Gas barrier laminate, packaging film, packaging container, and packaging product

By using a specific ratio of water-soluble polymers and silaneoxy compounds in the gas barrier laminate, the lamination strength and oxygen barrier properties of the laminate after cooking are improved, solving the problem of insufficient gas barrier properties after cooking in the prior art and achieving excellent oxygen barrier effect.

CN119013139APending Publication Date: 2024-11-22TOPPAN HOLDINGS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380032788.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-04-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing gas-barrier laminates have room for improvement in terms of lamination strength and oxygen barrier properties after cooking, especially after cooking and abuse treatments, where gas barrier properties are insufficient.

Method used

The structure employs a substrate layer containing thermoplastic resin, an inorganic oxide layer, and a gas barrier coating layer. The gas barrier coating layer is composed of water-soluble polymers and silaneoxy compounds and their hydrolysis products. By controlling the ratio and type of water-soluble polymers and silicon compounds, the adhesion and durability of the laminate are improved.

Benefits of technology

It improves the lamination strength and oxygen barrier properties of the laminate after cooking, ensuring that oxygen can still be effectively blocked after cooking and torture treatment, preventing the quality of the contents from deteriorating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013139A_ABST
    Figure CN119013139A_ABST
Patent Text Reader

Abstract

This gas barrier laminate is provided with, in this order, a substrate layer containing a resin, an inorganic oxide layer, and a gas barrier coating layer. The gas barrier coating layer is a cured product of a composition containing a water-soluble polymer, a first silicon compound comprising a siloxy compound of formula (1) or the like, and a second silicon compound comprising a siloxy compound of formula (2) or the like. The ratio of the water-soluble polymer to the water-soluble polymer in the second silicon compound is 55-95 mass%, and the ratio of the first silicon compound in the first silicon compound and the second silicon compound is more than 0 mass% and 89 mass% or less. Si (OR1) 4 (1) (R2Si (OR3) 3) n (2) (In formulae (1) and (2), R1 and R3 each represent an alkyl group or the like, and R2 represents an organic functional group. And n represents an integer of 1 or more).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a gas barrier laminate, a packaging film, a packaging container, and a packaging product. Background Art

[0002] In order to suppress the deterioration and corruption of the contents and maintain their functions and properties, packaging containers such as packaging bags used for packaging food, medicines, etc. are required to have gas barrier properties that prevent water vapor, oxygen, and other gases that deteriorate the contents from entering. Therefore, gas barrier laminates have been used in packaging containers.

[0003] The gas barrier laminate generally comprises a substrate layer, an inorganic oxide layer and a gas barrier coating layer in this order. The gas barrier coating layer is formed by applying a composition for forming a gas barrier coating layer that can impart a gas barrier function onto the inorganic oxide layer and curing the composition.

[0004] As such a gas barrier laminate, various laminates have been disclosed in the past.

[0005] For example, the following Patent Document 1 discloses a barrier laminate comprising a multilayer substrate, a vapor-deposited film, and a barrier coating layer provided on the vapor-deposited film, wherein the barrier coating layer is a barrier coating film composed of a resin composition containing a metal alkoxide, a water-soluble polymer, and a silane coupling agent.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent No. 6902231 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, the gas barrier laminate described in Patent Document 1 has the following problems.

[0011] That is, the gas barrier laminate described in Patent Document 1 has room for improvement in terms of achieving both lamination strength after retorting and oxygen barrier properties after retorting and abuse.

[0012] The present disclosure has been made in view of the above problems, and an object of the present disclosure is to provide a gas barrier laminate, a packaging film, a packaging container, and a packaging product which are excellent in lamination strength after retorting and also excellent in oxygen barrier properties after retorting and abuse treatment.

[0013] Means for solving problems

[0014] In order to solve the above-mentioned problems, the first aspect of the present disclosure provides a gas barrier laminate, which comprises, in order: a substrate layer containing a thermoplastic resin, an inorganic oxide layer, and a gas barrier coating layer, wherein the gas barrier coating layer is a cured product of a composition for forming a gas barrier coating layer, wherein the composition for forming a gas barrier coating layer comprises: a water-soluble polymer, a first silicon compound composed of at least one of a silane alkoxy compound represented by the following general formula (1) and a hydrolyzate thereof, and a second silicon compound composed of at least one of a silane alkoxy compound represented by the following general formula (2) and a hydrolyzate thereof, wherein the second silicon compound is converted into (R 2 Si(OH)3) n In the case of the water-soluble polymer and the second silicon compound, the mass ratio of the water-soluble polymer in the total mass of the water-soluble polymer and the second silicon compound is 55 to 95 mass %, when the first silicon compound is converted to SiO2 and the second silicon compound is converted to (R 2 Si(OH)3) n In the case of , the mass ratio of the first silicon compound in the total mass of the first silicon compound and the second silicon compound is greater than 0 mass % and is 89 mass % or less.

[0015] Si(OR 1 )4···(1)

[0016] (R 2 Si(OR 3 )3) n ···(2)

[0017] (In the above general formulas (1) and (2), R 1 , R 3 represents an alkyl group or -C2H4OCH3, R 2 represents an organic functional group. n represents an integer greater than 1. )

[0018] The gas barrier laminate of the present disclosure is excellent in lamination strength after retorting treatment, and is also excellent in oxygen barrier properties after retorting treatment and abuse treatment.

[0019] The reason why the gas barrier laminate disclosed in the present invention can achieve such an effect is still uncertain, but it is speculated that this is because, in addition to the base layer containing a thermoplastic resin, the gas barrier coating layer is also formulated with a water-soluble polymer, a first silicon compound, and a second silicon compound in a well-balanced manner, thereby increasing the lamination strength of the gas barrier coating layer to the base layer, improving the adhesion between the base layer and the gas barrier coating layer, and imparting thermal and mechanical durability to the gas barrier coating layer.

[0020] The second aspect of the present disclosure provides a gas barrier laminate, which is the gas barrier laminate of the first aspect, wherein the first silicon compound is converted to SiO2, the second silicon compound is converted to (R 2 Si(OH)3) n In the case of, the mass ratio of the first silicon compound in the total mass of the first silicon compound and the second silicon compound is 20 mass % or more and 89 mass % or less.

