Battery diaphragm and preparation method thereof, secondary battery and electric device

By setting up a conductive coating on the lithium battery separator, lithium dendrites are intercepted and a micro-short circuit is formed, the short circuit risk caused by the lithium dendrites piercing the lithium battery separator is solved, the time of accidents is extended, and the frequency and losses of accidents are reduced.

CN119009367APending Publication Date: 2024-11-22CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202310551408.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During multiple charge and discharge cycles of lithium batteries, the growth of lithium dendrites due to the uneven deposition of lithium ions increases the risk of the diaphragm being pierced, which in turn causes catastrophic accidents such as battery short circuit, ignition, gas production explosions, etc.

Method used

A conductive coating is provided on the separator of the lithium battery. The conductivity of the conductive coating is 102~106S/m, including conductive materials and insulating materials, conductive materials such as carbon nanotubes, graphene, and insulating materials such as aluminum oxide, through conduction The coating intercepts lithium dendrites, forming a low-current micro-short circuit, extending the time of the short circuit to a serious accident.

Benefits of technology

It effectively extends the time when lithium dendrites pierce the diaphragm to a serious accident, provides a longer time for the battery management system to warn, and reduces the damage and losses caused by serious accidents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009367A_ABST
    Figure CN119009367A_ABST
Patent Text Reader

Abstract

The invention discloses a battery diaphragm and a preparation method thereof, a secondary battery and an electric device, and relates to the field of batteries. The battery diaphragm comprises a base membrane and a coating, the coating is arranged on the surface of one side, facing a cathode of a battery, of the base membrane, and the material of the coating comprises a conductive material and an insulating material. According to the battery diaphragm, the conductive coating is arranged on the surface of the side, facing the cathode of the battery, of the base diaphragm, so that when the obtained battery diaphragm is applied to the lithium battery and lithium dendrites grow to completely penetrate through the side, not provided with the coating, of the base diaphragm, the lithium dendrites are intercepted by the arranged coating and do not directly contact with the cathode; and meanwhile, a low-current micro short circuit is formed by the conductive coating, so that the time from short circuit to serious accidents is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and in particular to a battery separator and a preparation method thereof, a secondary battery and an electrical device. Background Art

[0002] With the continuous development of the lithium battery industry, the demand for higher energy density has brought challenges to battery safety, and the use of thinner separators has increased the risk of separator puncture. Among them, lithium dendrites are one of the problems in the use of lithium batteries. During the multiple charge and discharge cycles of the battery, due to the uneven deposition of lithium ions, lithium dendrites will continue to grow on the surface of lithium metal. A large number of dendrites have a large stress on the separator, which will cause the separator to be punctured, thereby causing catastrophic accidents such as battery short circuit, fire, gas explosion, etc. Summary of the invention

[0003] The main purpose of this application is to propose a battery separator and a preparation method thereof, a secondary battery and an electrical device, aiming to provide a way to alleviate the risk of battery short circuit caused by lithium dendrites piercing the separator.

[0004] In a first aspect, the present application provides a battery separator, the battery separator comprising:

[0005] basement membrane; and

[0006] The coating is arranged on the surface of the side of the base film facing the cathode of the battery, and the material of the coating includes a conductive material and an insulating material.

[0007] In the technical solution of the embodiment of the present application, a conductive material and an insulating material having an electrical conductivity of 10 are provided on the surface of the base film facing the cathode of the battery. 2 ~10 6 S / m conductive coating, thus, one side of the base film of the battery separator is insulated, and the coating side is conductive, so that the battery separator can be called a "partially conductive separator". When this battery separator is used in a lithium battery, when lithium dendrites grow to completely penetrate the side of the base film where no coating is set (i.e., the insulating side), the lithium dendrites will be intercepted by the conductive coating and will not directly contact the cathode. At the same time, a low-current micro-short circuit is formed by the conductive coating, thereby extending the time from the short circuit to the occurrence of a serious accident.

[0008] In some embodiments, the electrical conductivity of the coating is 10 2 ~10 6 S / m. By controlling the conductivity of the coating at 10 2 ~10 6 Within the S / m range, the obtained battery separator has a significant effect in alleviating battery short circuit conditions.

[0009] In some embodiments, the conductive material includes at least one of carbon nanotubes, graphene, graphene oxide, carbon black, polystyrene sulfonate, polyaniline, nickel, copper, and platinum. At least one of the above substances is selected as the conductive material, which has good conductivity.

[0010] In some embodiments, the insulating material includes at least one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, nickel oxide, cerium oxide, zirconium titanate, barium titanate, and magnesium fluoride. At least one of the above substances is selected as the insulating material, which is low in cost, easy to obtain, and easy to control the conductivity of the coating.

[0011] In some embodiments, the conductive material is in granular form, and the Dv50 of the conductive material is 0.1-10 μm. By selecting a granular conductive material with a Dv50 of 0.1-10 μm, it is advantageous to control the thickness of the coating and its apparent properties.

[0012] In some embodiments, the conductive material is in granular form, and the Dv50 of the conductive material is 0.1 to 10 μm. By selecting a granular conductive material with a Dv50 of 1 to 3 μm, the conductive material is easier to disperse in the slurry used to prepare the coating, and the surface of the coating prepared subsequently is smoother and more uniform.

[0013] In some embodiments, the insulating material is in granular form, and the Dv50 of the insulating material is 0.1-10 μm. By selecting a granular insulating material with a Dv50 of 0.1-10 μm, it is helpful to control the thickness of the coating and its apparent properties.

