Polycarbonate resin, method for producing same, and polycarbonate resin composition

By introducing specific terminal groups into the polycarbonate resin and controlling its proportion, combining ester exchange and polycondensation reaction, the problems of volatile impurities residues and insufficient heat resistance in the aromatic polycarbonate resin are solved, and high temperature and high humidity are achieved Stability and low odor characteristics under conditions are suitable for food containers and other applications.

CN119013327AActive Publication Date: 2024-11-22MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202480002138.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-15
Filing Date
2024-03-15
Publication Date
2024-11-22
Estimated Expiration
2044-03-15

AI Technical Summary

Technical Problem

In the prior art, aromatic polycarbonate resin produced by melting method has high melt viscosity, making it difficult to completely remove volatile impurities, resulting in residual odor of molded products, and low heat resistance (humidity and heat stability), which limits its In applications such as food containers.

Method used

By setting the terminal group of the polycarbonate resin to a specific terminal group, such as methylphenoxy, the ratio is controlled to 0.024-4.0 mol%, and using specific catalysts and conditions in the transesterification reaction, further performing Hydrolysis and polycondensation reactions to reduce the amount of volatile impurities and improve moisture and heat stability.

Benefits of technology

It effectively reduces the amount of volatile impurities during the manufacturing process, improves the heat resistance and humidity stability of polycarbonate resin, inhibits the generation of odor of molded products, and is suitable for use under high temperature and high humidity conditions such as food containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013327A_ABST
    Figure CN119013327A_ABST
Patent Text Reader

Abstract

A polycarbonate resin having a terminal group represented by formula (1), the ratio of the terminal group represented by formula (1) to the total terminal group being 0.024-4.0 mol%. # imgabs0 # (In formula (1), X1 to X5 may be the same as or different from each other, and each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. In formula (1), at least one of X1-X5 represents an alkyl group having 1-3 carbon atoms. And * represents a bond to a polycarbonate resin chain).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polycarbonate resin having excellent heat resistance (wet heat stability) and reduced odor during melt molding or in the obtained molded product, and a method for producing the same. More specifically, the present invention relates to a polycarbonate resin that can be used for food containers and the like, and a method for producing the same. Background Art

[0002] Polycarbonate resins, particularly aromatic polycarbonate resins, are resins that are excellent in mechanical properties such as heat resistance and impact resistance, dimensional stability, and transparency, and are used in various applications.

[0003] Polycarbonate resins are produced by a melt method (ester exchange method) and a phosgene method (interfacial polymerization method), etc. Aromatic polycarbonate resins produced by a melt method are poor in water resistance (wet heat stability) because they are obtained by reacting an aromatic dihydroxy compound with a carbonic acid diester in a molten state.

[0004] As a method for improving the water resistance of an aromatic polycarbonate resin, there is a method of carrying out an ester exchange reaction in the presence of a specific catalyst (such as a nitrogen-containing basic compound) and further capping the hydroxyl terminals of the obtained polycarbonate resin with a specific compound (Patent Document 1).

[0005] In either the melt method or the phosgene method, the polycarbonate resin is produced as a crude polycarbonate resin (a polycarbonate resin composition containing impurities) containing volatile impurities such as unreacted raw materials, low molecular weight products, and reaction solvents. Examples of low molecular weight products include phenol in the melt method.

[0006] In the melt method, phenol generated in the transesterification reaction is distilled off under reduced pressure. In this case, due to the equilibrium relationship between the reaction liquid phase and the gas phase, phenol remains in the reaction liquid phase and is contained in the polycarbonate resin.

[0007] As a method for removing such volatile impurities, for example, the following method is known.

[0008] A method in which nitrogen and water are supplied to the extrusion kneading section of a melt extruder to perform a decompression treatment when an aromatic polycarbonate resin is melt-extruded and pelletized (Patent Documents 2 and 3);

[0009] Methods of adding saturated aliphatic hydrocarbons and aromatic hydrocarbons (Patent Documents 4 and 5);

[0010] A method of supplying carbon dioxide under pressure and performing a decompression treatment (Patent Document 6);

[0011] A method in which a polycarbonate resin and water are kneaded at 0.3 to 10 MPa using a multi-stage vented melt extruder and then subjected to a reduced pressure treatment (Patent Document 7).

[0012] Patent Document 8 describes a method of adding an aromatic polycarbonate or an oligomer thereof having a terminal group having a structure with a volume higher than that of a phenoxy group when producing an aromatic polycarbonate resin, with the improvement of heat resistance as a subject. However, no research is conducted on water resistance (wet heat stability) and residual volatile impurities.

[0013] Prior art literature

[0014] Patent Literature

[0015] Patent Document 1: Japanese Patent Application Laid-Open No. 2-175723

[0016] Patent Document 2: Japanese Patent Application Laid-Open No. 9-59367

[0017] Patent Document 3: Japanese Patent Application Laid-Open No. 9-59368

[0018] Patent Document 4: Japanese Patent Application Laid-Open No. 9-67433

[0019] Patent Document 5: Japanese Patent Application Laid-Open No. 9-157375

[0020] Patent Document 6: Japanese Patent Application Publication No. 2000-302879

[0021] Patent Document 7: Japanese Patent Application Publication No. 2001-31753

[0022] Patent Document 8: Japanese Patent No. 4267344 Summary of the invention

[0023] Problems to be solved by the invention

[0024] Aromatic polycarbonate resins produced by a melt process tend to have high melt viscosity, and therefore, it may be difficult to completely remove volatile impurities remaining with the produced aromatic polycarbonate resin.

[0025] In addition, aromatic polycarbonate resins generate odor during melt molding due to volatile impurities. As a result, the obtained molded products also retain odor. Therefore, their use in food containers and the like is sometimes limited.

[0026] Food containers and the like are often exposed to high temperature and high humidity conditions. Therefore, molded articles made of aromatic polycarbonate resins may suffer from defects such as whitening in a short period of time due to their low heat resistance (wet heat stability).

[0027] The object of the present invention is to provide a polycarbonate resin or a polycarbonate resin composition which can reduce the amount of volatile impurities that may be generated during production, has excellent heat resistance (wet heat stability), is unlikely to cause the problem of whitening even when exposed to high temperature and high humidity conditions, and has suppressed odor of the molded product obtained during melt molding.

[0028] Methods for solving problems

[0029] The present inventors have found that a polycarbonate resin meeting the above-mentioned purpose can be obtained by using a part of the terminal groups of a polycarbonate resin as specific terminal groups.

[0030] The gist of the present invention is as follows.

[0031] [1] A polycarbonate resin having a terminal group represented by the following formula (1), wherein the ratio of the terminal group represented by the following formula (1) to all terminal groups is 0.024 to 4.0 mol %.

[0032] [Chemistry 1]

[0033]

[0034] (In the above formula (1), X 1 ~X 5 may be the same or different, and each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 1 ~X 5 At least one of them is an alkyl group having 1 to 3 carbon atoms. * represents a bond with the polycarbonate resin chain.

[0035] [2] The polycarbonate resin according to [1], wherein the ratio of the terminal groups represented by the formula (1) relative to all terminal groups of the polycarbonate resin is 0.024 to 2.0 mol %.

[0036] [3] The polycarbonate resin according to [2], wherein the ratio of the terminal groups represented by the formula (1) to all terminal groups of the polycarbonate resin is 0.030 to 2.0 mol %.

[0037] [4] The polycarbonate resin according to any one of [1] to [3], wherein the terminal group represented by the formula (1) is a methylphenoxy group.

[0038] [5] The polycarbonate resin according to any one of [1] to [4], which is a transesterification product of a dihydroxy compound and a carbonic acid diester, wherein the dihydroxy compound includes at least one selected from the group consisting of aromatic dihydroxy compounds, aliphatic dihydroxy compounds and alicyclic dihydroxy compounds.

[0039] [6] The polycarbonate resin according to [5], wherein the aromatic dihydroxy compound is bisphenol A.

[0040] [7] The polycarbonate resin according to any one of [1] to [6], wherein the total amount of the compounds represented by the following formulae (A) to (E) in the hydrolyzate obtained by hydrolyzing the polycarbonate resin is 500 to 6,000 ppm by mass based on the polycarbonate resin.

[0041] [Chemistry 2]

[0042]

[0043] (R in the above formula (A) 1 , R in formula (B) 2 , R in formula (C) 3 , R 4 and R in formula (D) 5 , R 6 Each independently represents a hydrogen atom or a methyl group. )

[0044] [8] The polycarbonate resin according to [7], wherein the total amount of the compounds represented by the formulae (A) to (E) in the hydrolyzate obtained by hydrolyzing the polycarbonate resin is 2,000 to 6,000 ppm by mass based on the polycarbonate resin.

[0045] [9] The polycarbonate resin according to [8], wherein the total amount of the compounds represented by the formulae (A) to (E) obtained by hydrolyzing the polycarbonate resin is 3,000 to 6,000 ppm by mass based on the polycarbonate resin.

[0046]

[10] The polycarbonate resin according to any one of [1] to [9], wherein the terminal hydroxyl concentration of the polycarbonate resin is 1000 ppm by mass or less.

[0047]

[11] The polycarbonate resin according to

[10] , wherein the terminal hydroxyl group concentration of the polycarbonate resin is 700 ppm by mass or less.

[0048]

[12] The polycarbonate resin according to any one of [1] to

[11] , wherein the viscosity average molecular weight of the polycarbonate resin is 14,000 to 30,000.

[0049]

[13] The polycarbonate resin according to any one of [1] to

[12] , wherein the total amount of the compound represented by the following formula (2) in the hydrolyzate obtained by hydrolyzing the polycarbonate resin is 4 to 1,500 ppm by mass relative to the polycarbonate resin.

[0050] [Chemistry 3]

[0051]

[0052] (In the above formula (2), X 1 ~X 5 Respectively with X in the above formula (1) 1 ~X 5 Synonymous.)

[0053]

[14] The polycarbonate resin according to any one of [1] to

[13] , wherein the polycarbonate resin is molded under the following molding condition I, and the molded body has a Δ haze of 4.3 or less after 100 hours at 120°C under saturated steam.

[0054] (Forming condition I)

[0055] The polycarbonate resin pellets were dried at 120° C. for 4 hours and then injection molded using an injection molding machine at a cylinder temperature of 350° C. and a mold temperature of 140° C. to obtain a plate-shaped molded body having a thickness of 3 mm, a length of 25 mm, and a width of 25 mm.

[0056]

[15] A polycarbonate resin composition comprising the polycarbonate resin according to any one of [1] to

[14] .

[0057]

[16] The polycarbonate resin composition according to

[15] , wherein the content of the aromatic monohydroxy compound in the polycarbonate resin composition is 20 ppm by mass or less.

