Carbon cloth electrode for iron-chromium flow battery and preparation method of carbon cloth electrode
The preparation of three-dimensional braided carbon cloth electrodes through electrospinning technology solves the structural problems of traditional two-dimensional carbon felt electrodes, improves the fluidity and electrochemical activity of the electrolyte, and improves the performance and life of the iron-chromium flow battery.
Patent Information
- Application Number
- CN202411111668.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The two-dimensional carbon felt electrodes used in traditional iron-chromium flow batteries have problems such as thick structure, low electrochemical activity and poor hydrophilicity, which leads to the inability to fully wet the electrolyte inside the electrode, resulting in large resistance to electrochemical reactions and failure to Meet the performance requirements of flow batteries.
Electrospinning technology is used to prepare three-dimensional braided carbon cloth electrodes. Through pre-oxidation, textile, high-temperature carbonization and activation treatment, the parameters and processes of carbon cloth electrodes are optimized, their surface defect positions are increased, electrocatalytic activity is improved, and the electrolyte flow resistance is reduced.
It improves the energy efficiency of the carbon cloth electrode, increases the reactive site, reduces the resistivity, enhances the specific surface area and load bearing capacity of the electrode, and is suitable for the mass transfer performance of the flow battery.
Smart Images

Figure CN119008980A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of functional carbon fiber preparation, and in particular to a carbon cloth electrode for an iron-chromium liquid flow battery and a preparation method thereof. Background Art
[0002] With the development of renewable energy, how to integrate wind energy, solar energy and other new energy sources with randomness and intermittency into the existing power grid system has become a technical challenge. The energy storage system can realize the peak load regulation and valley load balancing of the power grid, thereby improving the power grid's ability to absorb renewable energy generation.
[0003] Liquid flow batteries have the advantages of long cycle life, recyclable electrolyte, and high safety. They are considered to be one of the preferred technologies for large-scale energy storage. They can be applied to power generation such as solar energy and wind energy, as well as smart microgrids and user-side, and have good prospects for industrialization and market promotion. 2+ / Fe 3+ and Cr 2 + / Cr 3+ The raw materials of iron ions and chromium ions have large output and low price, which determines that the iron-chromium flow battery has a large cost advantage; its operating temperature is -20℃ to 70℃, and it has good environmental adaptability; at the same time, the iron-chromium flow battery adopts a storage tank design and has no self-discharge. Electric energy is stored in the electrolyte solution, and the electrolyte solution is stored in the storage tank, so there is no self-discharge phenomenon, which is especially suitable for backup power supply, etc.; waste batteries are easy to handle and can be recycled. The structural materials, ion exchange membranes and electrode materials of the iron-chromium flow battery are metals, plastics (or resins) and carbon materials, respectively, which are easy to handle in an environmentally friendly manner and are relatively friendly to the environment. Therefore, the iron-chromium flow battery is considered to be the most promising flow battery energy storage technology.
[0004] Carbon felt is a common electrode material used in traditional iron-chromium flow batteries. However, due to the thick structure of carbon felt electrodes and the large resistance in contact with the electrolyte, it is easy for the electrolyte to eddy inside the carbon felt, causing a "dead zone" phenomenon. The two-dimensional carbon felt electrode has low electrochemical activity and poor hydrophilicity, and its thick structure makes it unable to be fully wetted when the electrolyte flows through it. The resistance between the electrolyte and the electrode is large, and the electrochemical activity and hydrophilicity cannot meet the needs of the flow battery. In addition, the carbon cloth electrode that has not been activated is hydrophobic and cannot achieve full contact and immersion in the electrolyte, so the battery performance cannot achieve the expected effect. Summary of the invention
[0005] The object of the present invention is to provide a carbon cloth electrode for an iron-chromium liquid flow battery and a preparation method thereof.
