Heterojunction solar cell and preparation method thereof, photovoltaic module and photovoltaic system

By forming a porous suede layer and an anti-reflective layer with a porous structure on the polishing substrate of a heterojunction solar cell, the problem of uneven passivation layer thickness is solved, the photoelectric conversion efficiency and stability of the battery are improved, and excellent photoelectricity is achieved performance.

CN119008732APending Publication Date: 2024-11-22TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411229530.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the preparation process, the passivation layer thickness is uneven due to the suede structure on the substrate surface, which affects the stability of the battery and the photoelectric conversion efficiency.

Method used

Using the first and second suede layers that polish the substrate and form a porous structure on its surface, and an anti-reflection layer, an uneven structure is formed by mask treatment, gel liquid coating and annealing treatment, reducing light reflection and improving Passivation effect.

Benefits of technology

The uniformity of the passivation effect and the anti-reflection effect are achieved, the photoelectric conversion efficiency and light stability of heterojunction solar cells are significantly improved, and the anti-reflection effect of conventional velvet substrates is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008732A_ABST
    Figure CN119008732A_ABST
Patent Text Reader

Abstract

The invention provides a heterojunction solar cell, a preparation method thereof, a photovoltaic module and a photovoltaic system. The heterojunction solar cell comprises a cell piece, the cell piece comprises a substrate, a first conducting layer and a second conducting layer, the substrate is a polished substrate, and the first conducting layer and the second conducting layer are located on the two opposite side faces of the substrate respectively; the first suede layer is located on the surface of the side, away from the substrate, of the first conductive layer, the second suede layer is located on the surface of the side, away from the substrate, of the second conductive layer, and the first suede layer and the second suede layer are each of a porous structure; the first anti-reflection layer is located on the surface of the side, away from the first conductive layer, of the first suede layer, and the second anti-reflection layer is located on the surface of the side, away from the second conductive layer, of the second suede layer. The heterojunction solar cell has excellent photoelectric conversion efficiency and illumination stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to a heterojunction solar cell and a preparation method thereof, a photovoltaic module, and a photovoltaic system. Background Art

[0002] As a clean and renewable energy technology, solar cells have great development prospects. With the continuous innovation of technology and the continuous decline in costs, the application areas of solar cells are constantly expanding, and they have great potential in the future energy field. Among solar cells, silicon-based heterojunction cells (HJT) have the advantages of high conversion efficiency and good temperature characteristics, and have attracted more and more attention in the industry in recent years.

[0003] In the process of preparing heterojunction cells, the substrate silicon wafer is first cleaned and textured to give the silicon substrate a surface roughness and textured structure, which can effectively reduce light reflection and improve the photoelectric conversion efficiency. However, the textured structure on the surface of the silicon substrate will lead to uneven thickness of the passivation layer deposited thereon, poor local passivation effect, and may even cause local loss of the passivation layer, thereby affecting the stability of the cell and the photoelectric conversion efficiency.

[0004] It should be noted that the above content is not necessarily prior art, nor is it intended to limit the scope of patent protection of this application. Summary of the invention

[0005] The embodiments of the present application provide a heterojunction solar cell and a preparation method thereof, a photovoltaic module, and a photovoltaic system to solve or alleviate the problems of poor stability and low photoelectric conversion efficiency of the battery mentioned above.

[0006] In a first aspect of the present application, the present application proposes a heterojunction solar cell, comprising:

[0007] A battery cell, the battery cell comprising a substrate, a first conductive layer and a second conductive layer, the substrate being a polished substrate, the first conductive layer and the second conductive layer being respectively located on two opposite side surfaces of the substrate; a first suede layer and a second suede layer, the first suede layer being located on a surface of the first conductive layer away from the substrate, the second suede layer being located on a surface of the second conductive layer away from the substrate, and both the first suede layer and the second suede layer having a porous structure; a first anti-reflection layer and a second anti-reflection layer, the first anti-reflection layer being located on a surface of the first suede layer away from the first conductive layer, and the second anti-reflection layer being located on a surface of the second suede layer away from the second conductive layer.