[0021] In this case, by curing the gas barrier coating layer-forming composition, more excellent gas barrier properties can be imparted to the gas barrier laminate.

[0022] The third aspect of the present disclosure provides a gas barrier laminate according to the first or second aspect, wherein when the second silicon compound is converted into (R 2 Si(OH)3) n In the case of the present invention, the mass ratio of the water-soluble polymer in the total mass of the water-soluble polymer and the second silicon compound is 75 to 90 mass %.

[0023] In this case, the oxygen barrier properties after retorting tend to be further improved compared to the case where the mass ratio of the water-soluble polymer is not within the above range.

[0024] A fourth aspect of the present disclosure provides a gas barrier laminate according to any one of the first to third aspects, wherein the thermoplastic resin is a polyolefin resin.

[0025] Generally, when a packaging container is manufactured using a gas barrier laminate in which the thermoplastic resin contained in the substrate layer is a polyolefin resin, intralayer peeling tends to occur easily when the packaging container is subjected to a retort treatment. In contrast, according to the gas barrier laminate of the present disclosure, the lamination strength of the gas barrier coating layer to the substrate layer is increased, so that even if a packaging container is manufactured using the gas barrier laminate and the packaging container is subjected to a retort treatment, the gas barrier coating layer is difficult to peel off from the substrate layer.

[0026] The fifth aspect of the present disclosure provides a gas barrier laminate according to any one of the first to fourth aspects, wherein the silane alkoxy compound constituting the second silicon compound is R in the general formula (2): 2 For NCO-R 4 -, said R 4 An alkylene group having an integer of 1 or more carbon atoms and a trimer 1,3,5-tris(3-trialkoxysilylalkyl)isocyanurate in which n is 3.

[0027] In this case, the moisture and heat resistance of the gas barrier coating layer is improved, and the lamination strength (adhesion strength) of the gas barrier coating layer to the base material layer after the retort treatment is improved.

[0028] A sixth aspect of the present disclosure provides a gas barrier laminate according to any one of the first to fourth aspects, wherein the silane alkoxy compound constituting the second silicon compound is R in the general formula (2): 2 It is 3-glycidoxypropyl, 3-glycidoxypropyltrialkoxysilane wherein n is 1.

[0029] In this case, the moisture and heat resistance of the gas barrier coating layer is improved, and the lamination strength (adhesion strength) of the gas barrier coating layer to the base material layer after the retort treatment is improved.

[0030] A seventh aspect of the present disclosure provides a gas barrier laminate according to any one of the first to sixth aspects, further comprising an anchor coating layer between the substrate layer and the inorganic oxide layer.

[0031] In this case, the surface smoothness of the anchor coating layer is improved compared to the surface smoothness of the substrate layer. Therefore, the thickness of the inorganic oxide layer can be made uniform, and the gas barrier properties of the gas barrier laminate can be further improved. In addition, the adhesion between the gas barrier coating layer and the inorganic oxide layer can be improved, and the intralayer peeling in the gas barrier laminate can be suppressed.

[0032] Moreover, the 8th aspect of this disclosure provides a packaging film provided with: the gas barrier laminate according to any one of the 1st to 7th aspects, and a sealant layer.

[0033] Since the packaging film includes the gas barrier layered product, it is excellent in lamination strength after retorting and also excellent in oxygen barrier properties after retorting and abuse.

[0034] Furthermore, a ninth aspect of the present invention provides a packaging container comprising the packaging film according to the eighth aspect.

[0035] Since the packaging container includes the packaging film, the gas barrier coating layer is unlikely to peel off even if the packaging film is retorted after being filled with the contents, and even if a force that deforms the packaging film is applied after the retorting treatment, degradation of the content quality due to oxygen intrusion can be suppressed for a long time.

[0036] Furthermore, a tenth aspect of the present disclosure provides a packaged product comprising: the packaging container according to the ninth aspect and a content filled in the packaging container.

[0037] Since the packaging product includes the above-mentioned packaging container, the gas barrier coating layer is difficult to peel off even if it is subjected to retorting treatment, and even if a force that deforms the packaging film is applied after the retorting treatment, the mixing of oxygen into the content can be suppressed, and the reduction in the quality of the content caused by the mixing of oxygen can be suppressed for a long time.

[0038] Effects of the Invention

[0039] According to the present disclosure, there are provided a gas barrier laminate, a packaging film, a packaging container, and a packaging product which are excellent in lamination strength after retorting treatment and also excellent in oxygen barrier properties after retorting treatment and abuse treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] [ Figure 1 ] is a cross-sectional view showing one embodiment of the gas barrier laminate disclosed in the present invention.

[0041] [ Figure 2 ] is a cross-sectional view showing an embodiment of the packaging film of the present disclosure.

[0042] [ Figure 3 ] is a side view showing an embodiment of the packaging product of the present disclosure DETAILED DESCRIPTION

[0043] Hereinafter, embodiments of the present disclosure will be described in detail.

[0044] <Gas Barrier Laminate>

[0045] First, refer to Figure 1 One embodiment of the gas barrier laminate of the present disclosure will be described. Figure 1 : is a cross-sectional view showing one embodiment of the gas barrier laminate disclosed in the present invention. Figure 1 In the embodiment, the gas barrier laminate 10 comprises, in order: a substrate layer 1 containing a thermoplastic resin, an inorganic oxide layer 3, and a gas barrier coating layer 4. The gas barrier coating layer 4 is a cured product of a composition for forming a gas barrier coating layer, and the composition for forming a gas barrier coating layer comprises: a water-soluble polymer, a first silicon compound composed of at least one of a silane alkoxy compound represented by the following general formula (1) and a hydrolyzate thereof, and a second silicon compound composed of at least one of a silane alkoxy compound represented by the following general formula (2) and a hydrolyzate thereof. When the second silicon compound is converted into R 2 In the case of Si(OH)3, the mass ratio of the water-soluble polymer to the total mass of the water-soluble polymer and the second silicon compound is 55 to 95 mass %, when the first silicon compound is converted to SiO2 and the second silicon compound is converted to R 2In the case of Si(OH) 3 , the mass ratio of the first silicon compound in the total mass of the first silicon compound and the second silicon compound is greater than 0 mass % and is 89 mass % or less.