[0014] In some embodiments, the insulating material is in granular form, and the Dv50 of the insulating material is 0.1-10 μm. By selecting a granular insulating material with a Dv50 of 1-3 μm, the insulating material is easier to disperse in the slurry used to prepare the coating, and the surface of the coating prepared subsequently is smoother and more uniform.

[0015] In some embodiments, the mass fraction of the conductive material in the coating is 30-90%. By controlling the mass fraction of the conductive material to be 30-90%, the conductivity of the coating can be adjusted to match the requirements of batteries of various structures and capacities.

[0016] In some embodiments, the mass ratio of the conductive material to the insulating material is 30 to 90: 1 to 64. By controlling the addition ratio of the conductive material to the insulating material, it is beneficial to adjust the conductivity of the coating.

[0017] In some embodiments, the material of the coating layer further includes a binder. By adding the binder, the coating layer can be better bonded to the base film, thereby improving the structural stability of the battery separator.

[0018] In some embodiments, the binder includes at least one of polyacrylate, acrylic acid, carboxymethyl cellulose, and polyvinylidene fluoride. Selecting at least one of the above substances as the binder makes the bonding with the base film stronger.

[0019] In some embodiments, the mass ratio of the binder to the conductive material is 5 to 10:30 to 90. By controlling the addition ratio of the binder, it is helpful to obtain a coating with suitable conductivity and good bonding with the base film.

[0020] In some embodiments, the coating material further comprises a dispersant. The addition of the dispersant helps to adjust the dispersion of the solid matter in the coating to obtain a more uniform coating with better apparent quality.

[0021] In some embodiments, the dispersant includes at least one of polyethylene glycol and polyacrylamide. At least one of the above substances is selected as the dispersant, which has a good dispersing effect on solid substances.

[0022] In some embodiments, the mass ratio of the dispersant to the conductive material is 1 to 5:30 to 90. By controlling the addition ratio of the dispersant, the dispersibility of the solid material can be well improved, thereby facilitating the reduction of the difficulty of coating processing and preparation.

[0023] In some embodiments, the material of the base film includes at least one of polyolefin, polyether, polyetheretherketone, polyimide, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymer, and copolymer containing CF bond. At least one of the above substances is selected as the material for making the base film, and the comprehensive performance of the obtained battery separator is better.

[0024] In a second aspect, the present application provides a method for preparing a battery separator, comprising the following steps:

[0025] Mixing conductive material, insulating material, binder and solvent to prepare coating slurry;

[0026] applying the coating slurry onto a base film;

[0027] Curing the coating slurry on the base film to form a coating to prepare a battery separator;

[0028] Wherein, the coating slurry includes conductive material and insulating material.

[0029] In the technical solution of the embodiment of the present application, a coating slurry containing a conductive material and an insulating material is coated on the surface of one side of a base film, and a conductive coating is formed on the base film by curing. When the prepared battery separator is used in a lithium battery, when lithium dendrites grow to completely penetrate the side of the base film where no coating is set, the lithium dendrites will be intercepted by the set conductive coating and will not directly contact the cathode. At the same time, a low-current micro-short circuit is formed by the conductive coating, thereby prolonging the time from the short circuit to the occurrence of a serious accident.

[0030] In some embodiments, the solvent includes at least one of acetone, deionized water, methyl ethyl ketone, and 3-pentanone. Selecting at least one of the above substances as the solvent is conducive to the dispersion of the conductive material, insulating material and other materials, thereby obtaining a slurry with suitable viscosity and uniform dispersion of solid substances.

[0031] In some embodiments, the solvent includes acetone. When acetone is selected as the solvent, the solid matter is dispersed more fully, and the coating slurry obtained is coated more evenly on the base film, which is conducive to obtaining a more uniform coating.

[0032] In some embodiments, the solid content of the coating slurry is 40-45%. By controlling the solid content of the coating slurry within the range of 40-45%, the coating slurry has a suitable viscosity, good coating performance, and fast curing speed.

[0033] In some embodiments, the step of curing the coating slurry on the base film to form a coating comprises:

[0034] The base film coated with the coating slurry is placed at a temperature of 40 to 45° C. and dried for 25 to 30 seconds.

[0035] The coating slurry is cured on the base film to form a coating by drying at 40-45° C. for 20-25 seconds. The formed coating has good surface quality, good bonding with the base film, and fast curing rate.

[0036] In a third aspect, the present application provides a secondary battery, wherein the secondary battery comprises the battery separator in the above embodiment or the battery separator prepared in the above embodiment.

[0037] In a fourth aspect, the present application provides an electrical device, wherein the electrical device comprises the secondary battery in the above-mentioned embodiment. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying any creative work.

[0039] Figure 1 This is a schematic diagram of the structure of the battery separator in some embodiments of the present application.

[0040] Description of Figure Numbers:

[0041] 10 Basement membrane 20 coating

[0042] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0043] Hereinafter, the battery separator and its preparation method, secondary battery and electrical device of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0044] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0045] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0046] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0047] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0048] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0049] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0050] At present, from the perspective of market development, the application of power batteries is becoming more and more extensive. Power batteries are not only used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, but also widely used in electric vehicles such as electric bicycles, electric motorcycles, electric cars, as well as military equipment and aerospace and other fields. With the continuous expansion of the application field of power batteries, the market demand is also constantly expanding.

[0051] At present, from the perspective of market development, the application of power batteries is becoming more and more extensive. Power batteries are not only used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, but also widely used in electric vehicles such as electric bicycles, electric motorcycles, electric cars, as well as military equipment and aerospace and other fields. With the continuous expansion of the application field of power batteries, the market demand is also constantly expanding.