[0008] The heterojunction solar cell of the embodiment of the present application achieves the anti-reflection effect of the conventional velvet substrate while the passivation effect is more excellent, thereby showing excellent photoelectric conversion efficiency and light stability. This is because the substrate is a polished substrate, which has better flatness and smoothness than the conventional substrate, so that the thickness of the passivation layer formed on its surface is uniform, there is no phenomenon of local passivation effect disappearance, but a better passivation effect is presented, thereby significantly improving the light stability of the heterojunction solar cell; the first velvet layer and the second velvet layer have a porous structure, and this porous structure makes the first velvet layer and the second velvet layer present an uneven structure, which can reduce the reflection of light, thereby enhancing the absorption of sunlight by the heterojunction solar cell, and combined with the setting of the first anti-reflection layer and the second anti-reflection layer, the velvet structure formed by the first velvet layer and the first anti-reflection layer, and the velvet structure formed by the second velvet layer and the second anti-reflection layer can reduce the surface reflection loss of the heterojunction solar cell, that is, showing a good anti-reflection effect, thereby making the heterojunction solar cell of the embodiment of the present application show excellent photoelectric conversion efficiency. At the same time, the anti-reflection effect presented by the textured structure of the heterojunction solar cell of the present application can achieve the anti-reflection effect presented by the conventional silicon substrate texture.

[0009] According to an embodiment of the present application, the first suede layer and the second suede layer independently include at least one of silicon dioxide, titanium dioxide, and aluminum oxide.

[0010] According to an embodiment of the present application, the pore size of each pore in the porous structure is 10-100 nm.

[0011] According to an embodiment of the present application, the thickness of the first suede layer and the second suede layer are independently 50-200 nm.

[0012] According to an embodiment of the present application, the first anti-reflection layer and the second anti-reflection layer independently include at least one of magnesium fluoride and lithium fluoride.

[0013] According to an embodiment of the present application, the thickness of the first anti-reflection layer and the second anti-reflection layer are independently 50-100 nm.

[0014] In a second aspect of the present application, a method for preparing a heterojunction solar cell of the first aspect is proposed, the method comprising: performing mask processing on a cell to retain a grid line position, the cell comprising a polished substrate, a first conductive layer, and a second conductive layer; covering the first conductive layer and the second conductive layer of the cell after the mask processing with gel liquid respectively to form a gel layer; performing annealing processing on the cell containing the gel layer to form a first velvet layer having a porous structure and a second velvet layer having a porous structure; and depositing anti-reflection materials on the first velvet layer having a porous structure and the second velvet layer having a porous structure respectively to form a first anti-reflection layer and a second anti-reflection layer.

[0015] The method of the present application first performs masking on the cell and avoids the grid line position; the first conductive layer and the second conductive layer of the masked cell are respectively covered with gel liquid, and the cell covered with the gel layer is annealed to obtain a first velvet layer with a porous structure and a second velvet layer with a porous structure, and then the first velvet layer with a porous structure and the second velvet layer with a porous structure are respectively deposited with anti-reflection materials. The method is simple, easy to operate, and the process of covering with gel liquid is easy to control, and it will hardly affect other structures of the cell (such as over-etching during the etching process). The obtained heterojunction solar cell has a better passivation effect and achieves the anti-reflection effect of the conventional velvet substrate, thereby showing excellent photoelectric conversion efficiency and light stability.

[0016] According to an embodiment of the present application, the method for preparing the polished substrate includes: sequentially performing a rough polishing treatment and a phosphorus diffusion treatment on the substrate; and performing a fine polishing treatment on the phosphorus diffusion treatment product, wherein the fine polishing is performed in an alkaline polishing solution.

[0017] According to an embodiment of the present application, the masking process uses a tape as a mask plate, and the tape includes at least one of a polyimide tape and a polytetrafluoroethylene tape.

[0018] According to an embodiment of the present application, the gel solution contains silicon dioxide and polyethylene glycol.

[0019] According to an embodiment of the present application, the covering includes coating, and the gel liquid is coated by a spin coater. During the coating process, the spin coating speed of the spin coater is 2000-3000 rpm / min.

[0020] According to an embodiment of the present application, the annealing treatment takes 5-15 minutes at a temperature of 150-250°C.

[0021] According to an embodiment of the present application, the deposition method includes evaporation.

[0022] According to an embodiment of the present application, the method further includes removing the mask layer formed by the mask processing.

[0023] In a third aspect of the present application, a photovoltaic module is provided, wherein the photovoltaic module comprises a plurality of solar cells connected in series and / or in parallel; wherein at least one solar cell is a heterojunction solar cell according to the first aspect of the present application. A plurality of solar cells in series form a cell string, and adjacent heterojunction solar cells can be connected together by string welding.

[0024] The fourth aspect of the present application provides a photovoltaic system, comprising the photovoltaic assembly of the third aspect of the present application. The photovoltaic system also has the advantages of the above photovoltaic assembly, which will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.

[0026] Figure 1 It is a schematic diagram of the structure of a heterojunction solar cell according to some embodiments of the present application.