[0046] Si(OR 1 )4···(1)

[0047] (R 2 Si(OR 3 )3) n ···(2)

[0048] (In the above general formulas (1) and (2), R 1 , R 3 represents an alkyl group or -C2H4OCH3, R 2 represents an organic functional group. n represents an integer greater than 1. )

[0049] It should be noted that the gas barrier laminate 10 may include an anchor coating layer 2 between the base layer 1 and the inorganic oxide layer 3 .

[0050] The gas barrier laminate 10 is excellent in lamination strength after retorting treatment and is also excellent in oxygen barrier properties after retorting treatment and abuse treatment.

[0051] Hereinafter, the base material layer 1 , the anchor coating layer 2 , the inorganic oxide layer 3 , and the gas barrier coating layer 4 will be described in detail.

[0052] (Base material layer)

[0053] The base layer 1 is a layer that serves as a support for the gas barrier coating layer 4, and contains a thermoplastic resin. Examples of the thermoplastic resin include polyolefin resins, polyester resins, polyamide resins, polyether resins, acrylic resins, and natural polymer compounds (cellulose acetate, etc.). The thermoplastic resin may be composed of a single resin or a mixture of two or more resins.

[0054] The present disclosure is particularly useful when the thermoplastic resin is a polyolefin resin. Generally, when a packaging container is made using a gas barrier laminate in which the thermoplastic resin contained in the substrate layer is used as the polyolefin resin, intralayer peeling tends to occur easily when the packaging container is subjected to a retort treatment. In contrast, according to the gas barrier laminate of the present disclosure, the lamination strength of the gas barrier coating layer 4 relative to the substrate layer 1 becomes greater, so that even if a packaging container is made using the gas barrier laminate 10 and the packaging container is subjected to a retort treatment, the gas barrier coating layer 4 is difficult to peel off from the substrate layer 1.

[0055] Examples of the polyolefin resin include polyethylene and polypropylene, but polypropylene is preferred from the viewpoint of resistance to retorting. Here, the polypropylene may be homopolypropylene or a propylene copolymer (polypropylene copolymer), but polypropylene copolymer is more preferred from the viewpoint of oxygen barrier properties.

[0056] Examples of the polyester resin include polyethylene terephthalate resin (PET) and polyethylene naphthalate resin (PEN).

[0057] The substrate layer 1 may be a stretched film or a non-stretched film, but is preferably a stretched film from the viewpoint of oxygen barrier properties. Here, as the stretched film, uniaxially stretched films and biaxially stretched films can be listed, but from the viewpoint of improving heat resistance, biaxially stretched films are preferred.

[0058] The thickness of the substrate layer 1 is not particularly limited, and may be, for example, 0.1 mm or less. The thickness of the substrate layer 1 is preferably 40 μm or less, more preferably 35 μm or less, and particularly preferably 30 μm or less. When the thickness of the substrate layer 1 is 40 μm or less, the flexibility of the gas barrier laminate 10 is further improved compared to the case where the thickness of the substrate layer 1 exceeds 40 μm, and the oxygen barrier property of the gas barrier laminate 10 after abuse can be further improved. However, from the viewpoint of improving strength, it is preferably 10 μm or more, and more preferably 12 μm or more.

[0059] The base material layer 1 may contain additives such as an antistatic agent, an ultraviolet absorber, a plasticizer, and a lubricant as necessary.

[0060] (Anchor coating)

[0061] The anchor coating layer 2 is a layer for further improving the adhesion between the base layer 1 and the inorganic oxide layer 3 , and is provided between the base layer 1 and the inorganic oxide layer 3 .

[0062] The material constituting the anchor coating layer 2 is not particularly limited as long as it can improve the adhesion between the substrate layer 1 and the inorganic oxide layer 3. Such a material includes a reaction product of an organic silane or organic metal compound, a polyol compound, and an isocyanate compound. That is, the anchor coating layer 2 can also be called a urethane adhesive layer.

[0063] The organosilane is, for example, a trifunctional organosilane or a hydrolysis product of a trifunctional organosilane.

[0064] The organometallic compound is, for example, a metal alkoxide or a hydrolysis product of a metal alkoxide. The metal element contained in the organometallic compound is, for example, Al, Ti, Zr, and the like.

[0065] It is sufficient that the hydrolyzate of the organosilane and the hydrolyzate of the metal alkoxide each have at least one hydroxyl group.

[0066] From the viewpoint of transparency, the polyol compound is preferably an acrylic polyol.

[0067] The isocyanate compound mainly functions as a crosslinking agent or a curing agent.

[0068] The polyol compound and the isocyanate compound may be a monomer or a polymer.

[0069] The thickness of the anchor coating layer 2 is not particularly limited as long as it can improve the adhesion between the substrate layer 1 and the inorganic oxide layer 3, but is preferably 30 nm or more. In this case, compared with the case where the thickness of the anchor coating layer 2 is less than 30 nm, the smoothness of the surface of the anchor coating layer 2 can be further improved compared to the surface of the substrate layer 1, the thickness of the inorganic oxide layer 3 can be made more uniform, and the oxygen barrier property can also be further improved. Therefore, the oxygen barrier property of the gas barrier laminate 10 can be further improved.

[0070] The thickness of the anchor coating layer 2 is more preferably 40 nm or more, and further preferably 50 nm or more. By increasing the thickness of the anchor coating layer 2, it is possible to further suppress a decrease in water vapor barrier properties when an external force such as tension is applied.

[0071] The thickness of the anchor coating 2 is preferably 300 nm or less. In this case, the flexibility of the gas barrier laminate 10 is further improved compared to the case where the thickness of the anchor coating 2 exceeds 300 nm, and the oxygen barrier property of the gas barrier laminate 10 after abuse can be further improved. The thickness of the anchor coating 2 is more preferably 200 μm or less. The thickness of the anchor coating 2 may be 150 μm or less, 120 μm or less, 100 μm or less, or 80 μm or less.

[0072] (Inorganic oxide layer)

[0073] The inorganic oxide layer 3 is a layer containing an inorganic oxide. The gas barrier laminate 10 can further improve the gas barrier property by including the inorganic oxide layer 3.