[0006] The present invention develops a method for preparing a high-performance carbon cloth electrode to prepare a three-dimensional woven carbon cloth electrode to replace the two-dimensional carbon felt electrode, so as to reduce the dead zone of electrolyte flow, reduce the contact resistance between the electrolyte and the electrode, and better realize the flow of electrolyte between the electrodes.
[0007] In order to improve the electrocatalytic activity of the carbon cloth electrode surface, the present invention optimizes the parameters and processes of the carbon cloth electrode preparation method (pre-oxidation, spinning, high-temperature carbonization), prepares the original high-performance carbon cloth electrode, and activates it to increase the surface defect sites. By increasing the defect sites, the active sites of the carbon cloth electrode are increased, thereby improving the performance of the iron-chromium liquid flow battery.
[0008] In order to achieve the above purpose, the present invention adopts the following technical solutions:
[0009] In one aspect, the present invention provides a method for preparing a carbon cloth electrode for an iron-chromium liquid flow battery, wherein the preparation method comprises the following steps:
[0010] The precursor fibers of carbon cloth electrodes were prepared using viscose matrix by electrospinning technology;
[0011] Pre-oxidation: pre-oxidizing the precursor fiber at a temperature of 200 to 400° C. in an air atmosphere to prepare a precursor pre-oxidized fiber;
[0012] Weaving: Weaving the precursor preoxidized yarn into cloth to obtain preoxidized yarn cloth; the specifications of the weaving include: the twist is 300-500 twists, the yarn count is 10-20 yarns, and the strands are (10-20) yarns / 3 strands; the warp and weft density of the preoxidized yarn cloth is (8-10)×8 yarns / cm 2 , unit weight is 260~400g / m 2 ;
[0013] High temperature carbonization: in a protective gas atmosphere, the pre-oxidized silk cloth is subjected to high temperature carbonization at 1000-2000° C. to prepare an original carbon cloth;
[0014] Activation: The original carbon cloth is immersed in at least one solution of silicate, nitric acid, sulfuric acid, potassium permanganate, and hypochlorous acid to complete the activation treatment; then, a high-temperature treatment of 100 to 800° C. for 2 to 10 hours is performed in an oxygen-containing atmosphere to prepare the carbon cloth electrode.
[0015] According to the preparation method of the present invention, preferably, the main component of the viscose base is polyacrylonitrile, and the precursor fiber is polyacrylonitrile precursor.
[0016] According to the preparation method of the present invention, preferably, the diameter of the precursor fiber is 5-20 μm, the strength is 50-300 MPa, the elongation is 2%-5%, and the density is 0.8-1.5 g / cm3 .
[0017] More preferably, the diameter of the precursor fiber is 14-17 μm, the strength is 100-300 MPa, and the density is 1.0-1.5 g / cm 3 .
[0018] In the preparation method of the present invention, the pre-oxidation temperature is 200-400°C, and the gas atmosphere is air. More preferably, the pre-oxidation temperature is 250-280°C; further preferably, during the pre-oxidation process, the heating rate is 1-10°C / min, for example 5°C / min.
[0019] According to the preparation method of the present invention, preferably, the pre-oxidation time is 0.5 to 20 hours.
[0020] In the preparation method of the present invention, in the high temperature carbonization step, the temperature is 1000-2000°C, and the protective gas is nitrogen; in addition, the protective gas can also use an inert gas. Preferably, the temperature of the high temperature carbonization is 1200-1500°C; more preferably 1500°C.
[0021] According to the preparation method of the present invention, preferably, the high temperature carbonization time is 0.5 to 20 hours.
[0022] According to the preparation method of the present invention, preferably, the diameter of the precursor pre-oxidized filament obtained after pre-oxidation is 5 to 30 μm, more preferably 5 to 16 μm; the density is 1.1 to 1.5 g / cm 3 .
[0023] In the preparation method of the present invention, the textile specifications include: a twist of 300 to 500 twists, a yarn count of 10 to 20 yarns, and the strands are (10 to 20) yarns / 3 strands.