[0052] In the actual use of secondary batteries, lithium dendrites are one of the main problems. During multiple charge and discharge cycles of the battery, lithium dendrites will continue to grow on the surface of lithium metal due to the uneven deposition of lithium ions. A large number of dendrites exert great stress on the diaphragm, which will cause the diaphragm to be pierced, thereby causing catastrophic accidents such as battery short circuit, fire, gas explosion, etc. The inventors have found through research that functional coatings are currently used to inhibit the growth of lithium dendrites, which can only delay the penetration of lithium dendrites, but cannot alleviate the short circuit caused by lithium dendrites piercing the diaphragm. The subsequent short circuit will still lead to serious failures and accidents.

[0053] Based on the above problems, the inventors have conducted in-depth research and proposed a new type of battery separator that can reduce the short circuit distance and control failure. Specifically, the present application provides a battery separator, see Figure 1 As shown, the battery separator includes a base film 10 and a coating 20. The coating 20 is disposed on a surface of the base film 10 facing the cathode of the battery. The conductivity of the coating 20 is 10 2 ~10 6 S / m, the material of the coating 20 includes conductive material and insulating material.

[0054] In the technical solution of the embodiment of the present application, a conductive material and an insulating material having an electrical conductivity of 10 are provided on the surface of the base film 10 facing the cathode of the battery. 2 ~10 6 S / m coating 20, thus, one side of the base film 10 of the battery separator is insulated (the resistance of the insulating side is greater than 9990 megohms measured by an insulation resistance meter), while the side of the coating 20 is conductive, so that the battery separator can be called a "partially conductive separator". When this battery separator is used in a lithium battery, when the lithium dendrites grow to completely penetrate the side of the base film 10 where the coating 20 is not set (i.e., the insulating side), the lithium dendrites will be intercepted by the set coating 20 and will not directly contact the cathode. At the same time, a low-current micro-short circuit is formed by the coating 20, thereby extending the time from the short circuit to the occurrence of a serious accident. Therefore, although it may eventually cause battery failure, it can provide a longer time for the battery management system to issue a timely warning, which is conducive to minimizing the damage and losses caused by serious accidents to a large extent.

[0055] In some embodiments of the present application, the conductive material includes at least one of carbon nanotubes, graphene, graphene oxide, carbon black, polystyrene sulfonate, polyaniline, nickel, copper, and platinum, and can be any one of the above substances, or a combination of any two or more thereof. Selecting at least one of the above substances as the conductive material has the advantage of good conductive performance, and it is easier to adjust the conductivity of the coating 20 when it is matched with an insulating material.

[0056] In some embodiments of the present application, the insulating material includes at least one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, nickel oxide, cerium oxide, zirconium titanate, barium titanate, and magnesium fluoride, and can be any one of the above substances or a combination of any two or more thereof. Selecting at least one of the above substances as the insulating material is low in cost, easy to obtain, and easier to control the conductivity of the coating 20 when combined with a conductive material.

[0057] In some embodiments of the present application, the conductive material is in a granular form, and the Dv50 of the conductive material is 0.1 to 10 μm. Wherein, Dv50 of 0.1 to 10 μm means that the particle size corresponding to 50% of the particle volume distribution is 0.1 to 10 μm. Therefore, by selecting a granular conductive material with a Dv50 of 0.1 to 10 μm, it is helpful to control the thickness of the coating 20, obtain a coating 20 with a thickness of 1 to 10 μm, and also help to improve the apparent performance of the coating 20.

[0058] In some embodiments of the present application, the conductive material is in granular form, and the Dv50 of the conductive material is 0.1 to 10 μm. By selecting a granular conductive material with a Dv50 of 0.1 to 10 μm, the conductive material is easier to disperse in the slurry used to prepare the coating 20, and the surface of the subsequently prepared coating 20 is smoother and more uniform.

[0059] In some embodiments of the present application, the insulating material is in a granular form, and the Dv50 of the insulating material is 0.1 to 10 μm. By selecting a granular insulating material with a Dv50 of 0.1 to 10 μm, it is helpful to adjust the thickness of the coating 20, obtain a coating 20 with a thickness of 1 to 10 μm, and also help improve the apparent performance of the coating 20.

[0060] In some embodiments of the present application, the insulating material is in granular form, and the Dv50 of the insulating material is 0.1 to 10 μm. By selecting a granular insulating material with a Dv50 of 0.1 to 10 μm, the insulating material is easier to disperse in the slurry used to prepare the coating 20, and the surface of the coating 20 prepared subsequently is smoother and more uniform.

[0061] In some embodiments of the present application, the mass fraction of the conductive material in the coating 20 is 30-90%. By controlling the mass fraction of the conductive material to be 30-90%, the conductivity of the coating 20 can be adjusted to match the requirements of batteries of various structures and capacities; at the same time, since the coating 20 is usually obtained by curing the slurry, controlling the mass fraction of the conductive material is also helpful to adjust the dispersion performance of the conductive material in the slurry and the coating performance of the slurry.

[0062] In some embodiments of the present application, the mass ratio of the conductive material to the insulating material is 30 to 90:1 to 64. By controlling the amount of insulating material added, it is helpful to adjust the conductivity of the coating 20; similarly, it is also helpful to adjust the dispersion performance of the conductive material in the slurry and the coating performance of the slurry.

