Rapid method for initial activation of proton exchange membrane fuel cell stack
By optimizing the combination of the intake humidity and pressure of the cathode and anode, the current loading and decreasing speed and high current constant current time, the problem of long initial activation time of the stack is solved, rapid activation of the stack and reduced fuel consumption are achieved, and activation is improved efficiency.
Patent Information
- Application Number
- CN202411088086.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The initial activation process of the existing proton exchange membrane fuel cell stack is too long, resulting in high time and fuel costs and limited improvement in activation efficiency.
The initial activation process of the stack is optimized by controlling the intake humidity of the cathode, the intake pressure, the metering ratio of the cathode when hungry, the hunger time, the hunger current density, the loading speed of the activation current and the high current constant current time.
The initial activation time and hydrogen consumption of the stack are significantly shortened, the time and fuel costs are reduced, and the activation efficiency is improved.
Smart Images

Figure CN119009015A_ABST
Abstract
Description
Technical Field
[0002] The invention belongs to the field of fuel cells, and in particular relates to a rapid method for initial activation of a proton exchange membrane fuel cell stack. Background Art
[0003] A proton exchange membrane fuel cell is a chemical device that converts the chemical energy of a fuel directly into electrical energy. The stack is the heart of the proton exchange membrane fuel cell and is where the chemical reaction occurs. The stack is assembled from multiple cells. After the stack is assembled, it needs to undergo an activation process to activate the performance of the stack. Generally speaking, stack activation mainly activates the internal membrane electrode assembly, and the process mainly includes: 1. Wetting the proton exchange membrane to enhance the proton conductivity of the proton exchange membrane, thereby reducing the resistance of the battery; 2. Establishing water, proton and reaction gas transmission channels to accelerate the material transmission of the reaction process and improve the reaction efficiency; 3. Optimizing the internal structure of the electrode and improving the three interfaces; 4. Improving the activity and utilization of the cathode catalyst layer.
[0004] Existing stack initial activation technologies include constant current discharge activation, variable current discharge activation, hydrogen pump activation, hydrogen starvation and constant voltage discharge activation, etc. Using these activation technologies alone to perform initial activation on the stack will make the entire activation process too long. If the activation time is too long, the consumption of hydrogen will increase, which will eventually lead to a particularly high time cost and fuel cost of the entire activation process. At present, there are also some activation schemes that improve the activation efficiency by integrating different activation technologies, but the activation efficiency has not been improved too much, and there is still a lot of room for improvement. The present invention greatly reduces the time and fuel consumption of the initial activation of the stack by controlling and optimizing the reasonable matching of the cathode and cathode intake humidity, the cathode and cathode intake pressure, the cathode stoichiometric ratio when the cathode is starved, the cathode starvation time, the cathode starvation current density, the activation current loading and unloading speed, and the high current constant current time.
[0005] In the prior art, wetting of the proton exchange membrane is generally achieved by controlling the humidity of the fuel gas intake and adding and removing high current; the establishment of water, proton and reaction gas transmission channels is generally achieved by rapid addition and removal of loads and controlling the fuel gas intake pressure; the optimization of the internal structure of the electrode and the improvement of the three interfaces are achieved through rapid addition and removal of loads, constant current discharge, etc.; the activity and utilization rate of the cathode catalyst layer are improved, which is generally achieved through hydrogen starvation and hydrogen pump effect. Summary of the invention
[0006] The present invention greatly shortens the time and hydrogen consumption of initial activation of the fuel cell stack and reduces time and fuel costs by controlling the reasonable combination of anode and cathode air intake humidity, anode and cathode air intake pressure, cathode stoichiometric ratio during cathode starvation, cathode starvation time, cathode starvation current density, activation current loading and unloading speeds and high current constant current time.