[0058]

[17] A method for producing a polycarbonate resin, comprising: a reaction step of obtaining the polycarbonate resin described in any one of [1] to

[14] by subjecting a dihydroxy compound to an ester exchange reaction with a carbonic acid diester,

[0059] The above-mentioned carbonic acid diester includes a carbonic acid diester represented by the following formula (3).

[0060] [Chemistry 4]

[0061]

[0062] (In the above formula (3), X 1A ~X 5A and X 1B ~X 5B may be the same or different, and each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 1A ~X 5A and X 1B ~X 5BAt least one of them is an alkyl group having 1 to 3 carbon atoms.

[0063]

[18] The method for producing a polycarbonate resin according to

[17] , wherein the carbonic acid diester further comprises diphenyl carbonate, and the ratio of the amount of the carbonic acid diester represented by the formula (3) to the amount of the diphenyl carbonate is 80 to 35,000 ppm by mass.

[0064]

[19] The method for producing a polycarbonate resin according to

[17] , wherein the carbonic acid diester represented by the formula (3) is methylphenylphenyl carbonate.

[0065]

[20] The method for producing a polycarbonate resin according to any one of

[17] to

[19] , wherein the dihydroxy compound contains at least one selected from the group consisting of aromatic dihydroxy compounds, aliphatic dihydroxy compounds and alicyclic dihydroxy compounds.

[0066]

[21] The method for producing a polycarbonate resin according to

[20] , wherein the dihydroxy compound is bisphenol A.

[0067]

[22] The method for producing a polycarbonate resin according to any one of

[17] to

[21] , further comprising: after the reaction step, a step of devolatilizing the polycarbonate resin using a twin-screw extruder with a vent.

[0068]

[23] The method for producing a polycarbonate resin according to any one of

[17] to

[22] , wherein in the reaction step,

[0069] The above reaction treatment is carried out in the presence of an ester exchange catalyst.

[0070] After the reaction treatment, a catalyst deactivation treatment is further performed by adding 5 to 15 molar equivalents of a catalyst deactivator based on 1 mole of the transesterification catalyst.

[0071]

[24] A hollow container which is a blow-molded article of the polycarbonate resin according to any one of [1] to

[14] .

[0072]

[25] A hollow container which is a blow-molded product of the polycarbonate resin composition according to

[15] or

[16] .

[0073]

[26] The hollow container according to

[24] , which is a dairy product bottle, a soft drink bottle or a water bottle.

[0074]

[27] A sheet which is a molded product of the polycarbonate resin according to any one of [1] to

[14] .

[0075]

[28] A sheet which is a molded product of the polycarbonate resin composition according to

[15] or

[16] .

[0076] Effects of the Invention

[0077] The polycarbonate resin of the present invention can reduce the amount of volatile impurities that may be generated during production, has excellent heat resistance (wet heat stability), and is unlikely to cause whitening problems even when exposed to high temperature and high humidity conditions. In addition, the odor of the molded product obtained during melt molding can also be suppressed.

[0078] The polycarbonate resin of the present invention having excellent heat resistance (wet heat stability) and suppressed odor can be preferably used in hollow containers such as food containers. BRIEF DESCRIPTION OF THE DRAWINGS

[0079] [ Figure 1 ] Figure 1 This is a system diagram showing an example of the flow of transesterification treatment and polycondensation reaction treatment in the production of the polycarbonate resin according to one embodiment of the present invention. DETAILED DESCRIPTION

[0080] The embodiments of the present invention are described in detail below, but each configuration and combination thereof in each embodiment are examples, and addition, omission, substitution, and other changes of configurations may be appropriately made without departing from the gist of the present disclosure. This specification is not limited to the embodiments.

[0081] In addition, various aspects disclosed in this specification may be combined with any other features disclosed in this specification.

[0082] In addition, in this specification, "X to Y" indicating a range means "more than X and less than Y". In addition, when a numerical range represented by "X to Y" or "more than X and less than Y" is described in stages (for example, in a preferred order), the upper limit and lower limit of each numerical range can be arbitrarily combined.

[0083] In the present specification, the phrase “one or more selected from the group consisting of X, Y, and Z” means any one of X, Y, Z, a combination of X and Y, a combination of X and Z, a combination of Y and Z, or a combination of X, Y, and Z.

[0084] [Polycarbonate resin]

[0085] A polycarbonate resin according to one embodiment of the present invention (hereinafter also simply referred to as "polycarbonate resin") is characterized by having a terminal group represented by the following formula (1), wherein the ratio of the terminal group represented by the following formula (1) to all terminal groups is 0.024 to 4.0 mol %.

[0086] [Chemistry 5]

[0087]

[0088] In the above formula (1), X 1 ~X 5 may be the same or different, and each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 1 ~X 5 At least one of them is an alkyl group having 1 to 3 carbon atoms. * represents a bond with a polycarbonate resin chain.

[0089] Hereinafter, the terminal group represented by the above formula (1) may be referred to as "terminal group (1)". In addition, the ratio (molar ratio) of the terminal group (1) to all terminal groups of the polycarbonate resin may be referred to as "terminal group (1) / total terminal group ratio".

[0090] <Terminal group (1)>

[0091] In the above formula (1) representing the terminal group (1), X 1 ~X 5 may be the same or different, and each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 1 ~X 5 At least one of the groups is an alkyl group having 1 to 3 carbon atoms.

[0092] As X 1 ~X 5 Examples of the alkyl group include a methyl group, an ethyl group, and a propyl group.

[0093] From the viewpoint of the color tone of the polycarbonate resin, regarding the terminal group (1), in the above formula (1), it is preferred that X 1 ~X 5 At least one of them is an alkyl group having 1 to 3 carbon atoms, and more preferably X 1 ~X 5 1 to 2 of them are alkyl groups having 1 to 3 carbon atoms, and X other than alkyl groups 1 ~X 5 The terminal group (1) is preferably a methylphenoxy group, and particularly preferably an o-methylphenoxy group.

[0094] The polycarbonate resin may have one terminal group (1) or may have X 1 ~X 5 Two or more different terminal groups (1).

[0095] <Terminal group (1) / total terminal group ratio>

[0096] The ratio of the terminal group represented by the above formula (1) to 100 mol% of all the terminal groups of the polycarbonate resin (terminal group (1) / total terminal group ratio) may be 4.5 mol% or less, preferably 4.0 mol% or less, more preferably 2.0 mol% or less, and further preferably 1.5 mol% or less. If the terminal group (1) / total terminal group ratio exceeds 5 mol%, the polycarbonate resin may turn yellow, and the heat resistance (wet heat stability) may deteriorate. On the other hand, the terminal group (1) / total terminal group ratio of the polycarbonate resin is preferably 0.024 mol% or more, more preferably 0.03 mol% or more, further preferably 0.040 mol% or more, and particularly preferably 0.060 mol% or more. As described above, the upper and lower limits of the numerical range in this specification may be arbitrarily combined, and as long as it is the ratio, the upper and lower limits may be arbitrarily combined, such as 0.024 to 4.0 mol%, 0.024 to 2.0 mol%, or 0.03 to 2.0 mol%. When the terminal group (1) / total terminal group ratio is less than 0.021 mol%, the amount of volatile impurities that may be generated during production increases, the heat resistance (wet heat stability) deteriorates, and there is a possibility of causing odor problems.

[0097] The method for controlling the terminal group (1) / total terminal group ratio of the polycarbonate resin to fall within the above range is not particularly limited. When the polycarbonate resin is produced by an ester exchange reaction between a dihydroxy compound and a carbonic acid diester, for example, the following method may be used.

[0098] (I) As the carbonic acid diester, a carbonic acid diester represented by the following formula (3) (hereinafter sometimes referred to as "carbonic acid diester (3)") is used, and the amount of carbonic acid diester (3) in the raw carbonic acid diester is controlled. Alternatively, carbonic acid diester (3) is added to the raw carbonic acid diester in a desired amount.

[0099] [Chemistry 6]

[0100]

[0101] In the above formula (3), X 1A ~X 5A and X 1B ~X 5B may be the same or different, and each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 1A ~X 5A and X 1B ~X 5B At least one of the groups is an alkyl group having 1 to 3 carbon atoms.

[0102] In formula (3), X 1A ~X 5A and X1B ~X 5B Respectively with X in the above formula (1) 1 ~X 5 The same applies to the preferred aspects.

[0103] (II) Controlling the content of the compound represented by the following formula (2) (hereinafter sometimes referred to as "compound (2)") contained in the polycarbonate resin raw material, particularly the raw material dihydroxy compound. Alternatively, the compound (2) is added to the polycarbonate resin raw material in a desired amount.

[0104] [Chemistry 7]

[0105]

[0106] In the above formula (2), X 1 ~X 5 Respectively with X in the above formula (1) 1 ~X 5 The same applies to the preferred aspects.

[0107] The amount of the terminal group (1) in the polycarbonate resin can be calculated from the amount of the compound (2) in the hydrolyzate obtained by hydrolyzing the polycarbonate resin as shown in Example 1 described later, or can be substantially calculated from the amount of the compound (2) measured by hydrolyzing the polycarbonate resin. When the amount of the terminal group (1) cannot be calculated from the amount of the compound (2) in the hydrolyzate obtained by hydrolyzing the polycarbonate resin, the amount of the structural unit derived from the compound (2) can be measured by directly analyzing the polycarbonate resin by NMR.

[0108] The specific measurement and calculation method of the terminal group (1) / total terminal groups ratio is described in Example 1 below.

[0109] <Amount of specific by-products in hydrolyzate of polycarbonate resin>

[0110] The total amount of the compounds represented by (A) to (E) below (hereinafter, these compounds may be referred to as “specific by-products”) in the hydrolyzate obtained by hydrolyzing the polycarbonate resin (hereinafter, sometimes referred to as “specific by-product amount”) is preferably 500 to 6,000 ppm by mass based on the polycarbonate resin.

[0111] [Chemistry 8]

[0112]

[0113] In the above formula (A), R 1 , R in formula (B) 2 , R in formula (C)3 and R 4 And R in formula (D) 5 and R 6 Each independently represents a hydrogen atom or a methyl group.

[0114] If the amount of specific by-products in the hydrolyzate obtained by hydrolyzing the polycarbonate resin is less than 6,000 mass ppm, it is easy to suppress the generation of gel-like substances, and when the polycarbonate resin is formed, it is not easy to observe foreign matter in the molded product and become a poor appearance. From this viewpoint, the amount of the specific by-product is more preferably less than 5,000 mass ppm. On the other hand, the total amount of the specific by-product is preferably more than 500 mass ppm, more preferably more than 1,000 mass ppm, further preferably more than 1,500 mass ppm, further preferably more than 2000 ppm, particularly preferably more than 2500 ppm, particularly preferably more than 3000 ppm, and most preferably more than 3500 ppm. If you want to set the amount of specific by-products to less than 500 mass ppm, the polymerization activity becomes low, and a long reaction time is required. As a result, the color tone of the polycarbonate resin is likely to deteriorate.