[0024] In the preparation method of the present invention, the warp and weft density of the pre-oxidized silk cloth is (8-10)×8 pieces / cm 2 , unit weight is 260~400g / m 2 Preferably, the unit weight of the pre-oxidized silk cloth is 260-340 g / m 2 .
[0025] According to the preparation method of the present invention, preferably, the heating rate during the high-temperature carbonization is 1-25°C / min; more preferably 5°C / min.
[0026] According to the preparation method of the present invention, preferably, the oxygen-containing atmosphere is air.
[0027] According to the preparation method of the present invention, preferably, the concentration of the silicic acid, nitric acid, sulfuric acid, potassium permanganate and hypochlorous acid solution is 0.01 to 1 M; and the soaking time is 0.1 to 24 hours.
[0028] According to the preparation method of the present invention, preferably, the temperature of the high temperature treatment after the original carbon cloth is soaked is 500° C., and the time is 5 to 10 hours.
[0029] According to the preparation method of the present invention, preferably, before the activation, the method further comprises soot blowing treatment on the original carbon cloth.
[0030] In a preferred embodiment, Figure 8 As shown, the preparation steps of the high-performance carbon cloth electrode include: precursor fiber preparation, pre-oxidation, spinning, high-temperature carbonization, carbon cloth purging, and activated carbon cloth; the parameters of each process are as defined above.
[0031] Another aspect of the present invention provides a carbon cloth electrode obtained by the above preparation method.
[0032] The carbon cloth electrode prepared by the present invention has lower curvature and higher hydrophilic permeability, which is beneficial to improving the ion / mass transport performance of the electrode.
[0033] The beneficial effects of the present invention include:
[0034] 1) The carbon cloth electrode prepared by the present invention has higher energy efficiency than carbon felt, which can reduce energy loss and increase battery life.
[0035] 2) After being activated, the carbon cloth electrode prepared by the present invention has more grooves than the surface of a general electrode, and is accompanied by the generation of defect sites, providing more reactive sites.
[0036] 3) After activation, the carbon cloth electrode prepared by the present invention has lower resistivity and higher specific surface area than general electrodes, and is more suitable for mass transfer in liquid flow batteries.
[0037] 4) The carbon cloth electrode prepared by the present invention can withstand a large load in all directions and overcome its anisotropy. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a SEM image of the high-performance three-dimensional carbon cloth electrode prepared in Example 1;
[0039] Figure 2 This is a SEM image of the high-performance three-dimensional carbon cloth electrode prepared in Example 2;
[0040] Figure 3 This is a SEM image of the high-performance three-dimensional carbon cloth electrode prepared in Example 3;
[0041] Figure 4 This is a SEM image of the high-performance three-dimensional carbon cloth electrode prepared in Example 4;
[0042] Figure 5 A comparison chart of the energy efficiency of the high-performance three-dimensional carbon cloth electrodes prepared in Examples 1-4;
[0043] Figure 6 A comparison chart of the current efficiency of the high-performance three-dimensional carbon cloth electrodes prepared in Examples 1-4;
[0044] Figure 7 A comparison chart of the voltage efficiency of the high-performance three-dimensional carbon cloth electrodes prepared in Examples 1-4;
[0045] Figure 8 The present invention is a flow chart for preparing a high-performance carbon cloth electrode in a preferred embodiment of the present invention. DETAILED DESCRIPTION
[0046] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0047] All numerical specifications herein (e.g., temperature, time, concentration, and weight, etc., including ranges for each thereof) are generally approximate values that may be appropriately varied (+) or (-) in increments of 0.1 or 1.0. All numerical specifications may be understood as being preceded by the term "about."
[0048] Example 1
[0049] This embodiment prepares a high-performance three-dimensional carbon cloth electrode, including the following steps:
[0050] (1) Preparation of precursor fibers using viscose base:
[0051] The viscose base is soaked and washed in deionized water, and then placed at 80°C for drying to prepare precursor fibers for carbon cloth electrodes. The prepared precursor fibers have a diameter of 15 to 17 μm, a strength of 200 to 300 MPa, and a density of 1.2 to 1.5 g / cm 3 , elongation 3%.