[0027] Description of reference numerals:

[0028] 1: substrate; 2: first intrinsic hydrogenated amorphous layer; 3: P-type microcrystalline silicon layer; 4: first conductive layer; 5: first velvet layer; 6: first anti-reflection layer; 7: first metal electrode; 8: second intrinsic hydrogenated amorphous layer; 9: N-type microcrystalline silicon layer; 10: second conductive layer; 11: second velvet layer; 12: second anti-reflection layer; 13: second metal electrode. DETAILED DESCRIPTION

[0029] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, the sizes of the layers and their relative sizes may be exaggerated for clarity. The same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other without conflict.

[0030] It should be understood that when a layer is referred to as being "on", "adjacent to", "connected to" or "coupled to" another layer, it may be directly on, adjacent to, connected to or coupled to the other layer, or there may be intervening layers. It should be understood that although the terms first, second, third, etc. may be used to describe various layers and / or portions, these layers and / or portions should not be limited by these terms. These terms are only used to distinguish one layer or portion from another layer or portion. Therefore, without departing from the teachings of the present application, the layer or portion discussed below may be represented as the second layer or portion. When the second layer or portion is discussed, it does not mean that the first layer or portion must exist in the present application.

[0031] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0032] In the present application, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values ​​in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to an integer in the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical range disclosed in the present application should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows for broadly including quantitative intervals such as percentage intervals, ratio intervals, and ratio intervals.

[0033] The process of preparing heterojunction solar cells includes depositing a passivation layer directly on the surface of the silicon wafer after texturing. When the passivation layer is formed on the silicon wafer, due to the inverted pyramid structure on the surface of the silicon wafer after texturing, the thickness distribution of the passivation layer is uneven, resulting in poor passivation effect in local areas of the heterojunction solar cell. When light irradiates the heterojunction solar cell, it will cause uneven light incidence, which in turn leads to uneven local current in the heterojunction solar cell, reducing the overall photoelectric conversion efficiency.

[0034] Accordingly, in a first aspect of the present application, the present application proposes a heterojunction solar cell. Figure 1 The battery comprises a battery cell, the battery cell comprises a substrate 1, a first conductive layer 4 and a second conductive layer 10, the substrate 1 is a polished substrate, the first conductive layer 4 and the second conductive layer 10 are respectively located on two opposite sides of the substrate 1; a first suede layer 5 and a second suede layer 11, the first suede layer 5 is located on a side surface of the first conductive layer 4 away from the substrate 1, the second suede layer 11 is located on a side surface of the second conductive layer 10 away from the substrate 1, and the first suede layer 5 and the second suede layer 11 have a porous structure; a first anti-reflection layer 6 and a second anti-reflection layer 12, the first anti-reflection layer 6 is located on a side surface of the first suede layer 5 away from the first conductive layer 4, and the second anti-reflection layer 12 is located on a side surface of the second suede layer 11 away from the second conductive layer 10.

[0035] The heterojunction solar cell of the embodiment of the present application achieves the anti-reflection effect of the conventional velvet substrate while the passivation effect is more excellent, thereby showing excellent photoelectric conversion efficiency and light stability. This is because the substrate is a polished substrate, which has better flatness and smoothness than the conventional substrate, so that the thickness of the passivation layer formed on its surface is uniform, there is no phenomenon of local passivation effect disappearance, but a better passivation effect is presented, thereby significantly improving the light stability of the heterojunction solar cell; the first velvet layer and the second velvet layer have a porous structure, and this porous structure makes the first velvet layer and the second velvet layer present an uneven structure, which can reduce the reflection of light, thereby enhancing the absorption of sunlight by the heterojunction solar cell, and combined with the setting of the first anti-reflection layer and the second anti-reflection layer, the velvet structure formed by the first velvet layer and the first anti-reflection layer, and the velvet structure formed by the second velvet layer and the second anti-reflection layer can reduce the surface reflection loss of the heterojunction solar cell, that is, showing a good anti-reflection effect, thereby making the heterojunction solar cell of the embodiment of the present application show excellent photoelectric conversion efficiency. At the same time, the anti-reflection effect presented by the textured structure of the heterojunction solar cell of the present application can achieve the anti-reflection effect presented by the conventional silicon substrate texture.

[0036] In some embodiments, the first suede layer and the second suede layer independently include at least one of silicon dioxide, titanium dioxide, and aluminum oxide. These materials have high physical and chemical stability and thermal stability, and can further improve the light stability of heterojunction solar cells.

[0037] As an example, the first velvet layer and the second velvet layer are independently made of silicon dioxide. Silicon dioxide has very high optical transparency in the visible light range, which is conducive to the incidence of light. At the same time, the refractive index of SiO2 is lower than that of silicon, which helps to reduce the reflection loss of incident light, thereby improving the absorption of light by the solar cell.