[0115] As a method for controlling the amount of specific byproducts in the hydrolyzate obtained by hydrolyzing the polycarbonate resin within the above-mentioned preferred range, for example, there can be cited: a method of adjusting the catalyst amount of the transesterification catalyst, a method of adjusting the temperature (internal temperature) of the final reactor, a method of adjusting the reaction time in the final reactor, or a method of adjusting the terminal hydroxyl concentration of the polycarbonate resin. That is, the generation reaction of specific byproducts can be suppressed by reducing the catalyst amount of the transesterification catalyst, the temperature (internal temperature) of the final reactor, or the reaction time in the final reactor, and the amount of specific byproducts in the hydrolyzate obtained by hydrolyzing the polycarbonate resin can be reduced. If the terminal hydroxyl concentration of the polycarbonate resin is too low, the rate of the transesterification reaction decreases, resulting in an increase in the temperature (internal temperature) of the final reactor and the reaction time in the final reactor, and the amount of specific byproducts in the hydrolyzate obtained by hydrolyzing the polycarbonate resin will increase. In particular, the catalyst amount of the transesterification catalyst, the temperature (internal temperature) of the final reactor, or the terminal hydroxyl concentration of the polycarbonate resin is very important, and by selecting from each preferred range described later, the amount of specific byproducts can be controlled within the above-mentioned preferred range.

[0116] The amount of specific by-products in the hydrolyzate obtained by hydrolyzing the polycarbonate resin is measured by the method described in Example 1 described later.

[0117] <Content of Compound (2) in Hydrolyzate of Polycarbonate Resin>

[0118] The content (total amount) of the compound (2) in the hydrolyzate obtained by hydrolyzing the polycarbonate resin is preferably 1,500 mass ppm or less, more preferably 1,100 mass ppm or less, and further preferably 300 mass ppm or less, relative to the polycarbonate resin. If the content of the compound (2) in the hydrolyzate is below the above upper limit, yellowing of the polycarbonate resin can be suppressed, and the heat resistance (wet heat stability) is also improved. The lower limit of the content (total amount) of the compound (2) in the hydrolyzate obtained by hydrolyzing the polycarbonate resin is preferably 4 mass ppm or more, more preferably 6 mass ppm or more, and further preferably 10 mass ppm or more, relative to the polycarbonate resin. If the content of the compound (2) in the hydrolyzate is above the above lower limit, the amount of volatile impurities that may be generated during the production of the polycarbonate resin can be reduced, and the heat resistance (wet heat stability) is improved.

[0119] Examples of methods for controlling the content of the compound (2) in the hydrolyzate of the polycarbonate resin include a method of controlling the amount of the above-mentioned diester carbonate (3) contained in the diester carbonate used for producing the polycarbonate resin, and a method of separately adding the diester carbonate (3) as a raw material for the transesterification reaction.

[0120] The method for hydrolyzing the polycarbonate resin and the method for measuring the content of the compound (2) in the hydrolyzate of the polycarbonate resin are described in Example 1 below.

[0121] <Terminal hydroxyl concentration of polycarbonate resin>

[0122] The terminal hydroxyl concentration of the polycarbonate resin is not particularly limited, preferably 1000 mass ppm or less, more preferably 800 mass ppm or less, further preferably 700 mass ppm or less, particularly preferably 600 mass ppm or less, especially particularly preferably 500 mass ppm or less, and most preferably 450 mass ppm or less. If the terminal hydroxyl concentration is below the above upper limit, the amount of volatile impurities such as unreacted raw materials or low molecular weight products that may be produced during manufacture can be reduced, and the odor during melt molding and the odor of the obtained molded product can be suppressed. In addition, if the terminal hydroxyl concentration is below the above upper limit, the molecular weight reduction when the obtained molded product is exposed to high temperature and high humidity can be suppressed, and the molded product whitening or easy rupture due to the reduction in molecular weight can be suppressed. On the other hand, the lower limit of the terminal hydroxyl concentration of the polycarbonate resin is generally 100 mass ppm or more, preferably 200 mass ppm or more. If the terminal hydroxyl concentration is above the above lower limit, the transesterification reaction and polycondensation reaction during the manufacture of the polycarbonate resin will not slow down, and the polycarbonate resin of the desired viscosity average molecular weight can be obtained without being set to high temperature, high vacuum and high residence time. Therefore, yellowing of the polycarbonate resin can be suppressed.

[0123] As a method for controlling the terminal hydroxyl concentration of the polycarbonate resin within the above-mentioned preferred range, the following method can be cited: In the manufacture of the polycarbonate resin, as described later, the mixing ratio of the diaryl carbonate supplied to the transesterification reaction and the aromatic dihydroxy compound is adjusted. Specifically, it is preferred to use more than 1.03 times (molar ratio) of the diaryl carbonate relative to the aromatic dihydroxy compound, and more preferably use more than 1.04 times (molar ratio). By using diaryl carbonate above the above lower limit, the terminal hydroxyl concentration of the obtained aromatic polycarbonate resin can be suppressed to below the above upper limit. The upper limit of the amount of diaryl carbonate used is preferably less than 1.30 times (molar ratio) relative to the aromatic dihydroxy compound, and more preferably less than 1.20 times (molar ratio).

[0124] The terminal hydroxyl concentration of the aromatic polycarbonate resin is determined not only by the mixing ratio of the diaryl carbonate and the aromatic dihydroxy compound but also by the device shape and operating conditions. Therefore, it is preferred to measure the terminal hydroxyl concentration of the aromatic polycarbonate resin actually obtained and appropriately adjust the mixing ratio of the diaryl carbonate and the aromatic dihydroxy compound based on the result.

[0125] The terminal hydroxyl group concentration of the polycarbonate resin is measured by the method described in Example 1 described later.

[0126] The method for controlling the terminal hydroxyl group concentration of the polycarbonate resin will be described later.

[0127] <Viscosity average molecular weight of polycarbonate resin>

[0128] In the manufacturing process of polycarbonate resin, the polycarbonate resin is preferably not viscous for the purpose of reducing the amount of the above-mentioned volatile impurities. From this point of view, the viscosity average molecular weight of the polycarbonate resin that may be produced during the manufacturing is preferably 30,000 or less, more preferably 28,000 or less, and further preferably 27,000 or less. If the viscosity average molecular weight is below the above upper limit, the volatilization of volatile impurities in the manufacturing process of the polycarbonate resin becomes easy, and it is easy to reduce the amount of volatile impurities that may be produced during the manufacturing. In addition, if the viscosity average molecular weight is below the above upper limit, the cross-linking reaction can be suppressed, and the generation of gel-like substances caused by the cross-linking reaction can be suppressed, so that the gel-like substances can be suppressed as foreign matter in the molded product and become poor in appearance. On the other hand, the lower limit of the viscosity average molecular weight of the polycarbonate resin is usually 14,000 or more, preferably 15,000 or more, and more preferably 16,000 or more. If the viscosity average molecular weight is above the above lower limit, the obtained molded product can be suppressed from becoming brittle or easily broken.

[0129] The viscosity average molecular weight of the polycarbonate resin is measured by the method described in Example 1 described later.

[0130] <ΔHaze of polycarbonate resin after 100 hours at 120°C and saturated water vapor>

[0131] The Δ haze of a molded article obtained by molding a polycarbonate resin under the following molding condition I at 120°C under saturated water vapor after 100 hours is not particularly limited, but is more preferably 4.3 or less, further preferably 4.2 or less, and particularly preferably 4.1 or less. The lower limit of the Δ haze is not particularly limited as long as it is 0 or more. If the Δ haze is below the upper limit of the above range, it means that the molecular weight of the polymer is suppressed from decreasing, and the whitening of the plate is suppressed.

[0132] (Forming condition I)

[0133] The polycarbonate resin pellets were dried at 120° C. for 4 hours and then injection molded using an injection molding machine at a cylinder temperature of 350° C. and a mold temperature of 140° C. to obtain a plate-shaped molded body having a thickness of 3 mm, a length of 25 mm, and a width of 25 mm.

[0134] The Δ haze of the polycarbonate resin is measured by the method described in Example 1 described later.

[0135] [Method for producing polycarbonate resin]

[0136] The method for producing the polycarbonate resin is not particularly limited, and the polycarbonate resin can be produced by the following method as one example.

[0137] The polycarbonate resin is preferably a product of an ester exchange reaction between a dihydroxy compound and a carbonic acid diester, and more preferably can be produced by a method comprising: subjecting a hydroxy compound to an ester exchange reaction with a carbonic acid diester including the carbonic acid diester (3) to obtain the polycarbonate resin.

[0138] In particular, as the carbonic acid diester, diaryl carbonate is preferably used, and as the dihydroxy compound, at least one selected from the group consisting of aromatic dihydroxy compounds, aliphatic dihydroxy compounds and alicyclic dihydroxy compounds is preferably used. It should be noted that in this specification, the expression "as A, at least one selected from the group consisting of B and C is used" is sometimes also expressed as "A contains at least one selected from the group consisting of B and C".

[0139] That is, the polycarbonate resin is preferably an aromatic polycarbonate resin produced by an ester exchange reaction between a diaryl carbonate and an aromatic dihydroxy compound.

[0140] It should be noted that the above-mentioned reaction step may include not only the transesterification reaction treatment but also the polycondensation reaction treatment described later.

[0141] Hereinafter, a method for producing an aromatic polycarbonate resin using a diaryl carbonate as a carbonic acid diester and an aromatic dihydroxy compound as a dihydroxy compound will be described. The method for producing a polycarbonate resin is not limited to the following method.

[0142] Aromatic polycarbonate resins are generally produced by mixing an aromatic dihydroxy compound and a diaryl carbonate as raw materials to prepare a raw material mixture, and subjecting the raw material mixture to an ester exchange reaction (ester exchange reaction treatment) and a polycondensation reaction (polycondensation reaction treatment) in a polycondensation reaction apparatus in the presence of an ester exchange catalyst.

[0143] The reaction mode of the polycondensation treatment can be intermittent, continuous, or a combination thereof. In the present embodiment, the raw material preparation step and the reaction step are preferably carried out continuously, and after the transesterification reaction treatment and the polycondensation treatment, the steps of removing the unreacted raw materials and reaction byproducts in the polymerization reaction liquid after stopping the reaction, the step of adding a heat stabilizer, a release agent or a colorant, etc., the step of forming particles of a predetermined particle size as required, etc., are performed to produce the aromatic polycarbonate resin.

[0144] <Diaryl carbonate>

[0145] Examples of the diaryl carbonate include diphenyl carbonate (DPC) and substituted diphenyl carbonates such as ditolyl carbonate. These diaryl carbonates may be used alone or in combination of two or more.