[0063] In some embodiments of the present application, the material of the coating 20 also includes a binder. By adding the binder, the coating 20 is better bonded to the base film 10, and the structural stability of the battery separator is improved to ensure the performance of the battery.

[0064] In some specific embodiments of the present application, the binder includes at least one of polyacrylate, acrylic acid, carboxymethyl cellulose, and polyvinylidene fluoride, and can be any one of the above substances, or a combination of any two or more thereof. Selecting at least one of the above substances as a binder can make the conductive material, the insulating material and the base film 10 more firmly bonded, improve the bonding force between the coating 20 and the base film 10, and further improve the structural stability of the battery separator.

[0065] In some embodiments of the present application, the mass ratio of the binder to the conductive material is 5 to 10:30 to 90. By controlling the addition ratio of the binder, a coating 20 having excellent bonding properties with the base film 10 is obtained, and the conductive material and the insulating material are mixed and dispersed more evenly with the binder, which is beneficial to ensuring the conductivity of the coating 20.

[0066] In some embodiments of the present application, the material of the coating 20 further includes a dispersant. By adding the dispersant, the dispersion of the solid matter in the slurry used to prepare the coating 20 can be regulated, thereby helping to reduce the processing difficulty of the slurry, improve the coating performance of the slurry, and further adjust the dispersion of the solid matter in the coating 20, thereby obtaining a more uniform coating 20 with better apparent quality and more controllable conductivity.

[0067] In some specific embodiments of the present application, the dispersant includes at least one of polyethylene glycol and polyacrylamide, which can be any one of the above substances or a combination of the two substances. Selecting at least one of the above substances as the dispersant has a good dispersing effect on the conductive material, the insulating material and the binder.

[0068] In some embodiments of the present application, the mass ratio of the dispersant to the conductive material is 1 to 5:30 to 90. By controlling the addition ratio of the dispersant, the dispersibility of the solid substance in the slurry used to prepare the coating 20 can be well improved, thereby helping to reduce the processing difficulty of the slurry, improve the coating performance of the slurry, and reduce the process difficulty of preparing the coating 20.

[0069] In some embodiments of the present application, the material of the base film 10 includes at least one of polyolefin, polyether, polyetheretherketone, polyimide, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymer, and copolymer containing CF bond. At least one of the above substances is selected as the material for making the base film 10, and the comprehensive performance of the obtained battery separator is better. By selecting at least one of the above substances as the material for making the base film 10, the comprehensive performance of the obtained battery separator is better and the heat resistance is good. It should be noted that the “selection of any one of the above-mentioned substances” mentioned here means selecting polyolefin film, polyether film, polyetheretherketone film, polyimide film, polytetrafluoroethylene film, polyvinyl fluoride film, polyvinylidene fluoride film, polyvinylidene chloride film, polyethylene-propylene copolymer film or copolymer film containing CF bond as the base film 10; the “combination of any two or more of the above-mentioned substances may also be selected” means selecting a film made of a mixture formed by any two or more of the above-mentioned substances, or a composite film synthesized by a composite of any two or more of the films selected from polyolefin film, polyether film, polyetheretherketone film, polyimide film, polytetrafluoroethylene film, polyvinyl fluoride film, polyvinylidene fluoride film, polyvinylidene chloride film, polyethylene-propylene copolymer film and copolymer film containing CF bond as the base film 10. In the subsequent specific embodiments of the present application, the base film 10 will be described in detail by taking any one of the following as an example: a polyolefin film, a polyether film, a polyetheretherketone film, a polyimide film, a polytetrafluoroethylene film, a polyvinyl fluoride film, a polyvinylidene fluoride film, a polyvinylidene chloride film, a polyethylene-propylene copolymer film, or a copolymer film containing a CF bond.

[0070] In a second aspect, the present application provides a method for preparing a battery separator, comprising the following steps:

[0071] Mixing conductive material, insulating material, binder and solvent to prepare coating slurry;

[0072] Applying the coating slurry onto the base film 10;

[0073] The coating slurry is cured on the base film 10 to form a coating 20 to prepare a battery separator;

[0074] The coating slurry includes conductive material and insulating material.

[0075] In the technical solution of the embodiment of the present application, a coating slurry containing a conductive material and an insulating material is coated on one surface of the base film 10, and a coating slurry is cured on the base film 10 to form a coating 20, the conductivity of which is 10 2 ~10 6S / m, thus, one side of the base film 10 of the battery separator is insulated, while the side of the coating 20 is conductive, so that the battery separator can be called a "partially conductive separator". When this battery separator is used in a lithium battery, when the lithium dendrites grow to completely penetrate the side of the base film 10 where the coating 20 is not set, the lithium dendrites will be intercepted by the set coating 20 instead of directly contacting the cathode. At the same time, a low-current micro-short circuit is formed by the coating 20, thereby extending the time from the short circuit to the occurrence of a serious accident. Therefore, although it may still eventually cause battery failure, it can provide a longer time for the battery management system to issue a timely warning, which is conducive to minimizing the damage and losses caused by serious accidents to a large extent.

[0076] It is understandable that a dispersant may be added to the coating slurry to improve the dispersion of solid matter in the slurry and make the slurry coating more uniform. Correspondingly, in the step of preparing the coating slurry, the conductive material, insulating material, binder, dispersant and solvent are mixed.

[0077] Further, in some specific embodiments of the present application, the steps of preparing the coating slurry may be referred to as follows:

[0078] Mixing a binder with an insulating material to obtain a first mixture;

[0079] Dispersing the conductive material in a solvent to obtain a second mixed material;

[0080] The first mixed material and the second mixed material are mixed to prepare a coating slurry.

