar cell 2, the regions of the patterned n-type doped polysilicon layer 14 and the intrinsic polysilicon layer 26 are covered with hydrogenated silicon nitride SiN. x :H layer 24 covers, the SiN x The H layer 24 beneficially provides hydrogen for passivating the rear surface.
[0065] Al—Si contacts 16 , 160 , 161 , 162 and Ag contacts 18 extend through the hydrogenated dielectric layer to make electrical contact with the base of the silicon substrate 10 and the patterned n-type doped polysilicon layer 14 , respectively.
[0066] Figure 3 A cross section of a solar cell 3 according to an embodiment of the present invention is schematically shown.
[0067] Figure 3 The solar cell shown in FIG. 1 may be considered as described above with reference to Figure 2 Variants of the described solar cell 2 .
[0068] The tunnel oxide layer 12 is disposed on the rear surface R. The patterned n-type doped polysilicon layer 14 is disposed on the tunnel oxide layer 12 .
[0069] Within the pattern of the patterned n-type doped polysilicon layer, there is a region of an intrinsic polysilicon layer 26 that interfaces with the n-type doped polysilicon 14. A tunnel oxide layer 12 also exists between the intrinsic polysilicon layer 26 and the rear surface R of the silicon substrate.
[0070] Ag contact portion 18 Figure 2 is shown positioned on the patterned n-type doped polysilicon 14 .
[0071] In the region of the intrinsic polysilicon layer 26 , the Al—Si contacts 16 , 160 , 161 , 162 are arranged in electrical contact with the base layer of the silicon substrate 10 .
[0072] In this embodiment of the solar cell, the intrinsic polysilicon and the n-type doped polysilicon are covered by an aluminum oxide layer 22 which acts as a hydrogenated dielectric layer that provides hydrogen for surface passivation at the tunnel oxide.
[0073] The Al-Si contacts 16, 160, 161, 162 are positioned between the side-bounding elements 28, which are composed of a material characterized as being an inert material relative to the aluminum oxide dielectric, aluminum, and the Al-Si alloy. The bounding elements 28 are arranged on the stack of aluminum oxide 22 and the intrinsic polysilicon layer 26, which has been shown to be a stable configuration during the thermal treatment used to form the Al-Si contacts 16.
[0074] In an embodiment, the delimiting element material comprises aluminum oxide particles. Furthermore, the delimiting element material may comprise a material based on aluminum oxide or aluminum nitride.
[0075] The delimiting elements are configured to prevent undesirable Al-BSF formation at the edge of the Al. This reduces contact recombination. This is especially important if the Al paste is a fire-through paste with etchant particles (eg, glass frit).
[0076] Since the material of the delimiting element does not react with the dielectric layer or the silicon substrate at the annealing temperature, the delimiting element acts as an inert template during the annealing step. Typically, the annealing step is performed at about 660°C to about 800°C.
[0077] Additionally, because the pores (i.e., the width between the bounding elements) determine the surface area where the Al reacts with the Si, the bounding elements do not need to have a high aspect ratio and can have a circular cross-section or sloped sidewalls, such as mounds or embankments. The bounding elements can be printed in a similar manner to aluminum-based pastes (e.g., by screen printing).
[0078] Figure 4 Schematically showing the Figure 2 0 is a plan view of the rear surface of a solar cell of an embodiment of a solar cell 2 shown in . Al-Si contacts 16, Al-Si contacts 160, Al-Si contacts 161, Al-Si contacts 162, and Ag contacts 18 are arranged in the form of interdigitated electrodes on the rear surface R. The intrinsic polysilicon layer 26 and the n-type doped polysilicon layer 14 are arranged in a corresponding interdigitated pattern.
[0079] In the intrinsic polysilicon layer 26, elongated openings 34 to the silicon substrate have been created by laser scribing or by print etching paste. Al-Si contacts 16, 160, 161, 162 fill the elongated openings 34 and make electrical contact with the underlying silicon substrate, as shown in FIG. Figure 2 shown.
[0080] On the intrinsic polysilicon layer 26 , the Al head portion 160 of the Al—Si contact extends beyond the boundaries of the laser-scribed elongated opening 34 in both the lateral direction Y and the longitudinal direction X.
[0081] Both the Ag-contact interdigitated electrodes 18 and the Al—Si-contact interdigitated electrodes 16 are connected to respective bus bars 118 , 116 of n-type polarity and p-type polarity respectively, which extend in a transverse direction Y perpendicular to the longitudinal direction of the interdigitated electrodes 18 , 16 .
[0082] According to the present invention, bus bars 116 and 118 are both made of Ag (or Ag alloy). However, bus bars connecting Al-Si interdigitated electrodes may also be prepared in a similar manner to Al fingers. During manufacturing, the Ag bus bars are formed simultaneously with the Ag contacts (i.e., Ag interdigitated electrodes). The Ag bus bars used to connect the Al-Si contacts (Al-Si interdigitated electrodes) overlap 216 with the proximal ends of the Al-Si interdigitated electrodes 16 to obtain electrical contact. Typically, bus bars 116 and 118 have Ag interconnect pads.