[0007] The technical solution of the present invention is as follows: A rapid method for initial activation of a proton exchange membrane fuel cell stack, which controls the intake humidity of the cathode and anode of the stack, the intake pressure of the anode and cathode, the cathode stoichiometric ratio when the cathode is starved, the cathode starvation time, the cathode starvation current density, the speed of increasing and decreasing the activation current, and the constant current time of the high current, to achieve rapid initial activation of the stack; Here are the steps: During the activation process, the intake humidity of the cathode and anode of the coordinated stack, the intake pressure of the cathode and anode, the cathode stoichiometric ratio during cathode starvation, the cathode starvation time, the cathode starvation current density, the activation current loading and unloading speed and the high current constant current time are taken into consideration; The cathode and anode air inlet pressures are adjusted according to the cathode stoichiometric ratio during cathode starvation; the cathode starvation time is adjusted according to the cathode starvation current density and the cathode stoichiometric ratio during cathode starvation; the activation current loading and unloading speeds are adjusted according to the cathode and anode air inlet pressures.
[0008] In the above method, during the activation process, the humidity range of the anode and cathode of the stack is always controlled as follows: the anode air intake humidity is maintained at 40-100%, and the cathode humidity is maintained at 60-100%.
[0009] In the above method, during the activation process, the anode and cathode air intake pressure range of the fuel cell stack needs to be controlled as follows: anode air intake pressure 160-280 kPa, cathode air intake pressure: 140-260 kPa; at the same time, the anode and cathode air intake pressure difference needs to be controlled at 10-30 kPa, and the anode air intake pressure must always be greater than the cathode air intake pressure.
[0010] In the above method, during the activation process, the cathode stoichiometric ratio needs to be controlled within a range of 0.5-1.7 when the cathode is starved.
[0011] In the above method, the cathode starvation time needs to be controlled within 5-60s during the activation process.
[0012] In the above method, the cathode starvation current density needs to be controlled at 0.1-1.5A / cm during the activation process. 2 .
[0013] In the above method, during the activation process, the activation current loading and unloading rate needs to be controlled within a range of 3-40 A / s.
[0014] In the above method, the constant current time of the high current needs to be controlled within 1-20 minutes during the activation process.
[0015] A rapid method for initial activation of a proton exchange membrane fuel cell stack comprises the following steps: (1) Install the target activated fuel cell stack on the test bench, first purge the cathode and anode with nitrogen, then heat the fuel cell stack to 70℃-80℃, control the anode inlet humidity and the cathode inlet humidity. During the entire activation process, the anode inlet humidity is maintained at 40-100%, the cathode humidity is maintained at 60-100%, the anode stoichiometric ratio is maintained at 1.6-2.0, and the cathode stoichiometric ratio is maintained at 2.0-2.4 except for the cathode starvation activation. The anode inlet pressure and the cathode inlet pressure are 160-280kPa and 140-260kPa respectively except for the cathode starvation activation. (2) When the temperature and intake air humidity of the battery stack reach the target values, current loading begins, and the loading and unloading rate is set to 3-40A / s; Specifically: 1. First, load the current to 2A / cm 2 , constant current for 1-20min, then quickly reduce the load to 0.3~0.5A / cm 2 , the cathode stoichiometric ratio is reduced to 1-1.2, the anode inlet pressure and the cathode inlet pressure are adjusted to 190 kPa and 170 kPa, the cathode starvation time is 5-60 s, after the cathode starvation time is over, the cathode stoichiometric ratio is restored to 2.0-2.2, the anode inlet pressure and the cathode inlet pressure are restored to the set value in step (1); 2, then the current is loaded to 2.5 A / cm 2 , constant current 1-20min, then quickly reduce the load to 0.6~0.8A / cm 2 , the cathode stoichiometric ratio is reduced to 1-1.2, the anode inlet pressure and the cathode inlet pressure are adjusted to 200-220 kPa and 180-200 kPa, and the cathode starvation time is 5-60 s. After the cathode starvation time is over, the cathode stoichiometric ratio is restored to 2.0-2.2, and the anode inlet pressure and the cathode inlet pressure are restored to the set value in step (1); after completing steps 1 and 2, a round of activation test is completed. Repeating multiple rounds of activation test until the stack reaches the target performance is considered to be completed.