[0074] Examples of the inorganic oxide include oxides of at least one metal selected from the group consisting of Si, Al, Mg, Sn, Ti, and In; or non-metal-added metal oxides obtained by adding non-metals such as carbon or phosphorus to metal oxides. As the inorganic oxide, SiO is preferred from the viewpoint of water vapor barrier properties. x or AlO x Among them, SiO is preferred as the inorganic oxide. x In this case, the gas barrier laminate 10 can have more excellent water vapor barrier properties.

[0075] The inorganic oxide layer 3 may be composed of a single layer or a plurality of layers.

[0076] The thickness of the inorganic oxide layer 3 is not particularly limited, but is preferably 5 nm or more. In this case, the oxygen barrier property of the gas barrier laminate 10 is further improved compared to a case where the thickness of the inorganic oxide layer 3 is less than 5 nm.

[0077] The thickness of the inorganic oxide layer 3 is more preferably 8 nm or more, and particularly preferably 10 nm or more. The thickness of the inorganic oxide layer 3 may be 15 nm or more, or 20 nm or more.

[0078] In addition, the thickness of the inorganic oxide layer 3 is preferably 80 nm or less. In this case, compared with the case where the thickness of the inorganic oxide layer 3 exceeds 80 nm, the flexibility of the gas barrier laminate 10 is further improved, and the oxygen barrier property of the gas barrier laminate 10 after abuse can be further improved. In addition, the oxygen barrier property of the gas barrier laminate 10 after retorting can also be further improved.

[0079] The thickness of the inorganic oxide layer 3 is more preferably 70 nm or less, and particularly preferably 60 nm or less. The thickness of the inorganic oxide layer 3 may be 50 nm or less, 40 nm or less, or 30 nm or less.

[0080] (Gas barrier coating layer)

[0081] The gas barrier coating layer 4 is composed of a cured body or a cured product of the composition for forming a gas barrier coating layer.

[0082] The gas barrier coating layer-forming composition comprises: a water-soluble polymer, a first silicon compound consisting of at least one of a silane alkoxy compound represented by the general formula (1) and a hydrolyzate thereof, and a second silicon compound consisting of at least one of a silane alkoxy compound represented by the general formula (2) and a hydrolyzate thereof.

[0083] As water-soluble polymers, for example, polyvinyl alcohol resins, modified bodies thereof, and polyacrylic acid can be cited. They can be used alone or in combination of two or more. Among them, polyvinyl alcohol resins or modified bodies thereof are preferred as water-soluble polymers. In this case, the composition can impart better gas barrier properties to the gas barrier laminate 10 by curing. In addition, even if the composition is cured, it can impart better flexibility to the gas barrier laminate 10, and can further improve the oxygen barrier properties after abuse.

[0084] When the water-soluble polymer is composed of a polyvinyl alcohol resin or a modified product thereof, the saponification degree of the water-soluble polymer is not particularly limited, but is preferably 95% or more, and may be 100% from the viewpoint of improving the gas barrier properties of the gas barrier layered product 10 .

[0085] The degree of polymerization of the water-soluble polymer is not particularly limited, but is preferably 300 or more from the viewpoint of improving the gas barrier properties of the gas barrier laminate 10. The degree of polymerization of the water-soluble polymer is preferably 450 to 2,400.

[0086] The first silicon compound is composed of at least one of the silane alkoxy compound represented by the above general formula (1) and a hydrolyzate thereof.

[0087] In the general formula (1) representing the silane oxy compound, R 1 Represents an alkyl group or -C2H4OCH3. Examples of the alkyl group include a methyl group and an ethyl group. Among them, an ethyl group is preferred. In this case, the silane alkoxy compound becomes tetraethoxysilane, which can be relatively stable in an aqueous solvent after hydrolysis.

[0088] The second silicon compound is composed of at least one of the silane alkoxy compound represented by the general formula (2) and a hydrolyzate thereof. The second silicon compound functions as a curing agent and is also called a silane coupling agent.

[0089] In the general formula (1) representing the silane alkoxy compound constituting the second silicon compound, R 2 Represents a monovalent organic functional group, R 3 It represents an alkyl group or -C2H4OCH3.

[0090] In this case, the adhesion between the gas barrier coating layer 4 and the inorganic oxide layer 3 can be improved, and delamination in the gas barrier laminate 10 can be suppressed.

[0091] It should be noted that R 2 and R 3 They may be the same or different. 3 They can be the same as or different from each other.

[0092] As R 2 The monovalent organic functional group represented by , can include a monovalent organic functional group containing a vinyl group, an epoxy group, a mercapto group, an amino group or an isocyanate group. Among them, as the monovalent organic functional group, a monovalent organic functional group containing an isocyanate group is preferred. In this case, by curing the composition, it can have better hot water resistance, and even after the boiling treatment, it can give the gas barrier laminate 10 a greater lamination strength.

[0093] As R3 The alkyl group represented by , for example, methyl group, ethyl group, etc. are listed. Among them, methyl group is preferred. In this case, hydrolysis proceeds rapidly.

[0094] n represents an integer greater than 1. When n is 1, the second silicon compound represents a monomer, whereas when n is 2 or greater, the second silicon compound represents a polymer. n is preferably 3. In this case, the hot water resistance of the gas barrier coating layer 4 can be further improved, and a greater lamination strength can be imparted to the gas barrier laminate 10 even after the retort treatment.

[0095] The silane alkoxy compound constituting the second silicon compound is preferably R 2 For NCO-R 4 -、R 4 The alkylene group is an integer of 1 or more carbon atoms, and the trimer 1,3,5-tris(3-trialkoxysilylalkyl)isocyanurate wherein n is 3. In this case, the moisture-heat resistance of the gas barrier coating layer 4 is improved, and the lamination strength (adhesion strength) of the gas barrier coating layer 4 to the substrate layer 1 after the retort treatment is improved.

[0096] The silane alkoxy compound constituting the second silicon compound may also be R 2 3-glycidoxypropyl, 3-glycidoxypropyltrialkoxysilane wherein n is 1. In this case, the moisture-heat resistance of the gas barrier coating layer 4 is improved, and the lamination strength (adhesion strength) of the gas barrier coating layer 4 to the base layer 1 after the retort treatment is improved.