[0146] The above-mentioned diaryl carbonate can be preferably substituted with dicarboxylic acid or dicarboxylic acid ester in an amount of preferably less than 50 mol %, more preferably less than 30 mol %. Representative dicarboxylic acids or dicarboxylic acid esters include terephthalic acid, isophthalic acid, diphenyl terephthalate, or diphenyl isophthalate. When diaryl carbonate is substituted with dicarboxylic acid or dicarboxylic acid ester, polyester carbonate can be obtained.

[0147] The carbonic acid diester (3) may be contained in the diaryl carbonate, or may be separately added as a raw material for the transesterification reaction.

[0148] The method for changing the content of the carbonic acid diester (3) contained in the diaryl carbonate is not particularly limited. For example, the content of the carbonic acid diester (3) in the diaryl carbonate can be changed by changing the content of the compound (2) in the monohydroxyaryl compound as the raw material of the diaryl carbonate.

[0149] When diphenyl carbonate is used as the raw material diaryl carbonate, the ratio of the amount of carbonate diester (3) to the amount of diphenyl carbonate is preferably 35,000 mass ppm or less, more preferably 20,000 mass ppm or less, and further preferably 10,000 mass ppm or less. If the ratio of carbonate diester (3) to diphenyl carbonate is below the above upper limit, yellowing of the obtained polycarbonate resin can be suppressed, and heat resistance (wet heat stability) becomes good. The lower limit of the ratio of carbonate diester (3) to diphenyl carbonate is preferably 80 mass ppm or more, more preferably 200 weight ppm or more, more preferably 400 mass ppm or more, and further preferably 550 mass ppm or more. If the ratio of carbonate diester (3) to diphenyl carbonate is above the above lower limit, the amount of volatile impurities that may be generated during manufacturing can be reduced, and heat resistance (wet heat stability) becomes good.

[0150] As the carbonic acid diester (3), methylphenylphenyl carbonate is particularly preferred, and o-methylphenylphenyl carbonate is most preferred.

[0151] <Dihydroxy compounds>

[0152] As the dihydroxy compound, an aromatic dihydroxy compound, an aliphatic dihydroxy compound, or an alicyclic dihydroxy compound having an aromatic compound having two hydroxyl groups in the molecule can be cited, and an aromatic dihydroxy compound is preferred. Among the aromatic dihydroxy compounds, an aromatic dihydroxy compound having one or more aromatic rings in the molecule and two hydroxyl groups respectively bonded to the aromatic rings is preferably used.

[0153] Specific examples of the aromatic dihydroxy compound include bisphenols such as bis(4-hydroxydiphenyl)methane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, 4,4-bis(4-hydroxyphenyl)heptane, or 1,1-bis(4-hydroxyphenyl)cyclohexane; biphenols such as 4,4'-dihydroxybiphenyl or 3,3',5,5'-tetramethyl-4,4'-dihydroxybiphenyl; or bis(4-hydroxyphenyl)sulfone, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)ether, or bis(4-hydroxyphenyl)ketone. Among these, 2,2-bis(4-hydroxyphenyl)propane (ie, bisphenol A) is preferred. These aromatic dihydroxy compounds may be used alone or in combination of two or more.

[0154] Specific examples of the alicyclic dihydroxy compound include 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, pentacyclopentadecanedimethanol, 2,6-decahydronaphthalenedimethanol, 1,5-decahydronaphthalenedimethanol, 2,3-decahydronaphthalenedimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol, 1,3-adamantanedimethanol, isosorbide, isomannide, isoidol, oidide), 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane (common name: spirodiol), 3,9-bis(1,1-diethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane, 3,9-bis(1,1-dipropyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane, or dioxanediol, etc.

[0155] <Transesterification Catalyst>

[0156] In the transesterification reaction, a transesterification catalyst can be used. As the transesterification catalyst, the catalyst used when the polycarbonate resin is manufactured by the transesterification method can be generally cited, without particular limitation. Generally, for example, compounds of elements (excluding hydrogen) of Group 1 of the periodic table (hereinafter referred to as "Group 1"), compounds of elements of Group 2 of the periodic table (hereinafter referred to as "Group 2"), basic compounds such as basic boron compounds, basic phosphorus compounds, or basic ammonium compounds or amine compounds can be cited.

[0157] As compounds of Group 1 elements (excluding hydrogen), inorganic compounds such as hydroxides, carbonates, or bicarbonates of Group 1 elements (excluding hydrogen); organic compounds such as salts of Group 1 elements (excluding hydrogen) with alcohols, phenols, or organic carboxylic acids, etc., can be cited. As Group 1 elements (excluding hydrogen), for example, lithium, sodium, potassium, rubidium, or cesium can be cited. Among these compounds of Group 1 elements (excluding hydrogen), cesium compounds are preferred, and cesium carbonate, cesium bicarbonate, or cesium hydroxide is particularly preferred.

[0158] Examples of compounds of Group 2 elements include inorganic compounds such as hydroxides or carbonates of beryllium, magnesium, calcium, strontium, or barium; and salts of Group 2 elements with alcohols, phenols, or organic carboxylic acids.

[0159] Examples of the basic boron compound include sodium salts, potassium salts, lithium salts, calcium salts, magnesium salts, barium salts, and strontium salts of boron compounds. Examples of the boron compound include tetramethylboron, tetraethylboron, tetrapropylboron, tetrabutylboron, trimethylethylboron, trimethylbenzylboron, trimethylphenylboron, triethylmethylboron, triethylbenzylboron, triethylphenylboron, tributylbenzylboron, tributylphenylboron, tetraphenylboron, benzyltriphenylboron, methyltriphenylboron, and butyltriphenylboron.

[0160] Examples of the basic phosphorus compound include trivalent phosphorus compounds such as triethylphosphine, tri-n-propylphosphine, triisopropylphosphine, tri-n-butylphosphine, triphenylphosphine, and tributylphosphine, and quaternary phosphonium salts derived from these compounds.

[0161] Examples of the basic ammonium compound include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, trimethylethylammonium hydroxide, trimethylbenzylammonium hydroxide, trimethylphenylammonium hydroxide, triethylmethylammonium hydroxide, triethylbenzylammonium hydroxide, triethylphenylammonium hydroxide, tributylbenzylammonium hydroxide, tributylphenylammonium hydroxide, tetraphenylammonium hydroxide, benzyltriphenylammonium hydroxide, methyltriphenylammonium hydroxide, and butyltriphenylammonium hydroxide.

[0162] Examples of the amine compound include 4-aminopyridine, 2-aminopyridine, N,N-dimethyl-4-aminopyridine, 4-diethylaminopyridine, 2-hydroxypyridine, 2-methoxypyridine, 4-methoxypyridine, 2-dimethylaminoimidazole, 2-methoxyimidazole, imidazole, 2-mercaptoimidazole, 2-methylimidazole, and aminoquinoline.

[0163] Among these transesterification catalysts, at least one compound selected from the group consisting of compounds of Group 1 elements (excluding hydrogen) and compounds of Group 2 elements is practically preferred. These transesterification catalysts may be used alone or in combination of two or more.

[0164] The amount of the transesterification catalyst used is preferably 1×10 -9 ~1×10 -1 mole, more preferably 1×10 -7 ~1×10 -3 mole, more preferably 1×10 -7 ~1×10 -5 Moore.

[0165] The transesterification catalyst is sometimes used as an aqueous solution. In this case, the concentration of the catalyst aqueous solution is not particularly limited and can be adjusted to any concentration according to the solubility of the catalyst in water. Other solvents such as acetone, alcohol, toluene or phenol may also be selected instead of water.

[0166] The properties of water used for dissolving the transesterification catalyst are not particularly limited as long as the types and concentrations of impurities contained are constant. Generally, distilled water or deionized water is preferably used.

[0167] <Mixing ratio of diaryl carbonate and aromatic dihydroxy compound>

[0168] As a method for manufacturing an aromatic polycarbonate resin having the above-mentioned suitable terminal hydroxyl concentration, a method for adjusting the mixing ratio of the diaryl carbonate and the aromatic dihydroxy compound provided for the transesterification reaction can be cited. Specifically, it is preferred to use a diaryl carbonate of 1.03 times (molar ratio) or more relative to the aromatic dihydroxy compound, and more preferably to use a 1.04 times (molar ratio) or more. By using a diaryl carbonate above the above lower limit, the terminal hydroxyl concentration of the obtained aromatic polycarbonate resin can be suppressed to below the above upper limit. The upper limit of the amount of diaryl carbonate used is preferably 1.30 times (molar ratio) or less relative to the aromatic dihydroxy compound, and more preferably 1.20 times (molar ratio) or less. By using a diaryl carbonate below the above upper limit, the reaction rate of the transesterification can be increased, and an aromatic polycarbonate resin with a desired molecular weight can be efficiently manufactured. In addition, the amount of diaryl carbonate that may remain during the manufacture of the aromatic polycarbonate resin can be reduced, and the odor during the molding process and the molding product can be suppressed. However, the terminal hydroxyl concentration of the aromatic polycarbonate resin is determined not only by the mixing ratio of the diaryl carbonate and the aromatic dihydroxy compound but also by the device shape and operating conditions. Therefore, it is preferred to measure the terminal hydroxyl concentration of the aromatic polycarbonate resin actually obtained and appropriately adjust the mixing ratio of the diaryl carbonate and the aromatic dihydroxy compound based on the result.

[0169] <Polycondensation reaction treatment>

[0170] The raw material mixture prepared by mixing the diaryl carbonate and the aromatic dihydroxy compound is transported in a molten state to Figure 1 A polycondensation reaction apparatus using a plurality of reactors connected in series as shown above is used for polycondensation reaction treatment. The polycondensation reaction in this step is usually carried out continuously in two or more stages, preferably in 3 to 7 stages. Specific reaction conditions include, for example, temperature: 150 to 320°C, pressure: normal pressure to 0.01 Torr (1.3 Pa), and average residence time: in the range of 5 to 150 minutes.

[0171] In the multi-stage method, in order to more effectively remove the aromatic monohydroxy compounds such as phenol produced as a by-product in the polycondensation reaction apparatus from the system, the reaction conditions are set to be higher in stages and higher in vacuum. In order to prevent the quality of the obtained aromatic polycarbonate resin, such as the color tone, from being reduced, it is preferably set to be as low as possible and the residence time is as short as possible.

[0172] When the polycondensation treatment is performed in a multi-stage manner, a plurality of reactors including a vertical reactor are usually installed to increase the average molecular weight of the aromatic polycarbonate resin. Usually, 3 to 6 reactors, preferably 4 to 5 reactors are installed.