[0016] In the present invention, the wetting time of the proton exchange membrane is shortened as much as possible by controlling the intake humidity of the cathode and anode and the high current constant current time within a certain suitable range. The rapid establishment of water, proton and reaction gas transmission channels is achieved by optimizing the rapid addition and subtraction rate of the current and controlling the reasonable combination of the fuel gas intake pressure. The activity and utilization rate of the cathode catalyst layer are rapidly improved by optimizing the cathode stoichiometric ratio, cathode starvation time and cathode starvation current density when the cathode is starved. Finally, by optimizing the reasonable combination of the intake humidity of the cathode and anode, the intake pressure of the cathode and anode, the cathode stoichiometric ratio, cathode starvation time, cathode starvation current density, the addition and subtraction speed of the activation current and the constant current time of the high current, the total activation time and the total consumption of hydrogen are shortened, and the purpose of rapid initial activation of the fuel cell stack is achieved.
[0017] In the present invention, the current during high current constant current is set according to the highest tolerable current value and the tolerable value of the test bench load. When the test bench has no restrictions, the highest current value when the battery stack does not trigger the lowest voltage protection value is used as the set value; the starvation current value is basically positively correlated with the cathode stoichiometric ratio during starvation, and the larger the starvation current value, the higher the cathode stoichiometric ratio; during the starvation process, the cathode intake pressure is adjusted according to the size of the cathode stoichiometric ratio, and the higher the cathode stoichiometric ratio, the greater the cathode intake pressure, and the anode intake pressure is adjusted according to the cathode intake pressure, and the anode intake pressure is always kept higher than the cathode intake pressure by a certain value.
[0018] Compared with the prior art, the advantages of the present invention are: 1. The air intake humidity and high current constant current time of the anode and cathode are optimized, and the wetting time of the proton exchange membrane is shortened; 2. The rapid rate of current loading and unloading and the reasonable combination of controlling the gas inlet pressure are optimized, shortening the establishment time of water, proton and reaction gas transmission channels; 3. The cathode stoichiometric ratio, cathode starvation time and cathode starvation current density are optimized to achieve rapid improvement in the activity and utilization of the cathode catalytic layer; 4. Finally, the reasonable mix and match of anode and cathode air intake humidity, cathode and cathode air intake pressure, cathode stoichiometric ratio during cathode starvation, cathode starvation time, cathode starvation current density, activation current loading and unloading speeds, and high current constant current time were optimized to shorten the total activation time and the total consumption of hydrogen, thereby achieving the purpose of rapid initial activation of the fuel cell stack. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is the activation time diagram in Example 1.
[0020] Figure 2 This is a comparison chart of the amount of hydrogen used in Example 1.
[0021] Figure 3 This is the activation time diagram in Example 2.
[0022] Figure 4 This is a comparison chart of hydrogen usage in Example 2.
[0023] Figure 5 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0025] Example 1 Install the target activated battery stack on the test bench, first purge the cathode and anode with nitrogen for three minutes, then heat the battery stack to 70°C, control the anode intake humidity to 100%, and the cathode intake humidity to 100%. During the entire activation process, the humidity of the cathode and anode is maintained at 100%, the anode stoichiometric ratio is maintained at 1.8, and the cathode stoichiometric ratio is maintained at 2.2 except for the cathode starvation activation. The anode intake pressure and cathode intake pressure are maintained at 250kPa and 230kPa except for the cathode starvation activation. When the temperature and intake humidity of the battery stack reach the target value, start current loading, and the load rate is set to 20A / s. 1. First load the current to 2A / cm 2 , constant current for 5 minutes, then quickly reduce the load to 0.3A / cm 2 , the cathode stoichiometric ratio is reduced to 1.2, the anode inlet pressure and cathode inlet pressure are adjusted to 190kPa and 170kPa, the cathode starvation time is 40s, after the cathode starvation time, the cathode stoichiometric ratio is restored to 2.2, the anode inlet pressure and cathode inlet pressure are restored to 250kPa and 230kPa. 2. Then the current is loaded to 2.5A / cm 2 , constant current for 5 minutes, then quickly reduce the load to 0.6A / cm 2 , the cathode stoichiometric ratio is reduced to 1.2, the anode inlet pressure and the cathode inlet pressure are adjusted to 200kPa and 180kPa, the cathode starvation time is 40s, after the cathode starvation time, the cathode stoichiometric ratio is restored to 2.2, the anode inlet pressure and the cathode inlet pressure are restored to 250kPa and 230kPa; the completion of steps 1 and 2 is considered to complete a round of activation test, and multiple rounds of activation tests are repeated until the stack reaches the target performance, and the activation is considered to be completed. Using this activation process, the stack reaches the target performance after 2h, and the activation is completed, which is 20% faster than the conventional activation method, and the hydrogen consumption is reduced by 15% or more (such as Figure 1 and Figure 2 as shown).