[0097] As the silane oxy compound constituting the second silicon compound, for example, there can be listed: silane coupling agents having a vinyl group such as vinyl trimethoxysilane and vinyl triethoxysilane; silane coupling agents having an epoxy group such as 3-glycidoxypropyl trimethoxysilane, 3-glycidoxypropyl triethoxysilane, 3-glycidoxypropyl methyl dimethoxysilane, 3-glycidoxypropyl ethyl diethoxysilane; silane coupling agents having a mercapto group such as 3-mercaptopropyl trimethoxysilane and 3-mercaptopropyl methyl dimethoxysilane; silane coupling agents having an amino group such as 3-aminopropyl trimethoxysilane and 3-aminopropyl triethoxysilane; silane coupling agents having an isocyanate group such as 3-isocyanate propyl triethoxysilane and 1,3,5-tris (3-methoxysilyl propyl) isocyanurate. These second silicon compounds can be used alone or in combination of two or more.

[0098] When the second silicon compound is converted into R 2In the case of Si(OH)3, the mass ratio of the water-soluble polymer in the total mass of the water-soluble polymer and the second silicon compound may be 55 to 95 mass %, preferably 60 to 90 mass %, and more preferably 75 to 90 mass %. In this case, compared with the case where the mass ratio of the water-soluble polymer is not within the above range, the oxygen barrier property after the retorting treatment tends to be further improved.

[0099] After converting the first silicon compound into SiO2 and the second silicon compound into R 2 In the case of Si(OH)3, the mass ratio of the first silicon compound in the total mass of the first silicon compound and the second silicon compound is greater than 0 mass% and less than 89 mass%, preferably greater than 20 mass% and less than 89 mass%. In this case, by curing the gas barrier coating layer forming composition, it is possible to impart a more excellent gas barrier property to the gas barrier laminate 10. In addition, the mass ratio of the first silicon compound may be greater than 0 mass% and less than 60 mass%, or may be 20 to 60 mass%. In this case, the oxygen barrier property after the retorting treatment and the abuse treatment tends to be further improved.

[0100] (Other ingredients)

[0101] The composition for forming a gas barrier coating layer may further contain known additives such as a dispersant, a stabilizer, a viscosity modifier, and a colorant as necessary within a range that does not impair the gas barrier properties of the gas barrier coating layer 4 .

[0102] (liquid)

[0103] The composition for forming the gas barrier coating layer may contain a liquid that dissolves or disperses the solid component. As such a liquid, an aqueous medium is generally used. As the aqueous medium, water, a hydrophilic organic solvent or a mixture thereof may be cited. As the hydrophilic organic solvent, for example, alcohols such as methanol, ethanol, and isopropanol; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; cellosolves; carbitols; nitriles such as acetonitrile, etc. may be cited. These may be used alone or in combination of two or more.

[0104] The aqueous medium is preferably an aqueous medium consisting only of water or an aqueous medium containing water as a main component. When the aqueous medium contains water as a main component, the content of water in the aqueous medium is preferably 70% by mass or more, more preferably 80% by mass or more.

[0105] The thickness of the gas barrier coating layer 4 is not particularly limited, but is preferably 50 nm or more.

[0106] In this case, compared with the case where the thickness of the gas barrier coating layer 4 is less than 50 nm, the oxygen barrier property of the gas barrier laminate 10 is further improved.

[0107] From the viewpoint of improving the gas barrier property, the thickness of the gas barrier coating layer 4 is more preferably 100 nm or more, particularly preferably 200 nm or more.

[0108] On the other hand, the thickness of the gas barrier coating layer 4 is preferably 700 nm or less. Compared with the case where the thickness of the gas barrier coating layer 4 exceeds 700 nm, the flexibility of the gas barrier laminate 10 is further improved, and the oxygen barrier property of the gas barrier laminate 10 after abuse can be further improved. In addition, the oxygen barrier property of the gas barrier laminate 10 after retorting can also be further improved.

[0109] From the viewpoint of further improving the flexibility of the gas barrier laminate 10 , the thickness of the gas barrier coating layer 4 is more preferably 500 nm or less, particularly preferably 400 nm or less.

[0110] <Method for producing gas barrier laminate>

[0111] Next, a method for producing the gas barrier laminate 10 will be described.

[0112] First, the base material layer 1 is prepared.

[0113] Next, the anchor coating layer 2 is formed on one surface of the base material layer 1 .

[0114] Specifically, the anchor coating layer 2 is formed by applying the anchor coating layer forming composition to one surface of the base layer 1 and heating and drying it. The heating temperature is, for example, 50 to 200° C. and the drying time is, for example, about 10 seconds to 10 minutes.

[0115] Next, the inorganic oxide layer 3 is formed on the anchor coating layer 2 .

[0116] The inorganic oxide layer 3 can be formed, for example, by a vacuum film forming method. Examples of the vacuum film forming method include physical vapor deposition and chemical vapor deposition. Examples of the physical vapor deposition method include vacuum evaporation, sputtering evaporation, and ion plating.

[0117] As the physical vapor deposition method, a vacuum deposition method is particularly preferably used. Examples of the vacuum deposition method include a resistance heating vacuum deposition method, an EB (electron beam) heating vacuum deposition method, and an induction heating vacuum deposition method.

[0118] Examples of the chemical vapor deposition method include a thermal CVD method, a plasma CVD method, and a photo CVD method.

[0119] Next, the gas barrier coating layer 4 is formed on the inorganic oxide layer 3 .

[0120] The gas barrier coating layer 4 can be formed, for example, by coating a composition for forming a gas barrier coating layer on the inorganic oxide layer 3 and curing it. Here, curing the solid component means that the first silicon compound and the water-soluble polymer, or the first silicon compound, the water-soluble polymer and the second silicon compound in the solid component react with each other to form an integrated structure. In addition, the composition for forming a gas barrier coating layer comprises a water-soluble polymer, a first silicon compound, and a second silicon compound, and is prepared such that: when the second silicon compound is converted into R 2 In the case of Si(OH)3, the mass ratio of the water-soluble polymer to the total mass of the water-soluble polymer and the second silicon compound is 55 to 95 mass %, when the first silicon compound is converted to SiO2 and the second silicon compound is converted to R 2 In the case of Si(OH) 3 , the mass ratio of the first silicon compound in the total mass of the first silicon compound and the second silicon compound is greater than 0 mass % and is 89 mass % or less.