[0052] (2) Pre-oxidation:
[0053] The precursor fiber is placed in a pre-oxidation furnace with a pre-oxidation temperature of 250°C, a starting temperature of 25°C, a heating rate of 5°C / min, and a diameter of 14-16 μm and a density of 1.5 g / cm 3 .
[0054] (3) Preparation of preoxidized silk yarn:
[0055] The preoxidized yarn is combed and placed on a spinning machine for spinning to prepare preoxidized yarn with a twist of 350 to 400 twists and a yarn count of 15 yarns.
[0056] (4) Textiles:
[0057] The pre-oxidized silk yarn is woven into 20-count / 3-ply yarn using a special loom. The width of the fabric is 1.5 meters, and the density of the warp and weft is 8×8 counts / cm 2 The square gram weight of the prepared pre-oxidized silk fabric is 260g / cm 2 .
[0058] (5) High temperature carbonization:
[0059] The pre-oxidized silk cloth was placed in a carbonization furnace with a protective atmosphere of nitrogen, and subjected to high-temperature carbonization treatment at an ambient temperature of 1500°C and a heating rate of 5°C / min to obtain an original high-performance carbon cloth.
[0060] (6) Dust treatment:
[0061] The prepared original high-performance carbon cloth is treated by soot blowing.
[0062] (7) Activation:
[0063] The prepared original high-performance carbon cloth electrode was soaked in 0.1M silicate solution for 10 hours, and the soaked product was placed at a temperature of 500°C and an ambient gas of air for 10 hours for high temperature treatment to prepare an activated carbon cloth electrode.
[0064] Example 2
[0065] This embodiment prepares a high-performance three-dimensional carbon cloth electrode, including the following steps:
[0066] (1) Preparation of precursor fibers using viscose base:
[0067] The viscose base is soaked and washed in deionized water, and then dried at 80°C to prepare the precursor fiber of the carbon cloth electrode with a diameter of 14-16 μm, a strength of 200-300 MPa, and a density of 1.2-1.5 g / cm 3 , elongated by 2.3%.
[0068] (2) Pre-oxidation:
[0069] The precursor fiber is placed in a pre-oxidation furnace with a pre-oxidation temperature of 250°C, a starting temperature of 25°C, a heating rate of 5°C / min, and a diameter of 5 to 15 μm after pre-oxidation, and a density of 1.4 g / cm 3 .
[0070] (3) Preparation of preoxidized silk yarn:
[0071] The preoxidized yarn is combed and placed on a spinning machine for spinning to prepare preoxidized yarn with a twist of 450 to 500 twists and a yarn count of 20 yarns.
[0072] (4) Textiles:
[0073] The pre-oxidized silk yarn is woven into 20-count / 3-ply yarn using a special loom. The width of the fabric is 1.5 meters, and the density of the warp and weft is 10×8 counts / cm 2 The square gram weight of the prepared pre-oxidized silk fabric is 340g / cm 2 .
[0074] (5) High temperature carbonization:
[0075] The pre-oxidized silk cloth was placed in a carbonization furnace with a protective atmosphere of nitrogen, and subjected to high-temperature carbonization treatment at an ambient temperature of 1500°C and a heating rate of 5°C / min to obtain an original high-performance carbon cloth.
[0076] (6) Dust treatment:
[0077] The prepared original high-performance carbon cloth is treated by soot blowing.
[0078] (7) Activation:
[0079] The prepared original high-performance carbon cloth electrode was soaked in 0.2M silicate solution for 2 hours, and the soaked product was placed at a temperature of 500°C and an ambient gas of air for 5 hours for high-temperature treatment to prepare an activated carbon cloth electrode.