[0081] The dispersion of the conductive material in the solvent can be carried out by means of ultrasonic treatment, so that the dispersion of the conductive material is more uniform and rapid. In addition, when the first mixed material and the second mixed material are mixed, they can be carried out under heating and stirring conditions to accelerate the rapid and uniform dispersion of the materials. For example, they can be stirred at a temperature of 55 to 65° C. for 20 to 30 hours.

[0082] In some embodiments of the present application, the solvent includes at least one of acetone, deionized water, methyl ethyl ketone, and 3-pentanone. Selecting at least one of the above substances as the solvent is conducive to the full dispersion of the conductive material, the insulating material, and the binder, thereby obtaining a slurry with suitable viscosity and uniform dispersion of solid substances.

[0083] In some specific embodiments of the present application, the solvent includes acetone. When acetone is selected as the solvent, the solid matter is dispersed more fully, and the coating slurry obtained is coated more evenly on the base film 10, which is conducive to obtaining a more uniform coating 20.

[0084] In some embodiments of the present application, the solid content of the coating slurry is 40-45%. By controlling the solid content of the coating slurry within the range of 40-45%, the coating slurry has a suitable viscosity, good coating performance, fast curing speed, and is also conducive to reducing the difficulty of preparing the coating slurry.

[0085] In some embodiments of the present application, the step of curing the coating slurry on the base film 10 to form the coating 20 includes:

[0086] The base film 10 coated with the coating slurry is placed at a temperature of 40 to 45° C. and dried for 25 to 30 seconds.

[0087] The coating slurry is cured on the base film 10 to form a coating 20 by drying at 40-45°C for 20-25s. The solvent in the coating slurry is basically evaporated completely. The formed coating 20 has good surface quality, good bonding with the base film 10, and a fast curing rate.

[0088] In a third aspect, the present application provides a secondary battery, which includes the battery separator in the above embodiment or the battery separator prepared in the above embodiment.

[0089] The secondary battery includes a battery separator as in the above-mentioned embodiment, and also includes a positive electrode sheet, a negative electrode sheet and an electrolyte. The secondary battery can be a battery cell. Taking a lithium-ion battery as an example, a lithium-ion battery cell mainly relies on the movement of lithium ions between the positive electrode sheet and the negative electrode sheet to work. In a cylindrical battery cell, the thin film structure of three layers of material is wound into a cylindrical electrode assembly, while in a rectangular battery cell, the thin film structure is wound or stacked into an electrode assembly having a roughly rectangular shape.

[0090] In a common battery cell structure, the battery cell includes a shell, an electrode assembly and an electrolyte. The electrode assembly is contained in the shell of the battery cell, and the electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator. The shell includes a shell and an end cap. The shell includes a housing formed by a plurality of walls and an opening. The end cap is arranged at the opening to close the housing chamber. In addition to the electrode assembly, the housing chamber also contains an electrolyte. The positive electrode sheet and the negative electrode sheet in the electrode assembly include tabs. In order to ensure that a large current passes without melting, the number of positive tabs is multiple and stacked together, and the number of negative tabs is multiple and stacked together. The tabs are electrically connected to the electrode terminals located outside the battery cell through connecting members, and the electrode terminals generally include a positive electrode terminal and a negative electrode terminal. For a rectangular battery cell, the electrode terminal is generally arranged at the end cap portion. A plurality of battery cells are connected in series and / or in parallel via the electrode terminals for application in various applications.

[0091] The battery composed of cells formed by winding is called a wound battery. Wound batteries are also called cells, and battery industry insiders call them roll cores. Compared with flat batteries, wound batteries are made of high-voltage winding of plates with a thickness of only about 1mm. Through special process means, the battery has many characteristics: super high-rate discharge capability, with a maximum discharge rate of 18C to 30C; excellent high and low temperature performance, can work at -55℃ to 150℃; stable high output voltage, higher energy density; sturdy structure, with excellent seismic resistance; no free electrolyte (such as colloidal acid), can be placed in any direction for work; can be quickly charged, and can be charged with more than 95% of the power within 40 minutes (1C charging); super long life, the designed floating charge life can reach more than 8 years; extremely high resistance to low current deep discharge.

[0092] The electrolyte used in the present application may be an electrolyte known in the prior art, including an organic solvent, a lithium salt and an additive; the isolation membrane used in the present application may be an isolation membrane known in the prior art.

[0093] The secondary battery proposed in this application has all the beneficial effects of the above-mentioned battery separator, which will not be described in detail here.

[0094] A secondary battery can be a battery module. A battery module is formed by electrically connecting a certain number of secondary batteries together and placing them in a frame in order to protect the battery cells from external impact, heat, vibration, etc. A commonly used battery module generally includes two end plates, and a plurality of battery cells (secondary batteries) are arranged between the two end plates. The end plate provided with the output pole of the battery module is also called the output pole plate, and the end plate without the output pole of the battery module is also called the non-output pole plate.

[0095] Secondary batteries can also be battery packs. In some battery production and processing technologies, multiple battery cells are first integrated into battery modules, and then the battery modules are packaged in the battery box to form a battery pack. A battery pack can be packaged in one row of multiple battery modules, or multiple rows of multiple battery modules. The arrangement of multiple rows of multiple battery modules can be double rows and multiple columns, multiple rows and double columns, multiple rows and multiple columns, etc. Taking a battery pack that packages double rows and multiple columns of battery modules as an example, the first end plate of each column is generally the head output extreme plate, the two adjacent end plates between the two rows of battery modules are the middle non-output extreme plates, and the last end plate of each column is the tail non-output extreme plate. The head output extreme plate and one of the middle non-output extreme plates belong to the first row of battery modules, and one of the middle non-output extreme plates and the tail output extreme plate belong to the second row of battery modules.