[0038] In some embodiments, the pore size of each pore in the porous structure is 10-100 nm, such as 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 80 nm, 90 nm, 100 nm, etc. The porous structure can exhibit a good anti-reflection effect, and the aforementioned pore size range can also make the layer have good mechanical properties to improve the reliability of long-term operation of heterojunction solar cells.

[0039] It is understandable that the pore size of each pore in the porous structure may be the same or different, as long as the pore size of these pores meets the range of 10-100 nm.

[0040] As an example, the heterojunction solar cell comprises: a cell, a first velvet layer, a second velvet layer, a first anti-reflection layer, and a second anti-reflection layer. The cell comprises a substrate, a first conductive layer, and a second conductive layer, the substrate is a polished substrate, the first conductive layer is located on the first surface of the substrate, and the second conductive layer is located on the second surface. The first velvet layer is located on the side surface of the first conductive layer away from the substrate, the second velvet layer is located on the side surface of the second conductive layer away from the substrate, and the first velvet layer and the second velvet layer have a porous structure. The first anti-reflection layer is located on the side surface of the first velvet layer away from the first conductive layer, the second anti-reflection layer is located on the side surface of the second velvet layer away from the second conductive layer, and the first velvet layer is a silicon dioxide velvet layer with a pore size of 10-100nm, and the second velvet layer is a silicon dioxide velvet layer with a pore size of 10-100nm.

[0041] In some embodiments, the thickness of the first suede layer and the second suede layer are independently 50-200 nm, such as 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, etc. Thus, the photoelectric conversion efficiency of the heterojunction solar cell is further improved.

[0042] According to the embodiments of the present application, the first anti-reflection layer and the second anti-reflection layer can prevent light incident on the heterojunction solar cell from the outside from being reflected to the outside again as much as possible.

[0043] In some embodiments, the first anti-reflection layer and the second anti-reflection layer independently include at least one of magnesium fluoride and lithium fluoride. These materials have a lower refractive index and can further reduce the reflection of incident light to the outside.

[0044] In some embodiments, the thickness of the first anti-reflection layer and the second anti-reflection layer is independently 50-200nm, such as 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 120nm, 150nm, 170nm, 190nm, 200nm, etc. Preferably, the thickness of the first anti-reflection layer and the second anti-reflection layer is independently 100-200nm, such as 100nm, 120nm, 150nm, 170nm, 190nm, 200nm, etc. The anti-reflection layer has a certain absorption and scattering effect on light. Controlling the thickness of the first anti-reflection layer and the second anti-reflection layer within the aforementioned range is conducive to reducing the interference effect of each layer of the solar cell and reducing the probability of outward reflection of the incident light, thereby improving the photoelectric conversion efficiency of the heterojunction solar cell.

[0045] In the examples of this application, refer to Figure 1 The heterojunction solar cell may also include a first intrinsic hydrogenated amorphous layer 2 and a second intrinsic hydrogenated amorphous layer 8, a P-type microcrystalline silicon layer 3, and an N-type microcrystalline silicon layer 9, wherein the first intrinsic hydrogenated amorphous layer 2 is located on a side surface of the substrate 1 close to the first conductive layer 4, the P-type microcrystalline silicon layer 3 is located on a side surface of the first intrinsic hydrogenated crystal layer 2 away from the substrate 1, the second intrinsic hydrogenated amorphous layer 8 is located on a side surface of the substrate 1 close to the second conductive layer 10, and the N-type microcrystalline silicon layer 9 is located on a side surface of the second intrinsic hydrogenated crystal layer 8 away from the substrate 1.

[0046] In the examples of this application, refer to Figure 1 , the heterojunction solar cell also includes a first metal electrode 7 and a second metal electrode 13. Wherein, the first metal electrode and the second metal electrode respectively and independently include a metal seed layer, a first electrode layer and a second electrode layer which are stacked, and the metal seed layer is in contact with the conductive layer. Specifically, the first metal electrode is in contact with the surface of the first conductive layer, the second metal electrode is released from the surface of the second conductive layer, and in the thickness direction of the heterojunction solar cell, part of the surface of the first metal electrode is in contact with both the first velvet layer and the first anti-reflection layer, and part of the surface of the second metal electrode is in contact with both the second velvet layer and the second anti-reflection layer. In this way, it is beneficial for the first metal electrode and the second metal electrode to draw out the current.

[0047] In a second aspect of the present application, a method for preparing a heterojunction solar cell according to the first aspect is provided, the method comprising:

[0048] (1) performing mask processing on the cell to retain the grid line position, the cell comprising a polished substrate, a first conductive layer and a second conductive layer; (2) covering the first conductive layer and the second conductive layer of the cell after the mask processing with gel liquid to form a gel layer; (3) performing annealing processing on the cell containing the gel layer to form a first velvet layer with a porous structure and a second velvet layer with a porous structure; (4) depositing anti-reflection materials on the first velvet layer with a porous structure and the second velvet layer with a porous structure to form a first anti-reflection layer and a second anti-reflection layer.