[0173] As an example, in Figure 1 In the process, three vertical reactors 11a to 11c and one horizontal reactor 11d are connected in series for use. The melt of the raw material mixture A is supplied to the initial vertical reactor 11a, and the transesterification reaction is started in the presence of the above-mentioned transesterification catalyst. Then, it is sent to the vertical reactor 11b, the vertical reactor 11c, and the horizontal reactor 11d in sequence to carry out the transesterification reaction. At this time, phenol is produced as a by-product. The by-product phenol is liquefied in the heat exchanger (condenser) 12 and sent to the phenol tank 13. The phenol in the phenol tank 13 is properly treated and reused as a raw material for aromatic dihydroxy compounds, diaryl carbonates, etc.

[0174] As the last reactor of a set of polycondensation reaction devices, a horizontal reactor 11d with a horizontal (horizontal) rotating shaft of a stirring blade is used. This is because the viscosity increases as the transesterification reaction proceeds, so the viscosity in the reactor becomes high in the final stage, which makes stirring at the high viscosity easier.

[0175] The aromatic polycarbonate resin B obtained by the polycondensation treatment is discharged from the horizontal reactor 11d, devolatilized, and then cooled.

[0176] In order to remove the above-mentioned volatile impurities as much as possible, it is preferred to set the temperature at a high temperature and a low pressure in the last reactor 11d. Specifically, the temperature is preferably 275°C or higher, and more preferably 280°C or higher. If the temperature is lower than 275°C, the residual amount of the above-mentioned volatile impurities will increase, and the odor generated during melt molding may become stronger. The upper limit of the temperature is preferably 320°C or lower, and more preferably 310°C or lower. If the temperature is higher than 320°C, the aromatic polycarbonate resin may turn yellow.

[0177] In addition, the pressure is preferably 100 Pa or less, more preferably 80 Pa or less. If the pressure is higher than 100 Pa, the residual amount of the above-mentioned volatile impurities will increase, and the odor generated during melt molding may become stronger. The lower limit of the pressure is not particularly limited, but is preferably 20 Pa or more, more preferably 30 Pa or more. The pressure may be lower than 20 Pa, but the vacuum pump may be increased to a value higher than required, and the driving power of the vacuum pump increases.

[0178] As vertical and horizontal reactors, for example, stirred tank reactors, thin film reactors, centrifugal thin film evaporation reactors, surface renewal type twin-shaft kneading reactors, twin-shaft horizontal stirring reactors, wet wall reactors, porous plate reactors that polymerize while freely falling, or porous plate reactors with metal wires that polymerize while falling along the metal wires, etc. are used.

[0179] Examples of the form of agitating blades for a vertical reactor include turbine blades, paddle blades, Pfaudler blades, anchor blades, Fullzone blades (manufactured by Shinko Pantec Co., Ltd.), SANMELER blades (manufactured by Mitsubishi Heavy Industries, Ltd.), Maxblend blades (manufactured by Sumitomo Heavy Industries, Ltd.), ribbon blades, and twisted lattice blades (manufactured by Hitachi, Ltd.).

[0180] Examples of stirring blades for a horizontal reactor include single-shaft stirring blades such as a disc type or a paddle type, and double-shaft stirring blades such as HVR, SCR, N-SCR (manufactured by Mitsubishi Heavy Industries, Ltd.), BIVOLAK (manufactured by Sumitomo Heavy Industries, Ltd.), spectacles-type blades, or lattice-type blades (manufactured by Hitachi, Ltd.).

[0181] <Catalyst deactivator>

[0182] In the reaction process, it is preferred to perform a catalyst deactivation treatment by adding a catalyst deactivator after the transesterification reaction is completed. By adding the catalyst deactivator, further transesterification reactions can be suppressed to obtain a desired viscosity average molecular weight. In addition, the generation of aromatic monohydroxy compounds can be suppressed, and the generation of odor can be suppressed.

[0183] The catalyst deactivator is not particularly limited as long as it is a compound that reduces the catalytic action of the transesterification catalyst, and examples thereof include acidic compounds.

[0184] Specifically, examples include hydrochloric acid, nitric acid, boric acid, sulfuric acid, sulfurous acid, phosphoric acid, phosphorous acid, hypophosphorous acid, polyphosphoric acid, adipic acid, ascorbic acid, aspartic acid, azelaic acid, adenosine phosphate, benzoic acid, formic acid, isovaleric acid, citric acid, glycolic acid, glutamic acid, glutaric acid, cinnamic acid, succinic acid, acetic acid, tartaric acid, oxalic acid, p-toluenesulfinic acid, p-toluenesulfonic acid, naphthalenesulfonic acid, nicotinic acid, picric acid, picolinic acid, phthalic acid, terephthalic acid, propionic acid, benzenesulfinic acid, benzenesulfonic acid, malonic acid, maleic acid and other Bronsted acids, or their esters, acid halides or salts thereof. These may be used alone or in combination of two or more.

[0185] Among these acidic compounds, sulfonic acid or its ester compound which is liquid and may be substituted with an alkyl group having 1 to 10 carbon atoms is preferred. Examples of sulfonic acid include benzenesulfonic acid, toluenesulfonic acid, and naphthalenesulfonic acid. Examples of sulfonic acid ester compounds include methyl ester compounds, ethyl ester compounds, butyl ester compounds, octyl ester compounds, and phenyl ester compounds. Among these, butyl p-toluenesulfonate is particularly preferred.

[0186] The amount of the catalyst deactivator added is usually preferably 0.5 to 20 molar equivalents relative to 1 mole of the transesterification catalyst, more preferably 5 to 15 molar equivalents, and further preferably in the range of 10 to 15 molar equivalents. If the amount of the catalyst deactivator added is greater than 20 molar equivalents, when the molded article obtained by molding the aromatic polycarbonate resin is exposed to high temperature and high humidity, the decrease in molecular weight may sometimes become greater. As a result, the molded article may be whitened or easily cracked. If the amount of the catalyst deactivator added is less than 0.5 molar equivalents, the molded article may easily turn yellow during the molding of the aromatic polycarbonate resin. In addition, due to insufficient deactivation of the transesterification catalyst, an ester exchange reaction will be carried out in the process of adding a heat stabilizer, a release agent or a colorant, in the process of forming into particles, or during the molding of the aromatic polycarbonate resin, generating an aromatic monohydroxy compound, and the odor of the molded article may become stronger.

[0187] Here, "molar equivalent" refers to the equivalent ratio of the transesterification catalyst to the catalytically active component. For example, when the catalyst compound contains two catalytically active metals, 1 molar equivalent to 1 mole of the catalyst is equivalent to 2 moles of the catalyst deactivator.

[0188] <Devolatile process>

[0189] In the method for producing an aromatic polycarbonate resin, from the perspective of reducing the amount of the above-mentioned non-volatile impurities including low molecular weight products in the obtained aromatic polycarbonate resin, it is preferred to set the following step: after the reaction step, specifically, for example, after the ester exchange reaction treatment (when the condensation reaction treatment is also applied, the condensation reaction treatment) is completed, the reaction product is melt-kneaded and devolatilized using a twin-screw extruder with a vent.

[0190] The axis rotation direction of the twin-screw extruder with vents can be different directions or the same direction, and is preferably the same direction from the viewpoint of mixing performance. By using a twin-screw extruder with vents rotating in the same direction, the supply of the aromatic polycarbonate resin to the filter in the rear stage can be stabilized.

[0191] As described above, non-volatile impurities that may adversely affect the product remain in the reaction product containing the polycarbonate resin obtained in the transesterification reaction. By using a twin-screw extruder with a vent as an extruder, and preferably using a vacuum pump or the like to reduce the pressure from the vent, the non-volatile impurities can be devolatilized and removed. At this time, volatile liquids such as water can also be introduced into the twin-screw extruder with a vent to promote devolatilization. The vent of the twin-screw extruder with a vent can be one or more, preferably more than two.

[0192] In a twin-screw extruder with a vent, the phosphorus compound described later, hindered phenol compound, commonly known heat stabilizer, neutralizer, ultraviolet absorber, light stabilizer, release agent, colorant, antistatic agent, slip, lubricant, plasticizer, compatibilizer, flame retardant, or the above-mentioned catalyst deactivator, etc. can also be added and kneaded.

[0193] The melt-kneading temperature in the twin-screw extruder with a vent depends on the molecular weight of the aromatic polycarbonate resin, etc., but the temperature of the aromatic polycarbonate resin at the outlet of the twin-screw extruder with a vent is preferably set to 275-350° C. If the melt-kneading temperature at the outlet of the extruder is above the above lower limit, the melt viscosity of the aromatic polycarbonate resin can be reduced, the load on the extruder can be reduced, and the productivity can be improved. If the melt-kneading temperature is below the above upper limit, the thermal degradation of the aromatic polycarbonate resin can be reduced, and the mechanical strength reduction, coloring, gas generation and other undesirable conditions caused by the reduction in molecular weight can be suppressed.

[0194] After melt kneading and devolatilization treatment using a twin-screw extruder with a vent, filtration using a filter is preferably performed to remove foreign matter such as burnt and gel in the aromatic polycarbonate resin.

[0195] Examples of a method of melt-extrude an aromatic polycarbonate resin using a twin-screw extruder with a vent, filter the mixture using a filter, and then cool and solidify the mixture to form pellets include the following method.

[0196] (1) A method in which an aromatic polycarbonate resin is supplied from a final polycondensation reactor in a molten state to a twin-screw extruder with a vent, melt-extruded, filtered with a filter, cooled and solidified in the form of strands, and pelletized with a rotary cutter or the like.

[0197] (2) A method in which an aromatic polycarbonate resin is directly supplied from a final polycondensation reactor to a twin-screw extruder with a vent in a molten state, melt-extruded, and then temporarily cooled and solidified in the form of strands to form pellets. The pellets are reintroduced into the extruder and melt-extruded, and then filtered with a filter and cooled and solidified in the form of strands to form pellets.

[0198] (3) An aromatic polycarbonate resin is taken out from a final polycondensation reactor in a molten state, cooled and solidified in the form of a strand without passing through an extruder, temporarily pelletized, and then supplied to a twin-screw extruder with a vent, melt-extruded, filtered with a filter, and cooled and solidified in the form of a strand to pelletize.

[0199] As the form of the filter, a known filter such as a candle type, a pleated type, or a leaf disk type can be used. Among them, a leaf disk type filter having a larger filtering area relative to the storage container is preferred. It is preferred that a plurality of filters are used in combination so that a larger filtering area can be obtained.

[0200] The pore size of the filter is preferably 50 μm or less, more preferably 40 μm or less, based on a filtration accuracy of 99% (absolute filtration accuracy). In the case of particularly reducing foreign matter, the pore size of the filter is preferably 20 μm or less, particularly preferably 10 μm or less. If the pore size becomes smaller, the pressure loss in the filter increases, which may cause damage to the filter or deterioration of the aromatic polycarbonate resin due to shear heat. Therefore, it is preferably 1 μm or more based on a filtration accuracy of 99%. The pore size of the above-mentioned filter is the pore size determined in accordance with ISO16889.