[0083] It should be noted that for reference Figure 1 and Figure 3 The layouts of the described solar cells, interdigitated electrodes 16, 18 and bus bars 116, 118 are similar.
[0084] Figure 5 Schematically shows a cross section of a solar cell according to an embodiment of the present invention. In this embodiment, the Al-Si contact 16 (specifically, the Al head 160) is flanked by Ag sub-contacts 181, 182, thereby establishing electrical contact between the Al head 160 and the top of the intrinsic polysilicon layer 26, which acts as an interconnect pad for solder and electrically conductive adhesive (ECA). Figure 4 As shown in FIG, Ag bus bars are produced on both the n-type doped polysilicon 14 and the intrinsic polysilicon layer 26. This layout allows the use of two-step printing, one step for printing Ag and another step for printing Al, to produce interdigitated electrodes, interconnect pads, and bus bars. In the case of single-step Ag paste printing, the Ag paste is a burn-through paste that penetrates into the polysilicon. Since the intrinsic polysilicon is not conductive, this will not cause shunting.
[0085] Figure 6 A plan view of the rear surface of a solar cell according to an embodiment of the present invention is schematically shown. The layout of the interdigitated electrodes on the rear surface is similar to that described above with reference to Figure 4 Similar to the description. Figure 6 In the embodiment of the solar cell shown in FIG. 1 , the width W of the Al head 160 of the Al-Si contact 16 is greater than the width of the elongated intrinsic polysilicon layer 26 surrounding the elongated opening 34 to the silicon substrate. The Al head 160 is configured to overlap a portion of the adjacent n-type doped polysilicon layer 14.
[0086] It will be appreciated that Al is the limiting factor for the conductivity of the metallization (compared to Ag). Lower resistance is obtained by using a wider Al-Si contact. In addition, lateral conductivity can be improved by overlapping with n-type doped polysilicon (the other polarity). In addition, by changing the Al paste width, the alloying process can be adjusted. In this way, the Al layer size, alloy layer size, and BSF thickness (i.e., the formation of the layered stack of the Al head 160, the Al-Si layer 161, and the Al-based BSF region 162 and their respective thicknesses within the Al-Si contact 16) can be adjusted for optimal performance.
[0087] Figure 7 Schematically shows a plan view of the rear surface of a solar cell according to an embodiment of the present invention. In this embodiment, the Al-Si interdigitated electrode 16 has a series of intermittent elongated openings 36 in the intrinsic polysilicon layer 26 over the length of the electrode. Figure 4 and Figure 6Compared to the single elongated opening 34 shown in FIG. 1 , the series of discontinuous openings have a shorter contact length with the underlying silicon substrate 10. Thus, contact recombination can be advantageously reduced.
[0088] As shown therein, the layout of intermittent openings 36 may be combined with an Al head layer 160 that partially overlaps the adjacent n-type doped polysilicon 14 to tailor performance.
[0089] Figure 8 A cross section of a solar panel comprising at least one solar cell according to an embodiment of the invention is shown.
[0090] The present invention also relates to a solar panel 800 or a photovoltaic module, which comprises the above reference Figures 1 to 7 One or more back-contact solar cells 1 , 2 , 3 are described.
[0091] The solar panel 800 further includes a transparent top plate 802 , a top encapsulant 804 , a bottom encapsulant 806 , and a back sheet 808 .
[0092] One or more solar cells 1, 2, 3 are arranged on a back sheet 808 having a conductor pattern (not shown) that is electrically contacted with bus bars 116, 118 connected to the Al-Si interdigitated electrodes 16 and Ag interdigitated electrodes, respectively, through solder or conductive adhesive 810. A bottom encapsulation layer 806 is arranged between the rear surface R of the one or more solar cells and the back sheet having contact openings at locations where the bus bars 116, 118 are connected to the back sheet 808.
[0093] On top of the solar cell, over its front surface F, a top encapsulant 804 is arranged between the solar cell and the top transparent plate 802 .
[0094] It should be noted that the front surface and / or the rear surface R may have a pyramidal texture.
[0095] It should also be noted that the thickness of the silicon nitride layer 24 at the rear surface R can be adjusted to reflect radiation that has reached the rear surface R. Specifically, the thickness can be adjusted with reference to the minimum wavelength of the radiation. In an embodiment, the minimum wavelength can be about 900nm. The thickness can be at least about 80nm, or about 150nm or preferably about 200nm.
[0096] The solar cell according to the invention can be produced by various production methods. These methods are described below.