[0096] In a fourth aspect, the present application provides an electrical device, which includes the secondary battery in the above embodiment.

[0097] The electrical devices proposed in the present application include but are not limited to: mobile phones, portable devices, laptop computers, electric vehicles, electric vehicles, ships, spacecraft, electric toys and electric tools, etc. For example, spacecraft include airplanes, rockets, space shuttles and spacecraft, etc. Electric toys include fixed or mobile electric toys, such as game consoles, electric vehicle toys, electric ship toys and electric airplane toys, etc. Electric tools include metal cutting electric tools, grinding electric tools, assembly electric tools and railway electric tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators and electric planers.

[0098] The electrical device proposed in this application has all the beneficial effects of the above-mentioned battery separator, which will not be described in detail here.

[0099] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0100] Example 1

[0101] The battery separator includes a polypropylene base film (thickness 4 μm, surface density 3 g / m 2 ) and a coating disposed on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 1 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (carbon nanotubes with an average length of 3μm and a conductivity of 207S / m), insulating material particles (silicon dioxide, Dv50 of 5μm) and a binder (polyvinylidene fluoride), and the mass ratio of the conductive material particles, the insulating material particles and the binder is 30:2:3.

[0102] Example 2

[0103] The battery separator includes a polypropylene base film (thickness 6 μm, surface density 4 g / m 2 ) and a coating disposed on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 2 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (graphene, Dv50 is 10μm), insulating material particles (aluminum oxide, Dv50 is 0.1μm) and binder (polyacrylate), and the mass ratio of conductive material particles, insulating material particles and binder is 40:1:5.

[0104] Example 3

[0105] The battery separator includes a polypropylene base film (thickness 8 μm, surface density 5 g / m 2 ) and a coating disposed on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 4 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (graphene oxide, Dv50 is 8μm), insulating material particles (zinc oxide, Dv50 is 1μm) and binder (acrylic acid), and the mass ratio of conductive material particles, insulating material particles and binder is 50:5:8.

[0106] Example 4

[0107] The battery separator includes a polypropylene base film (thickness 10 μm, surface density 6 g / m 2 ) and a coating disposed on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 4 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (carbon nanotubes with an average length of 3μm), insulating material particles (silicon dioxide, Dv50 is 5μm), a binder (polyvinylidene fluoride) and a dispersant (polyethylene glycol), and the mass ratio of the conductive material particles, the insulating material particles, the binder and the dispersant is 30:2:3:2.

[0108] Example 5

[0109] The battery separator includes a polypropylene base film (thickness 12 μm, surface density 7 g / m 2 ) and a coating disposed on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 5 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (carbon black, Dv50 is 6μm), insulating material particles (cerium oxide, Dv50 is 3μm), binder (polyacrylate, acrylic acid and carboxymethyl cellulose, mass ratio is 1:1:1) and dispersant (polyethylene glycol), and the mass ratio of conductive material particles, insulating material particles, binder and dispersant is 60:10:8:4.

[0110] Example 6

[0111] The battery separator includes a polypropylene base film (thickness 14 μm, surface density 8 g / m 2 ) and a coating disposed on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 6 μm and an electrical conductivity of 10 2 ~10 6S / m, the coating materials include conductive material particles (nickel, Dv50 is 0.1-10μm), insulating material particles (zirconium titanate, Dv50 is 10μm), binder (polyacrylate) and dispersant (polyethylene glycol), and the mass ratio of conductive material particles, insulating material particles, binder and dispersant is 70:30:7:3.

[0112] Example 7

[0113] The battery separator includes a polypropylene base film (thickness 5 μm, surface density 9 g / m 2 ) and a coating disposed on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 7 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (copper, Dv50 is 0.1-10μm), insulating material particles (titanium oxide, Dv50 is 6μm), binder (acrylic acid) and dispersant (polyacrylamide), and the mass ratio of conductive material particles, insulating material particles, binder and dispersant is 80:50:9:4.

[0114] Example 8

[0115] The battery separator includes a polypropylene base film (thickness 7 μm, surface density 10 g / m 2 ) and a coating disposed on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 8 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (carbon nanotubes with an average length of 1 μm, polystyrene sulfonate with a Dv50 of 3 μm, and a mass ratio of 1:1), insulating material particles (silicon dioxide with a Dv50 of 5 μm, nickel oxide with a Dv50 of 8 μm, and a mass ratio of 1:1), a binder (carboxymethyl cellulose) and a dispersant (polyacrylamide). The mass ratio of the conductive material particles, the insulating material particles, the binder and the dispersant is 90:64:10:5.

[0116] Example 9

[0117] The battery separator includes a polypropylene base film (thickness 9 μm, surface density 5 g / m 2 ) and a coating disposed on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 9 μm and an electrical conductivity of 10 2 ~10 6S / m, the materials of the coating include conductive material particles (polyaniline with a Dv50 of 0.1 to 10 μm, carbon black with a Dv50 of 0.1 to 10 μm, platinum with a Dv50 of 0.1 to 10 μm, and a mass ratio of 10:10:1), insulating material particles (calcium oxide with a Dv50 of 0.1 to 10 μm, zirconium oxide with a Dv50 of 4 μm, barium titanate with a Dv50 of 0.1 to 10 μm, and magnesium fluoride with a Dv50 of 0.1 to 10 μm, and a mass ratio of 1:1:1:1), a binder (carboxymethyl cellulose and polyacrylate, and a mass ratio of 1:1) and a dispersant (polyethylene glycol), and the mass ratio of the conductive material particles, the insulating material particles, the binder and the dispersant is 40:20:5:1.