[0201] [Polycarbonate resin composition]

[0202] A polycarbonate resin composition (also referred to as "polycarbonate resin composition" for short) according to another embodiment of the present invention is a resin composition containing the above-mentioned polycarbonate resin. The polycarbonate resin composition may also contain components (other components) other than the above-mentioned polycarbonate resin. The polycarbonate resin composition may be solid or liquid.

[0203] The content of the polycarbonate resin in the polycarbonate resin composition is not particularly limited and can be appropriately set according to the application. It is usually 60% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more. In addition, the upper limit of the content of the polycarbonate resin is not particularly limited and can be 100% by mass or less.

[0204] <Aromatic monohydroxy compound content in polycarbonate resin composition>

[0205] In the polycarbonate resin composition, the content of the aromatic monohydroxy compound measured for the polycarbonate resin composition (the content of the aromatic monohydroxy compound in the polycarbonate resin composition) is preferably 20 mass ppm or less, particularly 18 mass ppm or less, and especially 15 mass ppm or less relative to the polycarbonate resin composition. The aromatic monohydroxy compound in the polycarbonate resin composition is a causative substance of the odor during the melt molding of the polycarbonate resin composition and the odor of the obtained molded product, and preferably less. The lower limit of the content of the aromatic monohydroxy compound in the polycarbonate resin composition is not particularly limited, and can be 0 mass ppm (less than the detection limit) or more than 0 mass ppm.

[0206] As a method for controlling the aromatic monohydroxy compound content of the polycarbonate resin composition within the above preferred range, for example, there can be cited: a method of adjusting the terminal hydroxyl concentration of the polycarbonate resin, a method of adjusting the catalyst amount of the ester exchange catalyst, or a method of adjusting the catalyst deactivation amount. That is, by reducing the terminal hydroxyl concentration of the polycarbonate resin or the amount of the ester exchange catalyst, the rate of the ester exchange reaction is reduced, and the vacuum degree of the final polymerization tank is made high vacuum, the aromatic monohydroxy compound can be efficiently discharged to the outside of the system, and the aromatic monohydroxy compound content of the polycarbonate resin composition can be reduced. In addition, if the catalyst deactivation amount is small, the aromatic monohydroxy compound is generated by performing the ester exchange reaction after the final polymerization tank, and the aromatic monohydroxy compound content of the polycarbonate resin increases, so the catalyst deactivation material is preferably selected from the preferred range described later.

[0207] The content of the aromatic monohydroxy compound in the polycarbonate resin is measured by the method described in Example 1 described later.

[0208] <Content of other impurities in the polycarbonate resin composition>

[0209] The polycarbonate resin composition contains various non-volatile impurities produced as by-products in its manufacturing process. As the volatile impurities, unreacted raw materials such as carbonic acid diesters such as diphenyl carbonate, dihydroxy compounds such as bisphenol A, etc. used as raw materials for polycarbonate resin, or low molecular weight products can be cited. As low molecular weight products, reaction by-products such as the above-mentioned aromatic monohydroxy compounds such as phenol produced as by-products in polycondensation reactions (ester exchange reactions) can be cited.

[0210] The content of carbonic acid diesters such as diaryl carbonate contained in the polycarbonate resin composition is preferably below 120 mass ppm relative to the polycarbonate resin composition, and more preferably below 110 mass ppm. If the content of carbonic acid diesters is below the above-mentioned upper limit, the odor generated during melt forming can be suppressed. The lower limit of the content of carbonic acid diesters is not particularly limited, and can be 0 mass ppm (less than the detection limit), or more than 0 mass ppm.

[0211] The content of these nonvolatile impurities in the polycarbonate resin composition is measured by the method described in Example 1 described later.

[0212] [Other resins]

[0213] The polycarbonate resin composition may also include resins (other resins) other than the above-mentioned polycarbonate resin. The types of other resins are not particularly limited, and for example, polycarbonate resins other than the above-mentioned polycarbonate resins, polyacrylonitrile resins, polyethylene terephthalate resins, polybutylene terephthalate resins, polyethylene naphthalate resins, polyvinyl chloride resins, polyvinylidene chloride resins, polychlorotrichloroethylene resins, polyethylene resins, polypropylene resins, polystyrene resins, cyclic polyolefin resins, polynorbornene resins, polyether sulfone resins, polyether ether ketone resins, polyphenylene sulfide resins, polyarylate resins, polyamide resins, polyimide resins, triacetyl cellulose resins, polystyrene resins, epoxy resins, acrylic resins, or oxazine resins may be cited.

[0214] <Solvent, dispersion medium>

[0215] The polycarbonate resin composition may contain a solvent or a dispersion medium. The type of the solvent or the dispersion medium is not particularly limited, and a liquid capable of dissolving the components contained in the composition or a liquid capable of dispersing the components contained in the composition can be used.

[0216] <Additives for polycarbonate resin composition>

[0217] The polycarbonate resin composition may contain components (other components) other than the above-mentioned polycarbonate resin and other resins. An example of additives that may be added to contain the other components is described below.

[0218] A colorant may be added to the polycarbonate resin composition for the purpose of coloring a molded article.

[0219] The colorant is not particularly limited, but is preferably a dye or pigment colorant selected from phthalocyanine blue and anthraquinone dyes in order to improve odor caused by carbonic acid diesters that may be generated during the production of polycarbonate resins and to improve the hydrolyzability and initial haze of molded products.

[0220] Among phthalocyanine blues, Pigment Blue 15:3 (Colorant Index Common Name) is preferred. Among anthraquinone dyes, blue or violet dyes are preferred. Particularly preferred are Solvent Blue 90, Solvent Blue 97, Solvent Violet 36, or Solvent Violet 13 (Colorant Index Common Names, respectively). Among these, Pigment Blue 15:3 (Colorant Index Common Name) is most preferred.

[0221] There is no particular limitation on the amount of the colorant as long as the molded product is colored to a desired color tone. From the perspective of odor improvement, it is preferably 100 mass ppm or less, more preferably 0.1 to 40 mass ppm, and most preferably 5 to 30 mass ppm relative to the polycarbonate resin composition. If the amount of the colorant exceeds 100 mass ppm, the effect of reducing the odor is small. The method and period of adding the colorant to the polycarbonate resin composition are based on the method and period of adding the additives described later.

[0222] The polycarbonate resin composition may further contain at least one additive selected from stabilizers, ultraviolet absorbers, and release agents, etc., as required. Such additives are not particularly limited, and additives commonly used in polycarbonate resin compositions can be used.

[0223] Examples of the stabilizer include hindered phenol compounds, phosphorus compounds, sulfur compounds, epoxy compounds, and hindered amine compounds, etc. Among these, it is preferred to use at least one antioxidant selected from hindered phenol compounds and phosphorus compounds.

[0224] Specific examples of hindered phenol compounds include n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate, 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], pentaerythritol-tetrakis[3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate], 3,9-bis[1,1-dimethyl-2-{β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, triethylene glycol, alcohol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl) propionate] 3,5-di-tert-butyl-4-hydroxybenzyl phosphate-diethyl ester, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 2,2-thio-diethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-isocyanurate, or N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamic amide), etc. Among these, n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, 1,6-hexanediol-bis[3-(3',5'-tert-butyl-4'-hydroxyphenyl)propionate], or 3,9-bis[1,1-dimethyl-2-{β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane is preferred.

[0225] The phosphorus compound is preferably a trivalent phosphorus compound, and particularly preferably at least one of phosphites in which at least one ester selected from phosphites is esterified with phenol and / or phenol having at least one alkyl group having 1 to 25 carbon atoms, and tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenyl diphosphonate.

[0226] Specific examples of the phosphite include 4,4'-butylene-bis(3-methyl-6-tert-butylphenyl-di(tridecyl))phosphite, 1,1,3-tris(2-methyl-4-di(tridecyl)phosphite-5-tert-butylphenyl)butane, trisnonylphenylphosphite, dinonylphenylpentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, Phosphites such as phosphites, di(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2'-ethylene-bis(4,6-di-tert-butylphenyl)fluorinated phosphite, 2,2'-methylene-bis(4,6-di-tert-butylphenyl)octyl phosphite, or bis(2,4-dicumylphenyl)pentaerythritol diphosphite, and phosphites containing monononylphenol, dinonylphenol or hindered phenol may also be used.

[0227] The phosphorus compound is preferably tetrakis(2,4-di-tert-butylphenyl)-4,4′-biphenyl diphosphonate, tris(2,4-di-tert-butylphenyl)phosphite, or 2,2′-methylene-bis(4,6-di-tert-butylphenyl)octylphosphite.

[0228] The amount of the stabilizer is usually less than 1 part by mass, preferably less than 0.4 parts by mass, relative to 100 parts by mass of the polycarbonate resin composition. If the amount of the stabilizer exceeds 1 part by mass, there are problems such as deterioration of hydrolysis resistance. The mixing ratio when using with a stabilizer can be determined arbitrarily. In addition, which one to use or which one to use can be appropriately determined according to the purpose of the polycarbonate resin composition. Phosphorus compounds are usually effective for retention stability at high temperatures when the polycarbonate resin composition is formed, and heat resistance stability when using molded products. Hindered phenol compounds are usually effective for heat resistance stability when the polycarbonate resin composition is used after being made into molded products, such as heat aging resistance. By using phosphorus compounds and hindered phenol compounds in combination, the improvement effect of colorability is improved.

[0229] As the ultraviolet absorber, in addition to inorganic ultraviolet absorbers such as titanium oxide, cerium oxide or zinc oxide, organic ultraviolet absorbers such as benzotriazole compounds, benzophenone compounds or triazine compounds can also be listed. Among them, organic ultraviolet absorbers are preferred, and at least one selected from benzotriazole compounds, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol, 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-(octyloxy)phenol, 2,2'-(1,4-phenylene)bis[4H-3,1-benzoxazine-4-one], and [(4-methoxyphenyl)-methylene]-malonic acid-dimethyl ester is particularly preferred.

[0230] Specific examples of the benzotriazole compound include 2-bis(5-methyl-2-hydroxyphenyl)benzotriazole, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)benzotriazole, 2-(3',5'-di-tert-butyl-2'-hydroxyphenyl)-5-chlorobenzotriazole, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(3,5 -di-tert-amyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazol-2-yl)phenol], or [methyl-3-〔3-tert-butyl-5-(2H-benzotriazol-2-yl)-4-hydroxyphenyl〕propionate-polyethylene glycol] condensate, etc.

[0231] Among these, particularly preferred are 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazol-2-yl)phenol], 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol, or 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-(octyloxy)phenol.