[0097] Nomenclature
[0098] FT = Burn Through
[0099] NFT=Non Burn Through
[0100] LCO = Local Contact Opening
[0101] PGR=POCl3 glass removal
[0102] SSE = Single Side Etching
[0103] A p-type interdigitated back contact (IBC) solar cell is fabricated on a boron-doped p-type silicon wafer. An emitter is present at the rear surface R, which does not face the sunlight and may or may not have a front surface field (FSF) on the front surface of the silicon substrate. Preferably, there is no FSF, as this eliminates costly processing steps (e.g., BBr3 diffusion), and furthermore, in general, a top surface without FSF has a lower surface recombination current density. In addition, the high temperature boron diffusion step may have an adverse effect on the quality of the base material. Since p-type wafers with resistivity ranging from 1Ω·cm to 3Ω·cm from ingots are standard, FSF may not be required to have sufficient conductivity in the base. The front Si surface is passivated by a dielectric layer or a stack layer. At the rear surface R, alternating emitter / base regions are formed by different patterning techniques. A p-type IBC cell with three different types of rear architectures will be described below. These rear architectures are:
[0104] I. Rear surface with diffused emitter regions alternating with base regions, where the entire surface is covered by a dielectric layer or a layer stack with a negative surface charge.
[0105] II. A rear surface in which n-type polysilicon emitter regions alternate with base regions, wherein the entire surface is covered by a hydrogen-providing dielectric layer or a layer stack with a negative surface charge.
[0106] III. A rear surface in which n-type polysilicon emitter regions alternate with intrinsic polysilicon regions, wherein the entire surface is covered by a hydrogen-providing dielectric layer or a layer stack with random surface charge.
[0107] The solar cell manufacturing process consists of the following steps:
[0108] 1. Prepare p-type wafers;
[0109] 2. Produce a patterned emitter;
[0110] 3. Surface passivation before application;
[0111] 4. Surface passivation after application;
[0112] 5. Opening of dielectric;
[0113] 6. Apply metallization.
[0114] These process steps are described in detail below.
[0115] 1. Preparation of p-type wafer (Table 1)
[0116] Table 1 Process steps for preparing single crystal wafers and multicrystalline wafers
[0117]
[0118] 2. Generate a patterned emitter (Table 2).
[0119] Table 2 Class I rear surface area (bare base area alternating with conventional diffused emitter area)
[0120]
[0121]
[0122] For Class II and Class III rear surfaces, a polysilicon layer of typically 10nm to 300nm is applied. Prior to polysilicon deposition, a very thin (e.g., 0.5nm to 2nm) silicon dioxide layer is created on the silicon surface. This can be achieved by in-situ deposition in a low pressure chemical vapor deposition (LPCVD) system or a plasma enhanced vapor deposition (PECVD) system, or by ex-situ chemical oxidation (e.g., NAOS, RCA, H2O2, etc.).
[0123] On top of the oxide layer, an intrinsic polysilicon layer or n-type in-situ doped polysilicon with a thickness of typically 10 nm to 300 nm is deposited by LPCVD or by PECVD. In practice, PECVD deposition mainly causes the deposition of amorphous silicon (a-Si), which can be converted into polysilicon by a high temperature step (annealing).
[0124] Table 3 Class II rear side (bare base region alternating with n-type polysilicon emitter)
[0125]
[0126]
[0127] Table 4 Class III rear side (alternating intrinsic polysilicon and n-type polysilicon regions)
[0128]
[0129] For specific embodiments of type II and type III solar cells, an intrinsic polysilicon layer may be intentionally retained on the front side. x) is applied on the front surface F, and after removing the POCl3 treatment, an intrinsic polysilicon layer on the front side can be obtained. Due to the good passivation properties of the oxide intrinsic polysilicon stack, this embodiment can have very low front surface recombination. However, the intrinsic polysilicon layer will parasitically absorb blue light. Therefore, the goal of this solar cell type is to act as a bottom solar cell in a series device.
[0130] 3. Surface passivation before application
[0131] For all Type I, Type II, Type III, a (wet) chemical cleaning step may be applied before the front coating deposition, which may be RCA-1, RCA-2, HNO3, (buffered) HF, HCl in different combinations and in different sequences.
[0132] The front coating can be Al2O3 or Al2O3-SiN x A stack or SiN x The preferred coating is Al2O3-SiN x The stack is made of 6nm Al2O3 and 80nm SiN x A stack of can achieve this purpose.
[0133] 4. Surface passivation after application
[0134] Table 5.
[0135]
[0136] It should be noted that the front dielectric layer can be co-deposited with the back dielectric layer. For example, for all types (I, II, and III), double-sided Al2O3 can be applied first, followed by double-sided SiN x A deposition system that allows the semi-finished product to float and float through the deposition chamber may be suitable for this purpose. It should be noted that unlike single-sided deposition, which may not require wraparound deposition, double-sided deposition has more relaxed processing conditions.
[0137] The rear surface will be opened at the base area by laser ablation or by printing a chemical etching paste. This is followed by a (wet) chemical cleaning to remove laser damage and dielectric coating flakes.
[0138] Optionally, the dielectric is opened in a similar manner at the emitter region, which can then be used to contact the NFTAg paste.