[0118] Example 10

[0119] The battery separator includes a polypropylene base film (thickness 8 μm, surface density 8 g / m 2 ) and a coating disposed on the surface of the polypropylene base film on the side facing the battery cathode, the coating having a thickness of 10 μm and an electrical conductivity of 10 2 ~10 6 S / m, the coating materials include conductive material particles (carbon nanotubes with an average length of 3μm), insulating material particles (boehmite with a Dv50 of 0.1 to 10μm, tin dioxide with a Dv50 of 9μm, with a mass ratio of 3:1), a binder (polyvinylidene fluoride and acrylic acid, with a mass ratio of 2:1) and a dispersant (polyethylene glycol and polyacrylamide, with a mass ratio of 1:1), and the mass ratio of the conductive material particles, the insulating material particles, the binder and the dispersant is 30:10:10:5.

[0120] Embodiment 11

[0121] The structure and constituent materials of the battery separator are as described in Example 1. The preparation method of the battery separator includes:

[0122] (1) mixing a binder and insulating material particles in proportion to obtain a first mixture;

[0123] (2) adding the conductive material particles into acetone and dispersing them under ultrasonic conditions to obtain a second mixed material;

[0124] (3) adding the first mixture to the second mixture and stirring at 60° C. for 24 hours to obtain a coating slurry;

[0125] (4) The coating slurry was coated on a polypropylene base film, and then dried at 42° C. for 26 seconds to obtain a battery separator.

[0126] Example 12

[0127] The structure and constituent materials of the battery separator are as described in Example 1. The preparation method of the battery separator includes:

[0128] (1) mixing a binder and insulating material particles in proportion to obtain a first mixture;

[0129] (2) adding conductive material particles into deionized water and dispersing them under ultrasonic conditions to obtain a second mixed material;

[0130] (3) adding the first mixture into the second mixture and stirring at 55° C. for 30 hours to obtain a coating slurry;

[0131] (4) The coating slurry was coated on a polypropylene base film, and then dried at 40°C for 30 seconds to obtain a battery separator.

[0132] Embodiment 13

[0133] The structure and constituent materials of the battery separator are as described in Example 1. The preparation method of the battery separator includes:

[0134] (1) mixing a binder and insulating material particles in proportion to obtain a first mixture;

[0135] (2) adding conductive material particles into methyl ethyl ketone and dispersing the particles under ultrasonic conditions to obtain a second mixed material;

[0136] (3) adding the first mixture into the second mixture and stirring at 65° C. for 20 h to obtain a coating slurry;

[0137] (4) The coating slurry was coated on a polypropylene base film, and then dried at 45°C for 25 seconds to obtain a battery separator.

[0138] Embodiment 14

[0139] The structure and constituent materials of the battery separator are as described in Example 1. The preparation method of the battery separator includes:

[0140] (1) mixing a binder and insulating material particles in proportion to obtain a first mixture;

[0141] (2) adding conductive material particles to 3-pentanone and dispersing the particles under ultrasonic conditions to obtain a second mixed material;

[0142] (3) adding the first mixture into the second mixture and stirring at 65° C. for 20 h to obtain a coating slurry;

[0143] (4) The coating slurry was coated on a polypropylene base film, and then dried at 45°C for 25 seconds to obtain a battery separator.

[0144] Embodiment 15

[0145] The structure and constituent materials of the battery separator are as described in Example 3. The preparation method of the battery separator includes:

[0146] (1) mixing a binder and insulating material particles in proportion to obtain a first mixture;

[0147] (2) adding the conductive material particles into acetone and dispersing them under ultrasonic conditions to obtain a second mixed material;

[0148] (3) adding the first mixture to the second mixture and stirring at 60° C. for 24 hours to obtain a coating slurry;

[0149] (4) The coating slurry was coated on a polypropylene base film, and then dried at 42° C. for 27 seconds to obtain a battery separator.

[0150] Comparative Example 1

[0151] With a thickness of 4μm and a surface density of 3g / m 2 Polypropylene film is used as battery separator.

[0152] Comparative Example 2

[0153] The battery separator includes a polypropylene base film layer (thickness 4 μm, surface density 3 g / m 2 ), conductive coating (the conductive material in the coating is carbon nanotubes with an average length of 3μm) and insulating coating (the insulating material in the coating is silicon dioxide with a Dv50 of 5μm).

[0154] The battery separators prepared in each embodiment and the battery separators provided in the comparative examples were subjected to relevant performance tests, and the test methods and results are as follows:

[0155] (1) Production of coin battery:

[0156] Preparation of NMC (LiNi 0.5 Mn 0.2 Co 0.3 O2): Carbon: PVDF is a cathode slurry of 8:1:1, coated on aluminum foil, and the electrode thickness after drying and cold pressing is 80μm;

[0157] Assemble coin cells, use 1.0M LiPF DMC solution as electrolyte, use Li metal as anode, use 18mm diameter cathode and 20mm diameter anode for pairing, and assemble with the battery separator prepared in the embodiment and the battery separator provided in the comparative example respectively;

[0158] (2) Example Battery separator interception of lithium dendrites and the ability to generate controllable circuits:

[0159] At 1.2C (2mA / cm 2) and the short circuit condition of the battery was recorded. The results are shown in Table 1.