[0232] The amount of the ultraviolet absorber is usually 10 parts by mass or less, preferably 1 part by mass or less, based on 100 parts by mass of the polycarbonate resin composition. If the amount of the ultraviolet absorber exceeds 10 parts by mass, problems such as mold contamination during injection molding may occur.

[0233] The ultraviolet absorber may be used alone or in combination of two or more.

[0234] The mold release agent includes at least one compound selected from aliphatic carboxylic acids, aliphatic carboxylic acid esters, aliphatic hydrocarbon compounds having a number average molecular weight of 200 to 15000, and polysiloxane-based silicone oils. Among these, at least one selected from aliphatic carboxylic acids and aliphatic carboxylic acid esters is preferably used.

[0235] As the aliphatic carboxylic acid, saturated or unsaturated aliphatic monocarboxylic acid, dicarboxylic acid or tricarboxylic acid can be mentioned. Here, the aliphatic carboxylic acid also includes alicyclic carboxylic acid. Among them, preferred aliphatic carboxylic acid is a mono- or dicarboxylic acid having 6 to 36 carbon atoms, and more preferably an aliphatic saturated monocarboxylic acid having 6 to 36 carbon atoms. Specific examples of aliphatic carboxylic acids include palmitic acid, stearic acid, isovaleric acid, caproic acid, capric acid, lauric acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetratriacontanoic acid, montanic acid, glutaric acid, adipic acid, or azelaic acid.

[0236] As the aliphatic carboxylic acid component constituting the aliphatic carboxylic acid ester, the aliphatic carboxylic acid identical with the above-mentioned aliphatic carboxylic acid can be used. On the other hand, as the alcohol component constituting the aliphatic carboxylic acid ester, saturated or unsaturated monohydric alcohol or saturated or unsaturated polyhydric alcohol etc. can be listed. These alcohols can also be substituted by fluorine atoms or aromatic groups etc. Among these alcohols, monohydric or polyhydric saturated alcohols with less than 40 carbon atoms are preferred, and aliphatic saturated monohydric alcohols or polyhydric alcohols with less than 40 carbon atoms are further preferred. Here, aliphatic alcohols also include alicyclic alcohols.

[0237] Specific examples of these alcohols include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentyl glycol, di(trimethylol)propane, and dipentaerythritol.

[0238] The aliphatic carboxylic acid ester as a raw material may contain an aliphatic carboxylic acid and / or an alcohol as an impurity, or may be a mixture of a plurality of compounds.

[0239] Specific examples of aliphatic carboxylates include beeswax (a mixture with myristyl palmitate as the main component), stearyl stearate, behenyl behenate, octyldodecyl behenate, glyceryl monopalmitate, glyceryl monostearate, glyceryl distearate, glyceryl tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, or pentaerythritol tetrastearate.

[0240] The amount of the release agent is usually 5 parts by mass or less, preferably 1 part by mass or less, based on 100 parts by mass of the polycarbonate resin composition. If the amount of the release agent exceeds 5 parts by mass, problems such as reduced hydrolysis resistance and mold contamination during injection molding may occur.

[0241] The mold release agent may be used alone or in combination of two or more.

[0242] There is no particular limitation on the timing and method of adding additives such as the colorant, stabilizer, ultraviolet absorber, or release agent.

[0243] For example, the additive may be added (1) during the transesterification reaction, (2) at the end of the transesterification reaction, or (3) after the catalyst used in the transesterification reaction is deactivated by a catalyst deactivator and before pelletization. Furthermore, the additive may be added in a molten state of the polycarbonate resin during the kneading process of the polycarbonate resin composition. The additive may be mixed with a solid polycarbonate resin such as pellets or powder and then kneaded by an extruder or the like.

[0244] However, from the viewpoint of suppressing the decomposition of the additive and suppressing coloration, it is preferred to add the additive at any stage: (1) during the transesterification reaction, (2) at the end of the transesterification reaction, or (3) after the catalyst used in the transesterification reaction is deactivated by a catalyst deactivator and before pelletization.

[0245] As a method of adding, additives such as colorants, stabilizers, ultraviolet absorbers, or release agents can be directly mixed or kneaded in the polycarbonate resin, or can be added as a high-concentration masterbatch dissolved in an appropriate solvent or made from a small amount of polycarbonate resin or other resins. When these compounds are used in combination, they can be added to the polycarbonate resin composition separately or simultaneously.

[0246] In the range not impairing the purpose of the present invention, the polycarbonate resin composition may further contain additives such as other thermoplastic resins, flame retardants, impact resistance improvers, antistatic agents, slip agents, anti-blocking agents, lubricants, anti-fogging agents, natural oils, synthetic oils, waxes, organic fillers, or inorganic fillers. That is, the polycarbonate resin composition may be used as a polycarbonate resin composition containing these additives.

[0247] <Method for producing polycarbonate resin composition>

[0248] The method for producing the polycarbonate resin composition is not particularly limited, and examples thereof include a method of mixing the required raw materials, or a method of adding the required raw materials to a solvent or a dispersion medium and mixing them, etc. Examples of the mixer used for mixing include a tumbler, a V-type blender, a Nauta mixer, a Banbury mixer, a mixing roll, or an extruder, etc.

[0249] It should be noted that the polycarbonate resin composition may be a result obtained by the method for producing the polycarbonate resin (including not only the polycarbonate resin but also impurities, etc.). Therefore, the description of the method for producing the polycarbonate resin may also be treated as a description of the method for producing the polycarbonate resin composition.

[0250] [Hollow container]

[0251] Another embodiment of the present invention is a hollow container which is a blow-molded article obtained by blow-molding the above-mentioned polycarbonate resin (including a polycarbonate resin composition containing the polycarbonate resin in the present invention).

[0252] The blow molding of the hollow container can be carried out by applying generally known blow molding methods such as injection blow molding or injection stretch blow molding in addition to direct blow molding.

[0253] For example, in direct blow molding, polycarbonate resin pellets are supplied to a single-screw or twin-screw extruder with a barrel set temperature of 240 to 270°C, melted and kneaded under screw shearing, and a tubular molten parison is extruded through a nozzle. Then, it is sandwiched in a mold having a predetermined shape and set at 70 to 110°C, and air or an inert gas is blown to form a hollow container. It can also be formed by biaxial stretch blow molding disclosed in Japanese Patent Publication No. 6-122140. In order to improve the gas barrier properties of polycarbonate resin, it can also be formed by multilayer blow molding with polyethylene terephthalate or polyamide.

[0254] The size of the hollow container obtained by blow molding the polycarbonate resin is not particularly limited, but the wall thickness is preferably 0.1 to 7 mm, more preferably 0.2 to 5 mm, and most preferably 0.3 to 3 mm from the viewpoint of strength and shape retention of the hollow container.

[0255] Hollow containers can be used for a variety of purposes, and are particularly suitable for use in beverage or food containers such as dairy product bottles, soft drink bottles, or water bottles, other storage bottles, or transparent bottles, etc., due to their low odor.

[0256] [Sheet]

[0257] Another embodiment of the present invention is a sheet which is a molded product obtained by molding a polycarbonate resin (in the present invention, including a polycarbonate resin composition containing the polycarbonate resin).

[0258] It should be noted that, generally, "film" refers to a thin flat product with a very small thickness compared to the length and width and an arbitrarily limited maximum thickness, and is usually supplied in the form of a roll (JIS K6900), and "sheet" refers to a flat product defined in JIS as thin and having a thickness smaller than the length and width. However, the boundary between sheet and film is not clear, and there is no need to distinguish between the two in the language of this specification. Therefore, in this specification, when it is called "film", it also includes "sheet", and when it is called "sheet", it also includes "film".

[0259] The manufacturing method of the sheet material composed of polycarbonate resin is not particularly limited. For example, the polycarbonate resin and other resins and additives as required are melt-kneaded by a single screw or twin screw extruder, extruded into a sheet through a T-die (metal mouth), and quenched and solidified with a casting roll to produce a sheet material.

[0260] In addition, the sheet can be used as a forming sheet to perform various secondary processing, and can also be made into a thermoformed body by heat forming. There is no particular limitation on the method of thermoforming, and known forming methods such as foam forming, vacuum forming or pressure forming can be used.

[0261] The thickness of the sheet is not particularly limited. For example, in consideration of processability and practicality, it is preferably 0.01 mm to 5.0 mm, more preferably 0.03 mm to 3.0 mm, and even more preferably 0.05 to 1 mm. If the thickness of the sheet is within the above range, it is a preferred sheet with excellent impact resistance and flexibility.

[0262] The sheet has excellent heat resistance (wet heat stability) and is not prone to whitening or cracking even when exposed to high temperature and high humidity conditions. It also has low odor and can be suitably used as food packaging materials, pharmaceutical packaging materials, agricultural sheets, or building material sheets.

[0263] Example

[0264] Hereinafter, the present invention will be described in more detail based on examples. However, the present invention is not limited to the following examples.

[0265] [Amount of methylphenyl carbonate (MeDPC) in diphenyl carbonate]

[0266] 1.25 g of diphenyl carbonate was dissolved in acetonitrile and the volume was fixed to 25 mL. The solution was measured by liquid chromatography under the following conditions to quantify methylphenyl carbonate (MeDPC) in diphenyl carbonate.

[0267] Device: LC-20AD manufactured by Shimadzu Corporation

[0268] Chromatographic column: MCI GEL ODS-1HU 12cm×4.6mm

[0269] Analysis temperature: 40℃

[0270] Eluent composition:

[0271] Liquid A pure water

[0272] Liquid B Acetonitrile

[0273] Gradient Program:

[0274] When the analysis time is 0 to 60 minutes

[0275] Maintain A liquid: B liquid = 50:50 (volume ratio, the same applies below.)

[0276] Flow rate: 1.0mL / min

[0277] Detection wavelength: 254nm

[0278] The concentration of methylphenyl carbonate (MeDPC) in the solution was calculated from the total peak area of ​​o-MeDPC, m-MeDPC, and p-MeDPC based on a calibration curve prepared from diphenyl carbonate. Based on this, the amount of MeDPC in diphenyl carbonate was calculated.

[0279] [Evaluation method]

[0280] The physical properties of the polycarbonate resins obtained in the following Examples and Comparative Examples were evaluated by the following methods.

[0281] (1) Terminal hydroxyl concentration

[0282] The terminal hydroxyl group concentration obtained by the colorimetric quantitative method is measured by the colorimetric quantitative method using titanium tetrachloride / acetic acid and by the method described below.

[0283] (a) Preparation of 5 v / v% acetic acid solution

[0284] 50 mL of acetic acid was added to a 1000 mL volumetric flask, and the volume was fixed with dichloromethane and mixed to prepare a 5 v / v% acetic acid solution.