[0080] Example 3
[0081] This embodiment prepares a high-performance three-dimensional carbon cloth electrode, including the following steps:
[0082] (1) Preparation of precursor fibers using viscose base:
[0083] The viscose base is soaked and washed in deionized water, and then dried at 80°C to prepare the precursor fiber of the carbon cloth electrode with a diameter of 15-17 μm, a strength of 100-150 MPa, and a density of 1.1-1.2 g / cm 3 , elongation 2.2%.
[0084] (2) Pre-oxidation:
[0085] The precursor fiber is placed in a pre-oxidation furnace with a pre-oxidation temperature of 280°C, a starting temperature of 25°C, a heating rate of 5°C / min, and a diameter of 5 to 15 μm after pre-oxidation, and a density of 1.2 g / cm 3 .
[0086] (3) Preparation of preoxidized silk yarn:
[0087] The preoxidized yarn is combed and placed on a spinning machine for spinning to prepare preoxidized yarn with a twist of 450 to 500 twists and a yarn count of 20 yarns.
[0088] (4) Textiles:
[0089] The pre-oxidized silk yarn is woven into 10-count / 3-ply yarn using a special loom. The width of the fabric is 1.5 meters, and the density of the warp and weft is 8×8 counts / cm 2 The square gram weight of the prepared pre-oxidized silk fabric is 260g / cm 2 .
[0090] (5) High temperature carbonization:
[0091] The pre-oxidized silk cloth was placed in a carbonization furnace with a nitrogen protective atmosphere, and subjected to high-temperature carbonization treatment at an ambient temperature of 1200°C and a heating rate of 5°C / min to obtain an original high-performance carbon cloth.
[0092] (6) Dust treatment:
[0093] The prepared original high-performance carbon cloth is treated by soot blowing.
[0094] (7) Activation:
[0095] The prepared original high-performance carbon cloth electrode was soaked in 0.05M nitric acid solution for 5 hours, and the soaked product was placed at a temperature of 500°C and an ambient gas of air for 5 hours for high-temperature treatment to prepare an activated carbon cloth electrode.
[0096] Example 4
[0097] This embodiment prepares a high-performance three-dimensional carbon cloth electrode, including the following steps:
[0098] (1) Preparation of precursor fibers using viscose base:
[0099] The viscose base is soaked and washed in deionized water, and then dried at 80°C to prepare the precursor fiber of the carbon cloth electrode with a diameter of 15-17 μm, a strength of 100-150 MPa, and a density of 1.0-1.1 g / cm 3 , elongation 2.1%.
[0100] (2) Pre-oxidation:
[0101] The precursor fiber is placed in a pre-oxidation furnace with a pre-oxidation temperature of 280°C, a starting temperature of 25°C, a heating rate of 5°C / min, and a diameter of 5 to 15 μm after pre-oxidation, and a density of 1.1 g / cm 3 .
[0102] (3) Preparation of preoxidized silk yarn:
[0103] The preoxidized yarn is combed and placed on a spinning machine for spinning to prepare preoxidized yarn with a twist of 350 to 400 twists and a yarn count of 15 yarns.
[0104] (4) Textiles:
[0105] The pre-oxidized silk yarn is woven into 10-count / 3-ply yarn using a special loom. The width of the fabric is 1.5 meters, and the density of the warp and weft is 10×8 count / cm 2 The square gram weight of the prepared pre-oxidized silk fabric is 340g / cm 2 .
[0106] (5) High temperature carbonization:
[0107] The pre-oxidized silk cloth was placed in a carbonization furnace with a nitrogen protective atmosphere, and subjected to high-temperature carbonization treatment at an ambient temperature of 1200°C and a heating rate of 5°C / min to obtain an original high-performance carbon cloth.
[0108] (6) Dust treatment:
[0109] The prepared original high-performance carbon cloth is treated by soot blowing.
[0110] (7) Activation:
[0111] The prepared original high-performance carbon cloth electrode was soaked in 0.02M sulfuric acid solution for 2 hours, and the soaked product was placed at a temperature of 500°C and an ambient gas of air for 10 hours for high temperature treatment to prepare an activated carbon cloth electrode.