[0160] (3) Comparative battery separator short circuit test under lithium dendrites:

[0161] At 1.2C (2mA / cm 2 ) and the short circuit condition of the battery was recorded. The results are shown in Table 1.

[0162] Table 1 Short circuit test results of lithium dendrites of battery separators in Examples and Comparative Examples

[0163]

[0164]

[0165] According to the comparative test results in Table 1, the battery separator prepared in the embodiment began to alleviate the short circuit of the battery separator at least around the 60th cycle, which was manifested as an increase in the charging capacity required to reach the cut-off voltage. For example, the battery assembled with the battery separator prepared in Example 1 increased from (148mAh / g) in the 57th cycle to (165mAh / g) in the 60th cycle, and finally to (480mAh / g) in the 76th cycle. The battery separator prepared in the comparative example experienced a short circuit around the 49th cycle, which was manifested as a rapid drop in voltage, a rapid rise in current, and obvious self-discharge inside the surface battery. It can be seen that compared with the battery short circuit that occurred after the battery separator was pierced by lithium dendrites in the comparative example, the battery separator with a conductive coating prepared in the embodiment of the present application showed a relief of the battery short circuit after the lithium dendrites pierced the battery separator, thereby providing the operator with a certain warning and post-processing time, reducing the possibility of major accidents.

[0166] The above are only preferred embodiments of the present application, and do not limit the scope of the present application. For those skilled in the art, the present application may have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the scope of the patent protection of the present application.

Claims

1. A battery separator, characterized in that: The battery separator comprises: basement membrane; and The coating is arranged on the surface of the side of the base film facing the cathode of the battery, and the material of the coating includes a conductive material and an insulating material.

2. The battery separator according to claim 1, characterized in that The conductivity of the coating is 10 2 ~10 6 S / m.

3. The battery separator according to claim 1, characterized in that The conductive material includes at least one of carbon nanotubes, graphene, graphene oxide, carbon black, polystyrene sulfonate, polyaniline, nickel, copper, and platinum.

4. The battery separator according to claim 1, characterized in that The insulating material includes at least one of boehmite, aluminum oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, tin dioxide, titanium oxide, calcium oxide, zinc oxide, zirconium oxide, nickel oxide, cerium oxide, zirconium titanate, barium titanate, and magnesium fluoride.

5. The battery separator according to claim 1, characterized in that The conductive material is in granular form, and the Dv50 of the conductive material is 0.1 to 10 μm; and / or, The insulating material is in granular form, and the Dv50 of the insulating material is 0.1-10 μm.

6. The battery separator according to claim 1, characterized in that The conductive material is in granular form, and the Dv50 of the conductive material is 1 to 3 μm; and / or, The insulating material is in granular form, and the Dv50 of the insulating material is 1 to 3 μm.

7. The battery separator according to claim 1, characterized in that The mass fraction of the conductive material in the coating is 30-90%.

8. The battery separator according to claim 1, characterized in that The mass ratio of the conductive material to the insulating material is 30-90:1-64.

9. The battery separator according to claim 1, characterized in that The material of the coating layer also includes a binder.

10. The battery separator according to claim 9, characterized in that The binder comprises at least one of polyacrylate, acrylic acid, carboxymethyl cellulose and polyvinylidene fluoride; and / or, The mass ratio of the binder to the conductive material is 5-10:30-90.

11. The battery separator according to claim 1, characterized in that The coating material also includes a dispersant.

12. The battery separator according to claim 11, characterized in that The dispersant comprises at least one of polyethylene glycol and polyacrylamide; and / or, The mass ratio of the dispersant to the conductive material is 1-5:30-90.

13. The battery separator according to claim 1, characterized in that The material of the base film includes at least one of polyolefin, polyether, polyetheretherketone, polyimide, polytetrafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, polyvinylidene chloride, polyethylene-propylene copolymer, and copolymer containing CF bond.

14. A method for preparing a battery separator according to any one of claims 1 to 13, characterized in that: The following steps are involved: Mixing conductive material, insulating material, binder and solvent to prepare coating slurry; applying the coating slurry onto a base film; The coating slurry is cured on the base film to form a coating to prepare a battery separator.

15. The method for preparing a battery separator according to claim 14, characterized in that: The solvent includes at least one of acetone, deionized water, methyl ethyl ketone, and 3-pentanone.

16. The method for preparing a battery separator according to claim 14, characterized in that: The solvent includes acetone.

17. The method for preparing a battery separator according to claim 14, characterized in that: The solid content of the coating slurry is 40-45%.

18. The method for preparing a battery separator according to claim 14, characterized in that: The step of curing the coating slurry on the base film to form a coating comprises: The base film coated with the coating slurry is placed at a temperature of 40 to 45° C. and dried for 25 to 30 seconds.

19. A secondary battery, characterized in that: The secondary battery comprises the battery separator according to any one of claims 1 to 13 or a battery separator prepared by the method for preparing a battery separator according to any one of claims 14 to 18.

20. An electrical device, characterized in that: The electric device comprises the secondary battery as claimed in claim 19.

Citation Information

Cited By

  • Diaphragm and preparation method thereof, battery and power-related equipment

    CN119419448A

  • Battery separator and preparation method therefor, and secondary battery and electric device

    EP4668455A1

  • Battery separator and preparation method therefor, and secondary battery and electric device

    WO2024234652A1