[0139] 5. Dielectric opening
[0140] An opening in the dielectric layer at the base region is achieved. Depending on the targeted aluminum printing area, this opening can be linear or a series of smaller lines or dots. The opening can be achieved by laser ablation or by selective chemical etching (e.g. by printing an etching paste). These steps can be followed by a chemical cleaning step. Optionally, a local contact opening (LCO) on the emitter region can be achieved in the same process steps. The LCO can then be used to form a metallic contact to the emitter by (screen) printing of NFT Ag paste or by (photoinduced) plating. It should be noted that for these types of metallization, the metal does not penetrate into the n-type polysilicon emitter or into a conventional diffused emitter.
[0141] 6. Apply metallization
[0142] The processes used for metallization are listed in Table 6. Three metal types are envisaged for (screen) printing: Al paste, FT Ag paste and NFT Ag paste. The latter will not burn through the dielectric layer. For NFT pastes, two categories can be identified: the first is co-fired with Al paste and FT Ag paste, and the second is mainly printed and fired separately at lower firing temperatures. The second paste type is usually called "floating busbar" paste.
[0143] The NFT paste is used to contact the Al paste. Both the NFT Ag paste and the FT paste can be electrically connected to metal leads that connect the solar cells in series in a photovoltaic module, either by solder or by a conductive adhesive.
[0144] In all cases, the Al paste is printed on the rear dielectric layer so that the LCO in the dielectric layer in the base region is fully covered. The Al paste area may also partially overlap with the emitter region.
[0145] BSF is formed by an aluminum-silicon alloying process, in which the aluminum in the screen-printed Al paste melts the silicon in the base wafer material and optionally the intrinsic polysilicon during heating to above 660°C (i.e., the melting point of aluminum), and during the cooling phase, the Al-doped silicon no longer melts and recrystallizes, also known as epitaxial growth.
[0146] Table 6 shows the metallization options for Class I, Class II, and Class III.
[0147] Table 6 Metallization Options
[0148]
[0149]
[0150] After the (screen) printing step, Solar Cell 1, Solar Cell 2, Solar Cell 3, Solar Cell I, Solar Cell II, Solar Cell III can undergo a thermal step, where the FT Ag paste penetrates the dielectric layer and contacts the conventional diffused emitter, the n-type polysilicon emitter or the intrinsic polysilicon.
[0151] FT Ag pastes may be selected among the pastes for PERC front side emitter contact. Examples of NFT Ag pastes for PERC solar cell rear surfaces are SOL326, SOL 326S from Heraeus, PV56x from DuPont, BS828B from ENC and GB21 from Gonda.
[0152] The BSF is formed by an aluminum-silicon alloying process, where the aluminum in the screen-printed Al paste melts the silicon in the base wafer material during heating to above 660°C, and melts the intrinsic polysilicon for the Class III surface area, where during the cooling phase the Al-doped silicon no longer melts and recrystallizes, which is also indicated as epitaxial growth.
[0153] All metal conductive pastes can be sintered by co-firing at a certain temperature (usually 700°C to 840°C). Due to the application of three different pastes, three printing steps are required to complete the metallization of this type of p-IBC solar cell. For Class III, there is an option to apply two printing steps (i.e. FT Ag paste and Al paste). In this case, the FTAg paste also penetrates the intrinsic polysilicon, but since this layer is not conductive, it does not cause shunting.
[0154] Fig. 9 A cross section of a solar cell is shown during various stages of a method according to an embodiment. Here, successive stages of the method are described.
[0155] In stage 901, a silicon substrate (silicon wafer) 10 is provided as the base of a solar cell. Typically, the silicon substrate is etched during this stage. The etching step may include a polishing etch. Alternatively or additionally, the etching step may include a first texturing etch followed by a second smoothing etch.
[0156] In phase 902, a stack of thin oxide layer 12 and n-type polysilicon layer 14 is created on both the front and back surfaces of the silicon substrate. The thin oxide layer acts as a tunnel oxide layer and is arranged between each of the surfaces of the silicon substrate 10 and the n-type polysilicon layer 14.
[0157] In the next stage 903, a SiO2 layer or SiN2O3 indicated by the symbol 40 is produced on top of the n-type polysilicon layer on the back side of the silicon substrate (ie the side of the substrate where the back contact will be formed). xPreferably, a SiO2 layer or a SiN layer is produced on the back side of the silicon substrate 10 by plasma enhanced chemical vapor deposition PECVD. x Layer 40.
[0158] Then in a subsequent stage 904, the laser beam 50 is used to create a gap 42 or opening 42 in the cover layer 40 on the rear surface. The laser beam 50 is configured to selectively remove the SiO2 layer and / or SiN at predetermined locations on the rear surface. x Layer 40. Thus, a patterned SiO2 layer and / or SiN x Layer 40 - 1 , wherein gaps or openings 42 expose the underlying n-type polysilicon layer.