[0121] As a coating method of the gas barrier coating layer-forming composition, a known method can be adopted, and specific examples of the coating method include wet film-forming methods such as gravure coating, dip coating, reverse coating, bar coating, and die coating.

[0122] Curing can be performed by, for example, heating or the like.

[0123] When curing is performed by heating, the heating temperature and heating time may be set so as to simultaneously cure the solid content in the gas barrier coating layer-forming composition and remove the liquid such as the aqueous medium. The heating temperature may be, for example, 80 to 250° C., and the heating time may be, for example, 3 seconds to 10 minutes.

[0124] As described above, the gas barrier laminate 10 is obtained.

[0125] <Packaging film>

[0126] Next, refer to Figure 2 The embodiment of the packaging film disclosed in the present invention is described. It should be noted that Figure 2 In, with Figure 1 The same components are denoted by the same reference numerals, and repeated descriptions are omitted.

[0127] Figure 2 is a cross-sectional view showing an embodiment of the packaging film of the present disclosure. Figure 2 As shown, the packaging film 20 includes a gas barrier laminate 10 and a sealant layer 21 laminated on the gas barrier laminate 10. The sealant layer 21 is arranged on the gas barrier coating layer 4 side of the base layer 1 of the gas barrier laminate 10. Figure 2As shown, in the gas barrier laminate 10 , the gas barrier coating layer 4 and the sealant layer 21 may be bonded together via an adhesive layer 22 .

[0128] Since the packaging film 20 includes the gas barrier laminate 10, it is excellent in lamination strength after retorting and also excellent in oxygen barrier properties after retorting and abuse.

[0129] As the material of the adhesive layer 22, polyester-isocyanate resin, urethane resin, polyether resin, etc. can be used. When the packaging film 20 is used for retort application, a two-component curing type urethane adhesive having retort resistance can be preferably used.

[0130] (Sealing layer)

[0131] As the material of the sealing layer 21, thermoplastic resins such as polyolefin resins and polyester resins can be listed, and polyolefin resins are generally used. Specifically, as the polyolefin resin, ethylene resins such as low-density polyethylene resin (LDPE), medium-density polyethylene resin (MDPE), linear low-density polyethylene resin (LLDPE), ethylene-vinyl acetate copolymer (EVA), ethylene-α-olefin copolymer, ethylene-(meth)acrylic acid copolymer, etc.; polypropylene resins such as homopolypropylene resin (PP), propylene-ethylene random copolymer, propylene-ethylene block copolymer, propylene-α-olefin copolymer, etc.; or mixtures thereof, etc. can be used. The material of the sealing layer 21 can be appropriately selected from the above-mentioned thermoplastic resins according to the use purpose, boiling treatment, cooking treatment, etc. temperature conditions.

[0132] The thermoplastic resin constituting the sealant layer 21 may be stretched or not stretched, but is preferably not stretched from the viewpoint of lowering the melting point and facilitating heat sealing.

[0133] The thickness of the sealing layer 21 is appropriately determined according to the mass of the content, the shape of the packaging bag, etc., and is not particularly limited. The thickness of the sealing layer 21 may be 30 μm or more, 40 μm or more, or 50 μm or more. In addition, the thickness of the sealing layer 21 may be 150 μm or less, 120 μm or less, 100 μm or less, or 80 μm or less. From the viewpoint of the flexibility and adhesion of the packaging film 20, it is preferably 30 to 150 μm.

[0134] <Packaging products>

[0135] Next, refer to Figure 3 The embodiments of the packaging product disclosed in the present invention are described. It should be noted that: Figure 3 is a side view showing one embodiment of the packaging product of the present disclosure. Figure 3 In, with Figure 1 or Figure 2The same components are denoted by the same reference numerals, and repeated descriptions are omitted.

[0136] like Figure 3 As shown, the packaged product 40 includes a packaging container 30 and content C filled in the packaging container 30 . Figure 3 The packaging container 30 shown is obtained by using a pair of packaging films 20 and heat-sealing the peripheral edges of the packaging films 20 in a state where the sealing layers 21 face each other. Figure 3 In the figure, the adhesive layer 22 of the packaging film 20 is omitted.

[0137] Since the packaging product 40 includes the packaging container 30, the gas barrier coating layer 4 is difficult to peel off even if it is subjected to boiling treatment, and even if a force that deforms the packaging film 20 is applied after the boiling treatment, the mixing of oxygen into the content C can be suppressed, thereby suppressing the reduction in the quality of the content C caused by the mixing of oxygen for a long time.

[0138] In addition, the packaging container 30 can also be obtained by bending one packaging film 20 and heat-sealing the peripheral edge portion of the packaging film 20 in a state where the sealing layers 21 face each other.

[0139] Examples of the packaging container 30 include packaging bags, laminated tube containers, and liquid paper containers.

[0140] The content C is not particularly limited, and examples of the content C include food, liquid, medicine, and electronic components.

[0141] For example, in the above embodiment, in the packaging film 20, the sealing layer 21 is arranged on the gas barrier coating layer 4 side of the base layer 1 of the gas barrier laminate 10, but the sealing layer 21 may be arranged on the side of the base layer 1 opposite to the gas barrier coating layer 4.

[0142] Example

[0143] Hereinafter, the present disclosure will be specifically described by giving examples, but the present disclosure is not limited to these examples.

[0144] <Preparation of coating solution>

[0145] Coating liquids A to D for preparing the gas barrier coating layer-forming composition used in Examples or Comparative Examples were prepared as follows.

[0146] (Coating liquid A)

[0147] Polyvinyl alcohol (trade name: "Kuraray Poval 60-98", manufactured by Kuraray Co., Ltd., hereinafter also referred to as "PVA") and water were mixed to prepare a coating liquid A having a solid content of 5% by mass.

[0148] (Coating liquid B)

[0149] Tetraethoxysilane (trade name: "KBE04", solid content: 100%, manufactured by Shin-Etsu Chemical Co., Ltd., hereinafter also referred to as "TEOS") as a silane oxide compound (first compound), methanol (Kanto Chemical) and 0.1N hydrochloric acid (Kanto Chemical Co., Ltd.) were mixed in a mass ratio of 17 / 10 / 73 to prepare a coating liquid B having a solid content ratio of 5 mass%. At this time, the solid content ratio was calculated by converting TEOS into SiO2.