[0026] Example 2 Install the target activated battery stack on the test bench, first purge the cathode and anode with nitrogen for three minutes, then heat the battery stack to 70°C, control the anode intake humidity to 80%, and the cathode intake humidity to 70%. During the entire activation process, the humidity of the anode and cathode are maintained at 70% and 80% respectively, the anode stoichiometric ratio is maintained at 1.6, and the cathode stoichiometric ratio is maintained at 2.0 except for the cathode starvation activation. The anode intake pressure and cathode intake pressure are maintained at 240kPa and 220kPa except for the cathode starvation activation. When the temperature and intake humidity of the battery stack reach the target value, start current loading, and the load rate is set to 30A / s. 1. First load the current to 2A / cm 2 , constant current for 7 minutes, then quickly reduce the load to 0.5A / cm 2, the cathode stoichiometric ratio is reduced to 1, the anode inlet pressure and cathode inlet pressure are adjusted to 190 kPa and 170 kPa, the cathode starvation time is 30 s, after the cathode starvation time, the cathode stoichiometric ratio is restored to 2.0, the anode inlet pressure and cathode inlet pressure are restored to 240 kPa and 220 kPa. 2. Then the current is loaded to 2.5 A / cm 2 , constant current for 7 minutes, then quickly reduce the load to 0.8A / cm 2 , the cathode stoichiometric ratio is reduced to 1, the anode inlet pressure and the cathode inlet pressure are adjusted to 220kPa and 200kPa, the cathode starvation time is 30s, after the cathode starvation time, the cathode stoichiometric ratio is restored to 2.0, the anode inlet pressure and the cathode inlet pressure are restored to 240kPa and 220kPa; completing steps 1 and 2 is considered to complete a round of activation test, and multiple rounds of activation tests are repeated until the stack reaches the target performance, and activation is considered complete. Using this activation process, the stack reaches the target performance after 1.8h, and activation is completed, which is 28% or more faster than the conventional activation method, and the hydrogen consumption is reduced by 12% or more (such as Figure 3 and Figure 4 as shown).
[0027] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A rapid method for initial activation of a proton exchange membrane fuel cell stack, which is characterized by controlling the intake humidity of the cathode and anode of the stack, the intake pressure of the anode and cathode, the cathode stoichiometric ratio when the cathode is starved, the cathode starvation time, the cathode starvation current density, the speed of increasing and decreasing the activation current, and the constant current time of the high current, so as to achieve initial rapid activation of the stack; Here are the steps: During the activation process, the intake humidity of the cathode and anode of the coordinated stack, the intake pressure of the cathode and anode, the cathode stoichiometric ratio during cathode starvation, the cathode starvation time, the cathode starvation current density, the activation current loading and unloading speed and the high current constant current time are taken into consideration; The cathode and anode air inlet pressures are adjusted according to the cathode stoichiometric ratio during cathode starvation; the cathode starvation time is adjusted according to the cathode starvation current density and the cathode stoichiometric ratio during cathode starvation; the activation current loading and unloading speeds are adjusted according to the cathode and anode air inlet pressures.
2. The rapid method for initial activation of a proton exchange membrane fuel cell stack according to claim 1, characterized in that: During the activation process, the humidity range of the anode and cathode of the battery stack is always controlled: the anode air intake humidity is maintained at 40-100%, and the cathode humidity is maintained at 60-100%.