[0159] Then, in stage 905, the substrate is exposed to a full-side alkaline etch. The alkaline etch selectively removes the exposed polysilicon layer 14 and thin oxide 12 at the rear surface, while using a patterned SiO2 layer or SiN x Layer 40-1 acts as a shielding layer. Therefore, in the patterned SiO2 layer or SiN x In the gap or opening 42 in layer 40-1, the surface of substrate 10 is now exposed. At the same time, n-type polysilicon layer 14 and thin oxide layer 12 are removed from the front surface by alkaline etching. The alkaline etch may include a surfactant, and depending on its composition and temperature, the etch may be isotropic or anisotropic, resulting in a (random pyramidal) texture.
[0160] In stage 906, the alkaline etch is followed by a HF (hydrofluoric acid) etch, which now selectively removes the patterned SiO2 layer or SiN x Layer 40-1. A patterned layer stack of thin oxide 12-1 and n-type polysilicon 14-1 remains at the rear surface.
[0161] Subsequently, in stage 907, the silicon substrate including the patterned layer stack 12-1 and the patterned layer stack 14-1 on the rear surface is exposed to a dielectric layer Al2O3 layer 44 or SiN x Layer 44 or Al2O3 and SiN x Full-side deposition of the stack 44 of layers.
[0162] Finally, in stage 908, laser beam 52 is used to remove Al2O3 and / or SiN at locations 46 within gaps or openings 42 created earlier in stage 904. x Layer 44. Thus, at said location, a region portion of the silicon substrate is exposed.
[0163] At the exposed area portion at location 46, an Al-Si contact may be formed at a later stage, for example, as described above with reference to Figure 1 described.
[0164] The method involves: providing a layer stack of a tunnel oxide layer and a doped polysilicon layer of n-type conductivity on a rear surface, the tunnel oxide layer being arranged between the rear surface and the doped polysilicon layer; patterning the layer stack so as to have gaps in the layer stack; arranging an Al-Si alloyed contact within each of the gaps and in electrical contact with a base layer of a silicon substrate; and arranging one or more Ag contacts or transition metal contacts on the doped polysilicon layer of the patterned layer stack and in electrical contact with the doped polysilicon layer.
[0165] According to aspects of the method, patterning of a layer stack having gaps in the layer stack includes depositing or generating a layer including a SiO2 layer and / or a SiN x The SiO2 layer and / or SiN layer is locally removed by a laser beam. x The layer patterns the cover layer by creating openings in the cover layer.
[0166] In this exemplary embodiment, SiO2 and / or SiN x The layer is a sacrificial layer. Those skilled in the art will appreciate that the patterned SiO2 and / or SiN2 layers may be formed to form a barrier against alkaline etching. x Layers are a permanent way to modify methods.
[0167] In addition, it will be appreciated that the described stages may be combined with other intermediate processing steps not described herein. Such intermediate processing steps may be required for preparation, transport, intermediate cleaning, native oxide removal, etc.
[0168] Fig.10 A cross section of a solar cell is shown during various stages 1001 to 1008 of a method according to an embodiment. In this embodiment, the stack of thin oxide layer and n-type doped polysilicon layer is replaced by a stack of thin oxide layer 12 and intrinsic polysilicon layer 54. The term "intrinsic polysilicon" should be interpreted herein as undoped polysilicon or intentionally undoped polysilicon, i.e. the base dopant level is at least one order of magnitude lower than the n-type dopant level.
[0169] Here, successive stages of an embodiment of a method are described.
[0170] In stage 1001, a silicon substrate (silicon wafer) 10 is provided as the base of a solar cell. Typically, the silicon substrate is etched during this stage. The etching step may include a polishing etch. Alternatively or additionally, the etching step may include a first texturing etch followed by a second smoothing etch.
[0171] In phase 1002, a stack of thin oxide layer 12 and intrinsic polysilicon layer 54 is created on both the front and back surfaces of silicon substrate 10. The thin oxide layer acts as a tunnel oxide layer and is arranged between each of the surfaces of silicon substrate 10 and the intrinsic polysilicon layer.
[0172] In the next stage 1003, a SiO2 layer or SiN2O3 indicated by the symbol 40 is produced on top of the intrinsic polysilicon layer 54 on the back side of the silicon substrate 10 (ie the side of the substrate where the back contact will be formed). x Preferably, a SiO2 layer or a SiN layer is produced on the back side of the silicon substrate 10 by plasma enhanced chemical vapor deposition (PECVD). x Layer or combination of layers 40.
[0173] Then, in a subsequent stage 1004, a laser beam 56 is applied to the SiO2 layer or SiN x The laser beam is configured to selectively heat the SiO2 layer or SiN2 layer at a predetermined position 58 on the rear surface. x layer or a combination layer 40, thereby having a SiO2 layer or a SiN x The layer or combined layer 40 is structurally different from the SiO2 layer or SiN x The effect of modifying the portion 40-2 of the layer or combined layer 40 that is not irradiated by the laser beam 56. The structural modification at the predetermined location 58 may involve the irradiated SiO2 layer or SiN x Densification of a layer and / or a structural phase transition of said layer.