[0049] The method of the present application first performs masking on the cell and avoids the grid line position; the first conductive layer and the second conductive layer of the masked cell are respectively covered with gel liquid, and the cell covered with the gel layer is annealed to obtain a first velvet layer with a porous structure and a second velvet layer with a porous structure, and then the first velvet layer with a porous structure and the second velvet layer with a porous structure are respectively deposited with anti-reflection materials. The method is simple, easy to operate, and the process of covering with gel liquid is easy to control, and will not affect other structures of the cell (such as over-etching during the etching process). The obtained heterojunction solar cell has a better passivation effect and achieves the anti-reflection effect of the conventional velvet substrate, thereby showing excellent photoelectric conversion efficiency and light stability.

[0050] Specifically, the cell is masked to retain the main grid position, which is conducive to the subsequent production of electrodes for the cell. The gel layer is formed on the first conductive layer and the second conductive layer by coating. The method of covering the gel liquid is simple and easy to operate and easy to control thickness and other conditions, and does not cause any damage to the first conductive layer and the second conductive layer (such as over-etching during the etching process), and will hardly affect the conductive effect of the first conductive layer and the second conductive layer. The gel layer is a mesh structure formed by cross-linking of alternating particles and polymer molecules. The pores of the mesh structure are filled with liquid dispersion. The gel layer is annealed. The annealing treatment can remove the polymer molecules and liquid organic matter in the gel layer and leave holes. These holes make the first velvet layer present an uneven and porous structure. When external light is incident, the first velvet layer and the second velvet layer can reduce the reflection of the incident light to the outside world. A first anti-reflection layer is then deposited on the first velvet surface. The first anti-reflection layer also exhibits the same uneven and porous structure as the first velvet layer, so that the first anti-reflection layer not only reduces light reflection through its own material, but its uneven surface state can also further reduce light reflection.

[0051] According to an embodiment of the present application, in step (1), the cell is subjected to mask processing to retain the main grid, and the cell includes a polished substrate, a first conductive layer and a second conductive layer.

[0052] In some embodiments, in step (1), the preparation method of the polished substrate includes: sequentially performing a rough polishing treatment and a phosphorus diffusion treatment on the substrate; and performing a fine polishing on the phosphorus diffusion treatment product, wherein the fine polishing is performed in an alkaline polishing solution.

[0053] In some embodiments, phosphorus diffusion gettering introduces phosphorus atoms, causing them to migrate and capture these metal impurities during the high-temperature diffusion process, migrating them from the active area of ​​the silicon wafer to the inactive area, thereby increasing the minority carrier lifetime of the silicon wafer and improving the photoelectric conversion efficiency of the battery.

[0054] Further, the phosphorus source in the phosphorus diffusion process includes phosphorus oxychloride.

[0055] Furthermore, the atmosphere during the phosphorus diffusion process is a nitrogen and / or oxygen atmosphere.

[0056] Further, the diffusion temperature is 700-950°C, for example, 700°C, 750°C, 800°C, 900°C, 950°C, etc.

[0057] Furthermore, the diffusion time is 2-4 hours, such as 2 hours, 3 hours, 4 hours, etc.

[0058] In some embodiments, fine polishing is beneficial to remove the PSG (phosphosilicate glass) layer on the surface of the silicon wafer.

[0059] Furthermore, the alkaline polishing liquid includes an aqueous solution of potassium hydroxide, sodium hydroxide, or the like.

[0060] Furthermore, the concentration of the alkaline polishing solution is 2-30wt%, for example, 2wt%, 5wt%, 9wt%, 11wt%, 15wt%, 20wt%, 23wt%, 28wt%, 30wt% and the like.

[0061] Furthermore, the time for fine polishing is 100-300s, for example, 100s, 120s, 150s, 180s, 190s, 220s, 240s, 260s, 280s, 300s, etc.

[0062] In some embodiments, in step (1), the masking process uses adhesive tape as a mask plate. Using the adhesive tape as a mask plate is easy to remove in the subsequent electrode manufacturing process.

[0063] Furthermore, in step (1), the adhesive tape includes at least one of a polyimide tape and a polytetrafluoroethylene tape. These tapes are not only resistant to high temperatures to reduce burnout during subsequent annealing, but are also easy to remove and hardly leave residue on the conductive layer, thereby reducing adhesion between the electrode sheets after the tape is removed, and further reducing damage to the heterojunction solar cell caused by adhesion of the cell sheets. It also reduces the increase in resistance of the heterojunction solar cell caused by tape residue.