[0150] (Coating liquid C1)

[0151] 1,3,5-tris(3-methoxysilylpropyl)isocyanurate as a silane coupling agent (SC agent A) was added to a mixed solvent of water / IPA = 1 / 1 (mass ratio) to obtain a coating liquid C1 having a solid content ratio of 5 mass%. The solid content ratio was calculated by converting SC agent A into NCO(CH2)3Si(OH)3.

[0152] (Coating liquid C2)

[0153] 0.1N hydrochloric acid (manufactured by Kanto Chemical Co., Ltd.) was added to an isopropyl alcohol (IPA) solution of 3-glycidoxypropyltrimethoxysilane as a silane coupling agent (SC agent B), and the resulting solution was stirred for 30 minutes to hydrolyze the SC agent B, and then added to a mixed solvent of water / IPA = 1 / 1 (mass ratio), thereby obtaining a coating liquid C2 having a solid content ratio of 5 mass%. The solid content ratio was calculated by converting the SC agent B into (CH2O)CH2OC3H6Si(OH)3.

[0154] <Preparation of Anchor Coat Layer-Forming Composition>

[0155] The anchor coating layer-forming composition was prepared as follows.

[0156] Acrylic polyol and toluene diisocyanate were mixed so that the number of NCO groups of toluene diisocyanate was equal to the number of OH groups of acrylic polyol, and diluted with ethyl acetate so that the solid content (the total amount of acrylic polyol and toluene diisocyanate) was 5% by mass. β-(3,4-epoxycyclohexyl)trimethoxysilane was further added to the diluted mixed solution so that it was 5 parts by mass relative to 100 parts by mass of the total amount of acrylic polyol and toluene diisocyanate, and these were mixed to prepare a composition for forming an anchor coating layer (anchor coating agent).

[0157] <Production of Gas Barrier Laminate>

[0158] (Example 1)

[0159] First, the anchor coating agent prepared above was applied to a biaxially stretched polypropylene film (trade name "ME-1", manufactured by Mitsui Chemicals Tohcello Co., Ltd.) having a thickness of 20 μm as a substrate layer to a thickness of 50 nm, and then dried after heating at 100° C. to form an anchor coating layer. Next, silicon oxide as an inorganic oxide was vapor-deposited on the anchor coating layer by an electron beam vacuum vapor deposition method using an electron beam heating method to form an inorganic oxide layer having a thickness of 25 nm, thereby obtaining a laminate.

[0160] Then, the coating liquids A, B and C1 were mixed so that the mass ratio of the water-soluble polymer in the total mass of the water-soluble polymer and the second silicon compound (hereinafter, also referred to as "the mass ratio of the water-soluble polymer X1") and the mass ratio of the first silicon compound in the total mass of the first silicon compound and the second silicon compound (hereinafter, also referred to as "the mass ratio of the first silicon compound X2") were the ratios shown in Table 1 to prepare a mixed solution, and the mixed solution was applied to the surface of the inorganic oxide layer of the above-mentioned stacked body by a bar coating method with a thickness of 400 nm to form a gas barrier coating layer. In this way, a gas barrier stacked body having an inorganic oxide layer, a substrate layer, an anchor coating layer, an inorganic oxide layer and a gas barrier coating layer stacked in this order was obtained.

[0161] (Examples 2, 4 and 5)

[0162] A gas barrier laminate was obtained in the same manner as in Example 1 except that the coating liquids A, B, and C1 were mixed so that the mass ratio X1 of the water-soluble polymer and the mass ratio X2 of the first silicon compound were the ratios shown in Table 1 to prepare a mixed liquid.

[0163] (Examples 3 and 6)

[0164] A gas barrier laminate was obtained in the same manner as in Example 1 except that the coating liquids A, B and C1 were mixed to prepare a mixed liquid so that the mass ratio X1 of the water-soluble polymer and the mass ratio X2 of the first silicon compound were the ratios shown in Table 1 and no anchor coating layer was formed.

[0165] (Example 7)

[0166] A gas barrier laminate was obtained in the same manner as in Example 1 except that the coating liquids A, B and C2 were mixed so that the mass ratio X1 of the water-soluble polymer and the mass ratio X2 of the first silicon compound were the ratios shown in Table 1 to prepare a mixed liquid.

[0167] (Comparative Examples 1 to 3)

[0168] A gas barrier laminate was obtained in the same manner as in Example 1 except that the coating liquids A, B, and C1 were mixed so that the mass ratio X1 of the water-soluble polymer and the mass ratio X2 of the first silicon compound were the ratios shown in Table 1 to prepare a mixed liquid.

[0169] <Production of Laminated Film>

[0170] By using a two-component adhesive (trade name "Takelac A-525 / Takenate A-52", manufactured by Mitsui Chemicals & SKC Polyurethanes Inc.), a 60 μm thick unstretched polypropylene film (trade name "Torayfan (registered trademark) ZK207", manufactured by Toray Industries, Ltd.) was adhered to the surface of the substrate layer of the gas barrier laminate obtained in Examples 1 to 7 and Comparative Examples 1 to 3, thereby producing a laminate film with a surface width of 210 mm.

[0171] <Evaluation of Laminated Film>

[0172] The laminated films obtained above were evaluated for oxygen barrier properties and lamination strength as follows.

[0173] (1) Oxygen barrier properties

[0174] The oxygen barrier properties of the laminated films produced above after retorting and after retorting and abuse were evaluated as follows.

[0175] (1-1) Oxygen barrier properties after retorting

[0176] (Preparation of test samples)

[0177] First, in order to evaluate the oxygen barrier properties after retorting, a test sample A was prepared as follows.

[0178] First, a sheet of 315 mm in length and 230 mm in width was cut from the laminated film produced above, and a three-side sealed bag with an opening was produced using the sheet. At this time, the three-side sealed bag was formed by bending the laminated film so that the unstretched polypropylene films were opposite to each other and heat-sealing the unstretched polypropylene films to each other. Then, water was injected into the three-side sealed bag from the opening to seal the opening of the three-side sealed bag. In this way, test sample A was produced.

[0179] (Steaming treatment)

[0180] The test sample A obtained above was subjected to a retort treatment at 121°C for 30 minutes.