[0174] Then, in stage 1005, the substrate is exposed to a full-side HF etch. The HF etch selectively removes the SiO2 layer and / or SiN from the front and back surfaces. x The non-sintered portion 40 - 2 of the layer 40 .
[0175] The sintered polysilicon layer at the rear surface is retained and used as a patterned mask layer. In this way, the patterning is performed in a manner corresponding to the removal of the non-sintered SiO2 layer or SiN x The pattern of the locations of the layers exposes the intrinsic polysilicon on the rear surface.
[0176] After the HF etching process, the substrate undergoes an n-type doping process, which diffuses the n-type dopant into the exposed intrinsic polysilicon to produce n-type doped polysilicon 14 at the exposed locations. In an embodiment, the n-type dopant is phosphorus. The doping process can be the well-known POCl3 process, which uses phosphorus oxychloride as a precursor.
[0177] After stage 1005, the sintered SiO2 layer or SiN xBelow the layer region 41 , the polysilicon layer remains as an intrinsic polysilicon layer 54 - 1 .
[0178] In the next stage 1006, an HF etch is applied to remove the sintered oxide layer and (if present) the phosphorus glass produced by the POCl3 process, and then a single side etch is performed on the front surface of the silicon substrate 10. In this process, as shown in stage 1006, the n-type polysilicon 14 and the thin oxide layer 12 remain on the back surface but are removed from the front surface.
[0179] On the rear surface, a patterned polysilicon layer including a region of the intrinsic polysilicon layer 54 - 1 and a region of the n-type doped polysilicon 14 remains. A thin oxide layer 12 is disposed between the patterned polysilicon layer 14 , the patterned polysilicon layer 54 - 1 and the substrate 10 .
[0180] Subsequently, in stage 1007, the substrate 10 including the patterned polysilicon layer 14 and the patterned polysilicon layer 54-1 stacked on the thin oxide layer 12 on the rear surface is exposed to full-side deposition of a hydrogen-providing dielectric coating, which may be an Al2O3 layer or a SiN x Layer or Al2O3 and SiN x A stack of layers.
[0181] Finally, in stage 1008, laser beam 60 is used to remove Al2O3 and / or SiN at location 62 above intrinsic polysilicon layer 54-1 created earlier in stage 1005. x Layer 44 is opened or exposed. Thus, at location 62, a region portion of the intrinsic polysilicon layer 54-1 is exposed. At the exposed region portion, an Al-Si contact (not shown) may be formed at a later stage by depositing aluminum on the intrinsic polysilicon and subsequently annealing.
[0182] In this embodiment, the method involves: providing a layer stack of a tunnel oxide layer and an intrinsic polysilicon layer on the rear surface, the tunnel oxide layer being arranged between the rear surface and the intrinsic polysilicon layer; x The cover layer covers the layer stack and produces a sintered SiO2 layer and / or SiN x patterning of the layer area; removal of unsintered SiO2 layers and / or SiN x Layer area; unsintered SiO2 and / or SiN x The intrinsic polysilicon layer covering the patterned region of the layer is exposed to an n-type dopant species to produce an unsintered SiO2 layer and / or SiN x The pattern of the n-type doped polysilicon layer region covered by the layer; removing the patterned sintered SiO2 layer and / or SiN xThe invention relates to a method for forming an n-type doped polysilicon layer region so as to expose one or more regions of the underlying intrinsic polysilicon layer; arranging an Al-Si alloyed contact on the one or more regions of the intrinsic polysilicon layer, wherein each of the Al-Si alloyed contact is in electrical contact with a respective region of the intrinsic polysilicon layer; and producing an Ag contact or a transition metal contact on one or more of the patterned n-type doped polysilicon layer regions and in electrical contact with the patterned n-type doped polysilicon layer regions.
[0183] According to an embodiment, the method further comprises: producing a sintered SiO2 layer and / or SiN by using a laser beam as a local heat source for sintering x The pattern of the layer area.
[0184] According to an embodiment, the method further comprises removing the patterned sintered SiO2 layer and / or SiN x A step after the layer region: depositing a dielectric layer over the region of intrinsic polysilicon and the region of n-type doped polysilicon, and for one or more regions of intrinsic polysilicon, creating a gap or opening at a location in the dielectric layer covering the region of intrinsic polysilicon, wherein the gap or opening in the dielectric layer covering the region of intrinsic polysilicon is created by using a laser beam.
[0185] In the foregoing description, the invention has been described with reference to specific embodiments thereof. However, it will be apparent that various modifications and changes may be made thereto without departing from the scope of the invention as outlined in the appended claims.
[0186] In addition, many modifications may be made to adapt a particular situation or material to the teachings of the invention without departing from the essential scope thereof. Those skilled in the art will appreciate that the exemplary embodiments described above may be modified and combined within the scope and spirit of the invention.
[0187] Therefore, it is intended that the invention not be limited to the particular embodiments disclosed, but that the invention will include all embodiments falling within the scope of the appended claims.