[0064] In some embodiments, the preparation of the battery cell includes: after fine-polishing the substrate, it also includes depositing a first hydrogenated amorphous layer and a second hydrogenated amorphous layer on two opposite sides of the fine-polished substrate, respectively, and then depositing a P-type microcrystalline silicon layer on the surface of the first hydrogenated amorphous layer away from the substrate, depositing an N-type microcrystalline silicon layer on the surface of the second hydrogenated amorphous layer away from the substrate, depositing a first conductive layer on the surface of the P-type microcrystalline silicon layer away from the substrate, and depositing a second conductive layer on the surface of the N-type microcrystalline silicon layer away from the substrate.

[0065] According to the present application, in step (2), the first conductive layer and the second conductive layer of the battery cell after the mask processing are respectively covered with gel liquid to form a gel layer.

[0066] In some embodiments, in step (2), the method of covering the gel liquid includes coating.

[0067] Optionally, the coating method includes spin coating.

[0068] Optionally, the gel solution is coated by a spin coater, and during the spin coating process, the rotation speed of the spin coater is 2000-3000rpm / min, for example, 2000rpm / min, 2100rpm / min, 2500rpm / min, 2600rpm / min, 2800rpm / min, 2900rpm / min, 3000rpm / min, etc.

[0069] Optionally, the spin coating time is 10-30 s, such as 10 s, 15 s, 20 s, 25 s, 30 s, etc.

[0070] In some embodiments, in step (2), the gel solution includes silicon dioxide and polyethylene glycol, wherein the polyethylene glycol escapes outward during the later annealing process, so that the first suede layer and the second suede layer form a porous structure.

[0071] Optionally, the amount of polyethylene glycol added to the gel solution is 10-15wt%, such as 10wt%, 11wt%, 12wt%, 13wt%, 15wt%, etc.

[0072] Optionally, the molecular weight of the polyethylene glycol is 200-1000.

[0073] Furthermore, the gel liquid is a silica gel liquid prepared by a sol-gel method. In the process of preparing the silica gel liquid by the sol-gel method, silicon alkoxide is used as a raw material, alcohol is used as a co-solvent, an acid or a base is added as a catalyst, and silicon alkoxide is hydrolyzed and polycondensed to form silica gel. In the silica gel prepared by the gel-sol method, the silica particles in the gel liquid act as a skeleton, cross-link with polymer molecules to form a three-dimensional network structure, and the catalyst is embedded in the pores of the network structure, which is conducive to the subsequent production of the first suede layer and the second suede layer.

[0074] According to the embodiment of the present application, in step (3), the cell sheet containing the gel layer is annealed to form a first velvet layer having a porous structure and a second velvet layer having a porous structure. In this step, the annealing treatment can remove non-silicon dioxide components (such as polyethylene glycol, polymer molecules and catalysts) in the gel solution, leaving only silicon dioxide as the skeleton of the first velvet layer and the second velvet layer, and the skeleton structure presents a porous structure due to the escape of polyethylene glycol and polymer molecules, thereby making the first velvet layer and the second velvet layer have a better anti-reflection effect.

[0075] Optionally, the annealing temperature is 150-250°C, such as 150°C, 180°C, 200°C, 220°C, 250°C, etc.

[0076] Optionally, the annealing time is 5-15 min, for example, 5 min, 7 min, 9 min, 11 min, 14 min, 15 min, etc.

[0077] According to an embodiment of the present application, in step (4), anti-reflection materials are deposited on the first suede layer and the second suede layer, respectively, to form a first anti-reflection layer and a second anti-reflection layer.

[0078] In some embodiments, in step (4), the depositing includes evaporation.

[0079] In some embodiments, the method further includes step (5) of removing the mask layer formed by the mask processing.

[0080] Furthermore, the mask layer includes the above-mentioned tape. Removing the tape and the tape residue is conducive to reducing the adhesion between the cells, thereby reducing the damage to the heterojunction solar cell caused by the adhesion of the cells. It also reduces the increase in the resistance of the heterojunction solar cell caused by the tape residue.

[0081] Furthermore, the method of removing the mask includes tearing off the mask and then cleaning and drying with acetone. This process ensures that there is no tape residue on the mask, which will not cause adhesion between battery cells, and the grid lines without tape residue have better current conduction effect.

[0082] In some embodiments, the method further comprises step (6), printing the metal electrode by screen printing or laser transfer.

[0083] In a third aspect of the present application, a photovoltaic module is provided, wherein the photovoltaic module comprises a plurality of solar cells connected in series and / or in parallel; wherein at least one solar cell is a heterojunction solar cell according to the first aspect of the present application. A plurality of solar cells in a series state form a cell string, and adjacent heterojunction solar cells can be connected together by string welding.