[0112] Figure 1 to Figure 4 They are SEM images of the high-performance three-dimensional carbon cloth electrodes prepared in the examples, and as shown in the figures, they all show good etching effects.
[0113] Figure 5 to Figure 7 The energy efficiency comparison diagram, current efficiency comparison diagram, and voltage efficiency comparison diagram of the high-performance three-dimensional carbon cloth electrodes prepared in Examples 1 to 4 are shown in turn. Table 1 shows the specific surface area data of the high-performance three-dimensional carbon cloth electrodes prepared in Examples 1 to 4. By comparing the data in Examples 1 to 4, it can be seen that under the same test conditions, the specific surface area of the high-performance carbon cloth electrode material obtained in Example 1 is higher than the specific surface areas of Examples 2, 3, and 4, and its performance is the best.
[0114] Table 1 Specific surface area of electrodes after different treatments
[0115] electrode <![CDATA[Specific surface area (m 2 / g)]]> Example 1 8.32~8.48 Example 2 7.48~7.88 Example 3 6.35~6.12 Example 4 7.36~7.47
[0116] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A method for preparing a carbon cloth electrode for an iron-chromium flow battery, wherein: The preparation method comprises the following steps: The precursor fibers of carbon cloth electrodes were prepared using viscose matrix by electrospinning technology; Pre-oxidation: pre-oxidizing the precursor fiber at a temperature of 200 to 400° C. in an air atmosphere to prepare a precursor pre-oxidized fiber; Weaving: Weaving the precursor preoxidized yarn into cloth to obtain preoxidized yarn cloth; the specifications of the weaving include: the twist is 300-500 twists, the yarn count is 10-20 yarns, and the strands are (10-20) yarns / 3 strands; the warp and weft density of the preoxidized yarn cloth is (8-10)×8 yarns / cm 2 , unit weight is 260~400g / m 2 ; High temperature carbonization: in a protective gas atmosphere, the pre-oxidized silk cloth is subjected to high temperature carbonization at 1000-2000° C. to prepare an original carbon cloth; Activation: The original carbon cloth is immersed in at least one solution of silicate, nitric acid, sulfuric acid, potassium permanganate, and hypochlorous acid to complete the activation treatment; then, a high-temperature treatment of 100 to 800° C. for 2 to 10 hours is performed in an oxygen-containing atmosphere to prepare the carbon cloth electrode.
2. The preparation method according to claim 1, wherein The main component of the viscose base is polyacrylonitrile, and the precursor fiber is polyacrylonitrile precursor.
3. The preparation method according to claim 1, wherein The precursor fiber has a diameter of 5 to 20 μm, a strength of 50 to 300 MPa, an elongation of 2% to 5%, and a density of 0.8 to 1.5 g / cm 3 .
4. The preparation method according to claim 1, wherein The pre-oxidation time is 0.5 to 20 hours.
5. The preparation method according to claim 1, wherein The high temperature carbonization time is 0.5 to 20 hours.
6. The preparation method according to claim 1, wherein The diameter of the precursor pre-oxidized filament obtained after the pre-oxidation is 5 to 30 μm, and the density is 1.1 to 1.5 g / cm 3 .
7. The preparation method according to claim 1, wherein The textile specifications include: twist of 350-500 twists, yarn count of 15-20 yarns, and (10-20) yarns / 3 strands of yarn.
8. The preparation method according to claim 1, wherein The unit weight of the pre-oxidized silk cloth is 260-340 g / m 2 .
9. The preparation method according to claim 1, wherein The concentrations of the silicic acid, nitric acid, sulfuric acid, potassium permanganate and hypochlorous acid solutions are 0.01 to 1 M; and the soaking time is 0.1 to 24 hours.
10. A carbon cloth electrode obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Carbon cloth texturing method for improving electrical properties of carbon cloth
CN119939866A
A method for preparing and applying a high-performance pre-oxidized filament-based flow battery electrode cloth.
CN123095811A