[0181] (Determination of oxygen permeability)

[0182] Then, the oxygen permeability of the test sample A after the retorting treatment was measured at a temperature of 30°C and a relative humidity of 70% using an oxygen permeability measuring device (product name "OX-TRAN 2 / 20", manufactured by MOCON Co., Ltd.). The measurement was performed in accordance with JIS K-7126-2. The results are shown in Table 1.

[0183] (1-2) Oxygen barrier properties after retorting and abuse

[0184] (Preparation of test samples)

[0185] A sheet of 295 mm in length and 210 mm in width was cut out from the upper portion of the test sample A subjected to the retort treatment, and this sheet was designated as the test sample B.

[0186] (Abusive Testing)

[0187] Then, the test sample B was subjected to an abuse test (Gelbo flex test) as follows, thereby performing an abuse treatment.

[0188] That is, first, the test sample B was mounted on the fixed head of the Gelbo flex tester (manufactured by Tester Sangyo Co., Ltd.) in a cylindrical shape with a diameter of 87.5 mm × 210 mm to produce a cylindrical body. Then, the two ends of the cylindrical body were held, the initial holding interval was set to 175 mm, the stroke was set to 87.5 mm, and a reciprocating motion of applying a 440-degree twisting operation was repeated 5 times at a speed of 40 times / minute to bend the cylindrical body. In this way, an abusive test was performed.

[0189] (Determination of oxygen permeability)

[0190] Then, the oxygen permeability of the test sample B after the abuse treatment was measured in the same manner as the measurement of the oxygen permeability after the retort treatment described above. The results are shown in Table 1.

[0191] (2)Lamination strength

[0192] First, the lamination strength of the test sample A prepared as described above was measured in accordance with JIS Z-1707.

[0193] Specifically, the test sample A was first cut into short strips with a width of 15 mm to obtain a cut sample. Then, using a Tensilon universal material testing machine (product name "Tensilon RTC-1250", manufactured by Orientec Corporation), the gas barrier coating layer and the remaining part of the cut sample were stretched in opposite directions to each other so that the peeled gas barrier coating layer and the remaining part formed a T-shape with the unpeeled part, and peeled at a peeling speed of 300 mm / min, and the strength required for peeling (unit: N / 15 mm) was measured as the lamination strength. The results are shown in Table 1.

[0194] [Table 1]

[0195]

[0196] As shown in Table 1, it can be seen that the gas barrier laminates of Examples 1 to 7 have high lamination strength after retorting and low oxygen permeability after retorting and abuse. In contrast, it can be seen that the gas barrier laminates of Comparative Examples 1 to 3 have low lamination strength after retorting or high oxygen permeability after retorting and abuse.

[0197] In summary, it was confirmed that the gas barrier laminate of the present disclosure was excellent in lamination strength after retort treatment and was also excellent in oxygen barrier properties after retort treatment and abuse treatment.

[0198] Explanation of symbols

[0199] 1 ...substrate layer, 3 ...inorganic oxide layer, 4 ...gas barrier coating layer, 10 ...gas barrier laminate, 20 ...packaging film, 21 ...sealing layer, 30 ...packaging container, 40 ...packaging product.

Claims

1. A gas barrier laminate comprising, in order: a base layer containing a thermoplastic resin, an inorganic oxide layer, and a gas barrier coating layer, The gas barrier coating layer is a cured product of a composition for forming a gas barrier coating layer, The gas barrier coating layer-forming composition comprises: Water-soluble polymers, a first silicon compound consisting of at least one of a silane alkoxy compound represented by the following general formula (1) and a hydrolyzate thereof, and a second silicon compound composed of at least one of a silicon alkoxy compound represented by the following general formula (2) and a hydrolyzate thereof, When the second silicon compound is converted into R 2 In the case of Si(OH)3, the mass ratio of the water-soluble polymer to the total mass of the water-soluble polymer and the second silicon compound is 55 to 95 mass %, When the first silicon compound is converted into SiO2 and the second silicon compound is converted into R 2 In the case of Si(OH)3, the mass ratio of the first silicon compound in the total mass of the first silicon compound and the second silicon compound is greater than 0 mass % and less than 89 mass %, Si(OR 1 )4···(1) (R 2 Si(OR 3 )3) n ···(2) In the above general formulas (1) and (2), R 1 , R 3 represents an alkyl group or -C2H4OCH3, R 2 represents an organic functional group, and n represents an integer of 1 or greater.

2. The gas barrier laminate according to claim 1, wherein When the first silicon compound is converted into SiO2 and the second silicon compound is converted into R 2 In the case of Si(OH) 3 , the mass ratio of the first silicon compound in the total mass of the first silicon compound and the second silicon compound is 20 mass % or more and 89 mass % or less.

3. The gas barrier laminate according to claim 1 or 2, wherein When the second silicon compound is converted into R 2 In the case of Si(OH) 3 , the mass ratio of the water-soluble polymer in the total mass of the water-soluble polymer and the second silicon compound is 75 to 90 mass %.

4. The gas barrier laminate according to any one of claims 1 to 3, wherein The thermoplastic resin is a polyolefin resin.

5. The gas barrier laminate according to any one of claims 1 to 4, wherein The silane alkoxy compound constituting the second silicon compound is R 2 For NCO-R 4 -, said R 4 An alkylene group having an integer of 1 or more carbon atoms and a trimer 1,3,5-tris(3-trialkoxysilylalkyl)isocyanurate in which n is 3.

6. The gas barrier laminate according to any one of claims 1 to 4, wherein The silane alkoxy compound constituting the second silicon compound is R 2 It is 3-glycidoxypropyl, 3-glycidoxypropyltrialkoxysilane wherein n is 1.

7. The gas barrier laminate according to any one of claims 1 to 6, wherein An anchor coating layer is further provided between the substrate layer and the inorganic oxide layer. 8 . A packaging film comprising the gas barrier laminate according to claim 1 , and a sealant layer.

9. A packaging container comprising the packaging film according to claim 8. 10 . A packaged product comprising the packaging container according to claim 9 and a content filled in the packaging container.

Citation Information

Patent Citations

  • Barrier film, laminate, and packaging bag

    CN118265610A

  • Gas barrier laminate film

    CN1713983A