[0084] In the fourth aspect of the present application, a photovoltaic system is provided, comprising the photovoltaic assembly of the third aspect of the present application. The photovoltaic system also has the advantages of the above photovoltaic assembly, which will not be described in detail here.

[0085] In some embodiments, the photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it is understandable that the application scenarios of the photovoltaic system are not limited to this, that is to say, the photovoltaic system can be used in all fields that require solar energy to generate electricity. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to achieve solar power supply.

[0086] Hereinafter, exemplary embodiments according to the present application will be described in more detail with reference to the accompanying drawings. It should be noted that these exemplary embodiments can be implemented in many different forms and should not be construed as being limited to the embodiments described herein.

[0087] Example 1

[0088] S1: The silicon substrate after rough polishing is doped. The specific process of doping is to diffuse phosphorus into the silicon wafer. The phosphorus source is phosphorus oxychloride, the atmosphere is nitrogen and oxygen, the diffusion temperature is 850°C, and the time is 3 hours. The silicon wafer after doping is fine-polished with an alkaline aqueous solution. KOH solution is used for fine polishing with a concentration of 20wt%, to obtain a silicon substrate with a smooth surface (thickness of 140 microns).

[0089] S2: PECVD plasma deposition equipment is used to deposit a first intrinsic amorphous silicon layer with a thickness of 5nm on the front side of the polished silicon wafer, and a second intrinsic amorphous silicon layer with a thickness of 6nm is deposited on the back side of the silicon wafer. Intrinsic hydrogenated amorphous layers are deposited on both sides to achieve a passivation effect.

[0090] S3: Using PECVD plasma deposition equipment, a phosphorus-doped amorphous silicon layer (P-type doped layer) with a thickness of 8 nm is deposited on the surface of the first intrinsic amorphous silicon film layer, and a boron-doped amorphous silicon layer (N-type doped layer) with a thickness of 10 nm is deposited on the surface of the second intrinsic amorphous silicon film layer.

[0091] S4: A PVD magnetron sputtering device is used to deposit an ITO conductive film (first conductive layer) with a thickness of about 100 nm on the surface of the N-type amorphous silicon layer, and at the same time, an ITO conductive film (second conductive layer) with a thickness of about 100 nm is deposited on the surface of the P-type amorphous silicon layer to transmit carriers and enhance optical transmittance.

[0092] S5: Use special high-temperature tape (polyimide tape) to make a mask, retain the main grid position, and use spin coating to spin-coat a gel solution containing silicon dioxide and polyethylene glycol on the first conductive layer and the second conductive layer. The content of polyethylene glycol in the gel solution is 15wt%, the molecular weight is 500, and the spin coating speed is controlled at 2500rpm / min, and the spin coating time is 20s. Anneal the gelled battery cell at 200℃ for 10min to obtain the first velvet layer (thickness 105nm) and the second velvet layer (thickness 105nm) with a porous structure of the gel layer (pore size 60nm).

[0093] S6: using a vacuum evaporation device to deposit a first anti-reflection layer with a thickness of 70 nm and a second anti-reflection layer with a thickness of 70 nm on the first suede layer and the second suede layer respectively by evaporation, wherein the material is MgF2.

[0094] S7: After removing the masking tape and cleaning with acetone, blow drying in N2 atmosphere.

[0095] S8: Use screen printing or laser transfer printing to print metal electrodes. The metal electrodes are printed using conductive silver paste with a line width of 250um and a line height of 40um.

[0096] S9: Performing light injection treatment on the cell with the metal electrode to form a solar cell (heterojunction solar cell), wherein the light injection temperature is 220° C. and the time is 120 s to obtain a solar cell.

[0097] Examples 2-9 and Comparative Examples 1-3 are the same as Example 1, except for the differences shown in Table 1.

[0098] Table 1

[0099]

[0100] Test Case

[0101] The heterojunction solar cells of the above embodiments and comparative examples were subjected to the following performance tests, and the test results are shown in Table 2:

[0102] Photoelectric conversion efficiency, short-circuit current, open-circuit voltage, and fill factor testing: The specific testing method is to place the battery under a light source of 100mW / cm 2 The results are obtained by connecting a source meter using the four-wire method under AM 1.5G simulated sunlight at 25°C.