Claims
1. A back-contact solar cell based on a silicon substrate of p-type conductivity, having a front surface for receiving radiation, and a back surface; wherein the rear surface of the back-contact solar cell has a tunnel oxide layer and a doped polysilicon layer of n-type conductivity; the tunnel oxide layer and the doped polysilicon layer of n-type conductivity form a patterned layer stack having an opening exposing a base layer at the rear surface of the substrate; wherein an Al-Si alloyed contact is arranged within each of the openings exposing the base layer at the rear surface of the substrate, in direct and electrical contact with the base layer of the substrate, and One or more Ag contacts or transition metal contacts are disposed on and in electrical contact with the patterned doped polysilicon layer, The solar cell includes an intrinsic polysilicon layer, which interfaces with the patterned doped polysilicon layer of n-type conductivity and covers the base layer of the silicon substrate in the opening exposing the rear surface of the substrate, the tunnel oxide is additionally arranged between the intrinsic polysilicon layer and the base layer of the silicon substrate in the opening exposing the rear surface of the substrate, and the Al-Si contact extends through the intrinsic polysilicon layer and the tunnel oxide layer.
2. The solar cell of claim 1, wherein a hydrogen-providing dielectric layer is arranged to cover the intrinsic polysilicon layer and the patterned doped polysilicon layer, and the Al-Si contact and the Ag contact or transition metal contact each extend through the hydrogen-providing dielectric layer.
3. The solar cell of claim 2, wherein the hydrogen-providing dielectric layer comprises a-SiN x :H layer, Al2O3 layer, or a-SiN x : A stack of H layers and Al2O3 layers.
4. The solar cell of claim 2 or 3, wherein the hydrogen donating dielectric layer has a negative surface charge. 5 . The solar cell of claim 1 , wherein the tunnel oxide layer has a thickness of 0.5 nm to 2 nm, and the doped polysilicon layer or the intrinsic polysilicon layer has a thickness of 10 nm to 300 nm.
6. The solar cell of claim 1 , wherein the Al-Si alloyed contact is composed of a layered structure including an Al head, an Al-Si alloy layer, and an Al-doped BSF region, wherein the Al-doped BSF region contacts the silicon matrix or base region of the substrate and encapsulates the Al-Si alloy layer, and the Al head is positioned on top of the Al-Si alloy layer at the rear surface and extends from it. 7 . The solar cell of claim 1 , wherein the lateral dimensions of the Al—Si contacts at substrate level are smaller than the lateral dimensions of the gaps between the n-doped polysilicon regions.
8. The solar cell of claim 1, wherein the one or more Ag contacts interface with the Al-Si contacts on the intrinsic polysilicon layer.
9. The solar cell of claim 1, wherein the rear surface of the solar cell has an interdigitated electrode pattern including alternating regions of n-type polysilicon emitter regions and base regions, the base regions being covered by a stack of a tunnel oxide layer and an intrinsic polysilicon layer.
10. The solar cell of claim 1 , wherein the Al—Si contact and the Ag contact or transition metal contact are arranged as interdigitated electrodes between a first bus bar connecting the Ag contact or transition metal contact and a second bus bar connecting the Al—Si contact; the bus bar extending along the rear surface in a direction perpendicular to the length of the interdigitated electrodes. 11 . The solar cell according to claim 10 , wherein each of the bus bars consists of or includes Ag.
12. The solar cell of claim 1, wherein the Ag is based on a fired-through Ag paste material.
13. The solar cell of claim 10, wherein the Al-Si interdigitated electrode comprises a plurality of separate Al-Si contacts arranged along the length of the Al-Si interdigitated electrode, the plurality of Al-Si contacts being interconnected by an elongated Al or Al-Si alloy body extending over the plurality of Al-Si contacts.
14. The solar cell of claim 10, wherein a portion of the Al-Si interdigitated electrode extends laterally over a portion of an adjoining patterned doped polysilicon layer of n-type conductivity.
15. The solar cell of claim 2, wherein a laser scribed opening is positioned in said hydrogen providing dielectric layer above a location of said opening exposing said rear surface of said substrate.
16. The solar cell of claim 2, wherein a laser scribed opening is positioned in the hydrogen providing dielectric layer above the opening exposing the back surface of the substrate where the Al-Si contact is positioned, and wherein the laser scribed opening is positioned in the hydrogen providing dielectric layer, wherein the Ag contact or transition metal contact is positioned above the patterned doped polysilicon layer of n-type conductivity.
17. The solar cell of claim 16, wherein the Ag contact is based on a non-fired through Ag-based paste material.
18. The solar cell of claim 1 further comprising a dielectric layer on the front surface, the dielectric layer being configured with a negative surface charge.
19. The solar cell of claim 1 further comprising an intrinsic polysilicon layer on the front surface covered by a second hydrogen providing dielectric layer.
20. The solar cell of claim 2, wherein the Al-S contact is bordered at its edge by a delimiting element arranged on the hydrogen-providing dielectric layer, the delimiting element being composed of a material characterized by being an inert material relative to the hydrogen-providing dielectric layer material and aluminum.