3. The rapid method for initial activation of a proton exchange membrane fuel cell stack according to claim 1, characterized in that: During the activation process, the anode and cathode air intake pressures of the stack need to be controlled in the range of: anode air intake pressure 160-280 kPa, cathode air intake pressure: 140-260 kPa; at the same time, the difference between the anode and cathode air intake pressures needs to be controlled within a certain range, and ensure that the anode air intake pressure is always greater than the cathode air intake pressure.
4. The rapid method for initial activation of a proton exchange membrane fuel cell stack according to claim 1, characterized in that: During the activation process, the cathode stoichiometry ratio needs to be controlled at 0.5-1.7 when the cathode is starved.
5. The rapid method for initial activation of a proton exchange membrane fuel cell stack according to claim 1, characterized in that: During the activation process, the cathode starvation time needs to be controlled within 5-60s.
6. The rapid method for initial activation of a proton exchange membrane fuel cell stack according to claim 1, characterized in that: During the activation process, the cathode starvation current density needs to be controlled at 0.1-1.5A / cm 2 .
7. The rapid method for initial activation of a proton exchange membrane fuel cell stack according to claim 1, characterized in that: During the activation process, the activation current loading and unloading rate needs to be controlled at 3-40A / s.
8. The rapid method for initial activation of a proton exchange membrane fuel cell stack according to claim 1, characterized in that: During the activation process, the high current constant current time needs to be controlled within 1-20 minutes.
9. The rapid method for initial activation of a proton exchange membrane fuel cell stack according to claim 3, characterized in that: During the activation process, it is necessary to control the difference in intake pressure between the anode and cathode of the stack within a certain range, and ensure that the anode intake pressure is always greater than the cathode intake pressure by 10-30 kPa.
10. The rapid method for initial activation of a proton exchange membrane fuel cell stack according to claim 1, characterized in that: The specific quick method includes the following steps: (1) Install the target activated fuel cell stack on the test bench, first purge the cathode and anode with nitrogen, then heat the fuel cell stack to 70℃-80℃, control the anode inlet humidity and the cathode inlet humidity. During the entire activation process, the anode inlet humidity is maintained at 40-100%, the cathode humidity is maintained at 60-100%, the anode stoichiometric ratio is maintained at 1.6-2.0, and the cathode stoichiometric ratio is maintained at 2.0-2.4 except for the cathode starvation activation. The anode inlet pressure and the cathode inlet pressure are 160-280kPa and 140-260kPa respectively except for the cathode starvation activation. (2) When the temperature and intake air humidity of the battery stack reach the target values, current loading begins, and the loading and unloading rate is set to 3-40A / s; Specifically:
1. First, load the current to 2A / cm 2 , constant current for 1-20min, then quickly reduce the load to 0.3~0.5A / cm 2 , the cathode stoichiometric ratio is reduced to 1-1.2, the anode inlet pressure and the cathode inlet pressure are adjusted to 190 kPa and 170 kPa, the cathode starvation time is 5-60 s, after the cathode starvation time is over, the cathode stoichiometric ratio is restored to 2.0-2.2, the anode inlet pressure and the cathode inlet pressure are restored to the set value in step (1); 2, then the current is loaded to 2.5 A / cm 2 , constant current for 1-20min, then quickly reduce the load to 0.6~0.8A / cm 2 , the cathode stoichiometric ratio is reduced to 1-1.2, the anode inlet pressure and the cathode inlet pressure are adjusted to 200-220 kPa and 180-200 kPa, and the cathode starvation time is 5-60 s. After the cathode starvation time is over, the cathode stoichiometric ratio is restored to 2.0-2.2, and the anode inlet pressure and the cathode inlet pressure are restored to the set value in step (1); after completing steps 1 and 2, a round of activation test is completed. Repeating multiple rounds of activation test until the stack reaches the target performance is considered to be completed.
Citation Information
Patent Citations
Performance improvement strategy for proton exchange membrane fuel cell
CN107256976A
Method for activating fuel cell stack
CN118248902A
Fuel cell stack activation method
CN118263476A
Fuel cell system and its operating method
US20150207158A1
Cited By
Activation method of fuel cell, activated fuel cell and electric driving device
CN121839755A