[0103] Table 2

[0104]

[0105]

[0106] It can be seen from Table 2 that, by comparing Examples 1-8 with Comparative Examples 1-3, it can be seen that the photoelectric performance of the heterojunction solar cell of the present application is good, which is because the thickness of the passivation layer formed on the polished substrate is uniform, and there is no phenomenon of local passivation effect disappearance; the first suede layer and the second suede layer have a porous structure, and this porous structure makes the first suede layer and the second suede layer present an uneven structure, which can reduce the reflection of light, thereby enhancing the absorption of sunlight by the heterojunction solar cell, and combined with the arrangement of the first anti-reflection layer and the second anti-reflection layer, the suede structure formed by the first suede layer and the first anti-reflection layer, and the second suede layer and the second anti-reflection layer can respectively reduce the surface reflection loss of the heterojunction solar cell, that is, it shows a good anti-reflection effect.

[0107] Comparing Example 1 with Comparative Example 1, it can be seen that the substrate has not been polished and still has a lot of impurities and damage, which affects the photoelectric performance of the battery.

[0108] By comparing Example 1 with Comparative Example 2, it can be seen that Comparative Example 2 does not have an anti-reflection layer, and the photoelectric performance of its heterojunction solar cell is relatively poor.

[0109] By comparing Example 1 with Comparative Example 3, it can be seen that Comparative Example 3 does not have a suede structure, and its photon absorption rate is low and the incident light is easily reflected, resulting in a decrease in the photoelectric performance of the heterojunction solar cell.

[0110] It should also be noted that the "some embodiments", "other embodiments", "embodiments", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Furthermore, when a specific feature, structure or characteristic is described in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.

[0111] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0112] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A heterojunction solar cell, characterized in that: include: A battery cell, the battery cell comprising a substrate, a first conductive layer and a second conductive layer, the substrate being a polished substrate, the first conductive layer and the second conductive layer being respectively located on two opposite sides of the substrate; a first suede layer and a second suede layer, wherein the first suede layer is located on a surface of the first conductive layer away from the substrate, and the second suede layer is located on a surface of the second conductive layer away from the substrate, and both the first suede layer and the second suede layer have a porous structure; A first anti-reflection layer and a second anti-reflection layer, wherein the first anti-reflection layer is located on a side surface of the first suede layer away from the first conductive layer, and the second anti-reflection layer is located on a side surface of the second suede layer away from the second conductive layer.

2. The heterojunction solar cell according to claim 1, characterized in that: The first suede layer and the second suede layer independently include at least one of silicon dioxide, titanium dioxide and aluminum oxide.

3. The heterojunction solar cell according to claim 1 or 2, characterized in that: The pore size of each pore in the porous structure is 10-100 nm.

4. The heterojunction solar cell according to claim 1, characterized in that: The thickness of the first suede layer and the second suede layer are independently 50-200 nm.

5. The heterojunction solar cell according to claim 1, characterized in that: The first anti-reflection layer and the second anti-reflection layer independently include at least one of magnesium fluoride and lithium fluoride.

6. The heterojunction solar cell according to claim 5, characterized in that: The thickness of the first anti-reflection layer and the second anti-reflection layer are independently 50-100 nm.

7. A method for preparing the heterojunction solar cell according to any one of claims 1 to 6, characterized in that: include: Performing mask processing on a cell to retain a grid line position, the cell comprising a polished substrate, a first conductive layer and a second conductive layer; Covering the first conductive layer and the second conductive layer of the battery cell after the mask processing with gel liquid respectively to form a gel layer; Annealing the battery cell containing the gel layer to form a first suede layer having a porous structure and a second suede layer having a porous structure; Anti-reflection materials are deposited on the first suede layer having a porous structure and the second suede layer having a porous structure, respectively, to form a first anti-reflection layer and a second anti-reflection layer.

8. The method according to claim 7, characterized in that The method satisfies at least one of the following conditions: (1) The method for preparing the polished substrate comprises: sequentially performing a rough polishing treatment and a phosphorus diffusion treatment on the substrate; performing a fine polishing on the phosphorus diffusion treatment product, wherein the fine polishing is performed in an alkaline polishing solution; (2) The masking process uses a tape as a mask plate, and the tape includes at least one of a polyimide tape and a polytetrafluoroethylene tape; (3) The gel solution comprises silicon dioxide and polyethylene glycol; (4) The covering includes coating, and the gel solution is coated by a spin coater. During the coating process, the rotation speed of the spin coater is 2000-3000 rpm / min; (5) The annealing treatment time is 5-15 minutes and the temperature is 150-250°C; (6) The deposition method includes evaporation; (7) The method further includes removing the mask layer formed by the mask processing.

9. A photovoltaic module, characterized in that: The photovoltaic module comprises a plurality of solar cells connected in series and / or in parallel; wherein at least one solar cell is a heterojunction solar cell according to any one of claims 1 to 6.

10. A photovoltaic system, characterized in that: The photovoltaic system comprises the photovoltaic assembly according to claim 9.