21. A photovoltaic module comprising at least one solar cell as claimed in any one of the preceding claims, a transparent top sheet and a back sheet, wherein the at least one solar cell is arranged intermediate the top sheet and the back sheet.
22. Method for manufacturing a back-contact solar cell based on a silicon substrate of p-type conductivity, the back-contact solar cell having a front surface for receiving radiation, and a back surface; The method comprises: providing a layer stack of a tunnel oxide layer and a polysilicon layer on the rear surface of the back-contact solar cell, the tunnel oxide layer being arranged between the rear surface of the back-contact solar cell and the polysilicon layer; wherein the layer stack is patterned with regions of the layer stack where the polysilicon is doped with n-type conductivity and regions of the layer stack where the polysilicon is intrinsic; The region of the layer stack having doped polysilicon of n-type conductivity forms a patterned doped polysilicon layer; a region of the layer stack having intrinsic polysilicon formed on the base layer of the silicon substrate exposed at the rear surface of the substrate; a region of the layer stack in which the polysilicon is intrinsic formed over an opening in the patterned doped polysilicon layer; One or more Al-S i an alloyed contact is arranged on a region of the layer stack having intrinsic polysilicon, the Al-Si contact extending through the intrinsic polysilicon layer and the tunnel oxide layer in direct and electrical contact with the base layer of the substrate, and One or more Ag contacts or transition metal contacts are disposed on and in electrical contact with the doped polysilicon layer of the patterned layer stack.
23. The method of claim 22, wherein an intrinsic polysilicon layer is deposited and subsequently a barrier pattern for diffusion or implantation is applied and phosphorus atoms are applied by POCl3 diffusion or implantation and the barrier is then removed.
24. The method of claim 22, wherein the method further comprises: Before arranging the one or more Al-Si alloyed contacts on the region of the layer stack with intrinsic polysilicon and arranging the one or more Ag contacts or transition metal contacts on the doped polysilicon layer, arranging a hydrogen providing dielectric layer to cover the region of the layer stack with the intrinsic polysilicon and the region of the layer stack with the patterned doped polysilicon, respectively, so that the Al-Si contacts and the Ag contacts or transition metal contacts each extend through the hydrogen providing dielectric layer, and By selective chemical etching, gaps or openings are created in the hydrogen providing dielectric layer in the region covering the region of the intrinsic polysilicon by using a laser beam.
25. The method of claim 22, wherein the Al-Si alloyed contact is produced in an annealing step having a peak temperature of 600°C to 800°C.
26. The method of claim 22, wherein the Al-Si alloyed contact is produced in an annealing step at a temperature of 700°C to 840°C.
27. The method of claim 22, wherein the Al-Si alloyed contact is produced in an annealing step having a peak temperature above 660°C.
28. The method of claim 22, wherein the metallization contacts the base region in the opening by printing an Al paste pattern, and contacts the doped polysilicon region by printing an Ag paste pattern for bus bars, and then annealing to produce an Al-Si alloyed contact to the base region and an Ag contact to the doped polysilicon region.
29. A method for manufacturing a back-contact solar cell based on a silicon substrate of p-type conductivity, the back-contact solar cell having a front surface for receiving radiation, and a back surface; the method comprising: providing a layer stack of a tunnel oxide layer and an intrinsic polysilicon layer on the rear surface, the tunnel oxide layer being arranged between the rear surface and the intrinsic polysilicon layer; The SiO2 layer and / or SiN x A cover layer of the layer covers the layer stack and a sintered SiO2 layer and / or SiN x Pattern of layer area; Remove the unsintered SiO2 layer and / or SiN x Layer area; The SiO2 layer and / or SiN x The intrinsic polysilicon layer covering the pattern of layer regions is exposed to an n-type dopant species to produce SiO2 layers and / or SiN layers which are not sintered. x a pattern of an n-type doped polysilicon layer region covered by the layer; Remove the patterned sintered SiO2 layer and / or SiN x layer regions so as to expose one or more regions of the intrinsic polysilicon; disposing Al-Si alloyed contacts on one or more regions of the intrinsic polysilicon, each of the Al-Si alloyed contacts being in electrical contact with a respective region of the intrinsic polysilicon, and An Ag contact or a transition metal contact is created on and in electrical contact with one or more of the patterned n-doped polysilicon layer regions.
30. The method of claim 29, wherein the sintered SiO2 layer and / or SiN is produced by using a laser beam as a local heat source for sintering. x The pattern of the layer area.
31. The method of claim 29 or 30, further comprising: In the removal of the patterned sintered SiO2 layer and / or SiN x After forming the layer region, a dielectric layer is deposited over the region of the intrinsic polysilicon and the region of the n-type doped polysilicon, and for one or more regions of the intrinsic polysilicon layer, creating gaps or openings at locations in the dielectric layer overlying the regions of the intrinsic polysilicon layer; Wherein the gap or opening in the dielectric layer covering the region of the intrinsic polysilicon is created by using a laser beam.