[0285] (b) Preparation of titanium tetrachloride solution

[0286] In a 300-mL flask, add 90 mL of dichloromethane with a measuring cylinder, add 10 mL of 5 v / v% acetic acid solution with a measuring cylinder, add a stirrer and stir with a magnetic stirrer, and slowly add 2.5 mL of titanium tetrachloride solution and 2.0 mL of methanol with a 5-mL graduated pipette to prepare a titanium tetrachloride solution.

[0287] (c) Preparation of standard curve samples

[0288] The dichloromethane solution was prepared in such a way that the terminal hydroxyl concentration of the raw material dihydroxy compound became 10 mass ppm, and 0 mL (no addition), 3 mL or 5 mL were added to a 25 mL volumetric flask. Then, 5 mL of 5 v / v% acetic acid and 10 mL of titanium tetrachloride solution were added respectively. The volumes were fixed with dichloromethane and mixed thoroughly to prepare the standard curve samples.

[0289] (d) Preparation of standard curve

[0290] The absorbance of the prepared standard curve samples was measured at a detection wavelength of 546 nm. The obtained absorbance was plotted against the terminal hydroxyl concentration of the standard curve samples. The inverse of the slope was set as a factor.

[0291] (e) Preparation of test sample and measurement of absorbance

[0292] 0.2 g of polycarbonate resin and 5 mL of dichloromethane were added to a 25 mL volumetric flask and dissolved. Then, 5 mL of 5 v / v% acetic acid solution and 10 mL of titanium tetrachloride solution were added, and the volume was fixed with dichloromethane and mixed thoroughly. The absorbance of the solution thus prepared was measured at a detection wavelength of 546 nm.

[0293] (f) Calculation of terminal hydroxyl concentration

[0294] The terminal hydroxyl group concentration in the polycarbonate resin is calculated by dividing the product of the measured absorbance and the factor by the concentration of the measurement sample.

[0295] (2) Residual phenol, diphenyl carbonate, and bisphenol A

[0296] 1.25 g of a polycarbonate resin was dissolved in 7 mL of dichloromethane, and 30 mL of acetonitrile was added thereto while stirring to reprecipitate the mixture. The volume was further fixed to 50 mL with acetonitrile, and the supernatant was measured by liquid chromatography under the following conditions to quantify the amount of residual phenol, diphenyl carbonate, and bisphenol A.

[0297] Device: LC-20AD manufactured by Shimadzu Corporation

[0298] Column: SUPELCO Ascentis Express C18

[0299] 5cm×3.0mm, 2.7μm

[0300] Analysis temperature: 40℃

[0301] Eluent composition:

[0302] Liquid A: 0.1 mass% phosphoric acid aqueous solution: acetonitrile = 5:1 (volume ratio)

[0303] Liquid B Acetonitrile

[0304] Gradient Program:

[0305] At 0 minutes of analysis time, solution A: solution B = 97:3 (volume ratio, the same applies below).

[0306] The eluent composition was slowly changed to solution A:solution B = 55:45 during the analysis time of 0 to 6.5 minutes, and maintained at solution A:solution B = 2:98 during the analysis time of 7 to 14 minutes.

[0307] Flow rate: 1.0mL / min

[0308] Detection wavelength: 210nm

[0309] The phenol concentration, diphenyl carbonate concentration and bisphenol A concentration in the supernatant were calculated from the peak areas based on the calibration curves prepared from phenol, diphenyl carbonate and bisphenol A. Based on this, the residual phenol amount, diphenyl carbonate amount and bisphenol A amount in the polymer were calculated.

[0310] The detection position of each component is determined by the detection position of each standard curve.

[0311] (3) Viscosity average molecular weight (Mv)

[0312] A polycarbonate resin was dissolved in dichloromethane (concentration 6.0 g / L), and the intrinsic viscosity (limiting viscosity) [η] (unit: dL / g) at 20°C was determined using an Ubbelohde viscometer (manufactured by Moritomo Rika Kogyo Co., Ltd.), and the viscosity average molecular weight (Mv) was calculated based on Schnell's viscosity formula (the following formula).

[0313] η=1.23×10 -4 Mv 0.83

[0314] (4) Specific by-product amount

[0315] After dissolving 0.5 g of polycarbonate resin in 5 mL of dichloromethane, 45 mL of methanol and 5 mL of a 25% by mass sodium hydroxide aqueous solution were added, and the mixture was stirred at 70° C. for 30 minutes for hydrolysis (dichloromethane solution). Then, 6 N hydrochloric acid was added to the dichloromethane solution to adjust the pH of the solution to about 2, and the volume was adjusted to 100 mL with pure water.

[0316] Next, 20 μL of the prepared dichloromethane solution was injected into a liquid chromatograph, and the total content (unit: mass ppm) of the compounds represented by the above formulae (A) to (E) was measured as the specific by-product content.

[0317] The liquid chromatograph and measurement conditions are as follows.

[0318] Liquid chromatograph: LC-10AD manufactured by Shimadzu Corporation

[0319] Chromatographic column: YMC PACK ODS-AM M-307-3

[0320] 4.6mmID×75mmL

[0321] Detector: UV280nm

[0322] Eluent composition:

[0323] Solution A: 0.05 mass% trifluoroacetic acid aqueous solution

[0324] Liquid B Methanol

[0325] Gradient Program:

[0326] At 0 minutes of analysis time, solution A: solution B = 60:40 (volume ratio, the same applies below).

[0327] The eluent composition was slowly changed to solution A:solution B = 5:95 during the analysis time of 0-25 minutes, and maintained at solution A:solution B = 5:95 during the analysis time of 25-30 minutes.

[0328] The contents of the compounds represented by formulae (A) to (E) were calculated from the respective peak areas based on a calibration curve prepared using bisphenol A.

[0329] (5) Terminal group (1) amount

[0330] After dissolving 0.5-1.0 g of a polycarbonate resin in 5 mL of dichloromethane, 45 mL of methanol and 5 mL of a 25% by mass sodium hydroxide aqueous solution were added, and the mixture was stirred at 70° C. for 30 minutes for hydrolysis (dichloromethane solution). Then, 6 N hydrochloric acid was added to the dichloromethane solution to adjust the pH of the solution to about 2, and the volume was adjusted to 100 mL with pure water.

[0331] Next, 20 μL of the prepared dichloromethane solution was injected into a liquid chromatograph, and the cresol content (unit: mass ppm) was measured.

[0332] The liquid chromatograph and measurement conditions are as follows.

[0333] Liquid chromatograph: LC-10AD manufactured by Shimadzu Corporation

[0334] Chromatographic column: YMC PACK ODS-AM M-307-3

[0335] 4.6mmID×75mmL

[0336] Detector: UV280nm

[0337] Eluent:

[0338] Solution A: 0.05 mass% trifluoroacetic acid aqueous solution

[0339] Liquid B Methanol

[0340] Gradient Program:

[0341] At 0 minutes of analysis time, solution A: solution B = 60:40 (volume ratio, the same applies below).

[0342] The eluent composition was slowly changed to solution A:solution B = 5:95 during the analysis time of 0-25 minutes, and maintained at solution A:solution B = 5:95 during the analysis time of 25-30 minutes.

[0343] The cresol content corresponding to the amount of the terminal group (1) was calculated based on a calibration curve prepared using o-cresol.

[0344] (6) Total number of molecular ends, ratio of terminal groups (1) to total terminal groups

[0345] 0.02 g of polycarbonate resin was dissolved in 0.4 mL of deuterated chloroform and heated at 30 °C. 1 H-NMR (JNM-Al400 manufactured by JEOL Ltd.) was used to measure the terminal hydroxyl amount (μeq / g) and the terminal phenyl number (μeq / g). The total number of molecular terminals was calculated by adding the two together, and the terminal group (1) / total terminal group ratio was calculated by the following formula based on the cresol content calculated by (5) above.

[0346] Terminal group (1) / total terminal group ratio =

[0347] {(cresol content (mass ppm) / cresol molecular weight) / total number of molecular ends}×100

[0348] (7) Total aromatic terminal group amount, terminal group (1) / total aromatic terminal group ratio

[0349] After dissolving 0.5-1.0 g of a polycarbonate resin in 5 mL of dichloromethane, 45 mL of methanol and 5 mL of a 25% by mass sodium hydroxide aqueous solution were added, and the mixture was stirred at 70° C. for 30 minutes for hydrolysis (dichloromethane solution). Then, 6 N hydrochloric acid was added to the dichloromethane solution to adjust the pH of the solution to about 2, and the volume was adjusted to 100 mL with pure water.

[0350] Next, 20 μL of the prepared dichloromethane solution was injected into a liquid chromatograph, and the amount of aromatic terminal groups other than the terminal group (1) of the polycarbonate was measured (unit: mass ppm).

[0351] The liquid chromatograph and measurement conditions are as follows.

[0352] Liquid chromatograph: LC-10AD manufactured by Shimadzu Corporation

[0353] Chromatographic column: YMC PACK ODS-AM M-307-3

[0354] 4.6mmID×75mmL

[0355] Detector: UV280nm

[0356] Eluent:

[0357] Solution A: 0.05 mass% trifluoroacetic acid aqueous solution

[0358] Liquid B Methanol

[0359] Gradient Program:

[0360] At 0 minutes of analysis time, solution A: solution B = 60:40 (volume ratio, the same applies below).

[0361] During the analysis time of 0 to 25 minutes, the eluent composition was slowly changed to A solution: B solution = 5:95.

[0362] When the analysis time is 25 to 30 minutes, the ratio of liquid A to liquid B is maintained at 5:95.

[0363] The phenol content corresponding to the amount of aromatic terminal groups was calculated based on a calibration curve prepared using phenol.

[0364] The terminal group (1) / total aromatic terminal group amount ratio is obtained by the following formula from the above aromatic terminal group amount (mass ppm) and the amount of terminal groups (1) (cresol content, mass ppm) obtained by the above (5).

[0365] Terminal group (1) / total aromatic terminal group amount ratio =

[0366] Terminal group (1) amount / (aromatic terminal group amount + terminal group (1) amount)

[0367] (8) Molecular weight reduction and Δhaze after 100 hours at 120°C and saturated water vapor

[0368] The molecular weight reduction rate and Δhaze after 100 hours at 120° C. and saturated steam are obtained to evaluate heat resistance (wet heat stability). A larger value indicates a worse heat resistance (wet heat stability).

[0369] For the laboratory-scale test pieces (Examples 1, 2, 3, 4, 5, 6, Comparative Examples 1, 2, 3), the polycarbonate resin pellets were dried in a ventilation dryer at 120°C for 4 hours, and then injection molded using a small injection molding machine (SHINKO SELLBIC C, Mobile Co., Ltd.) to obtain a plate-shaped molded body with a thickness of 3 mm, a length of 25 mm, and a width of 25 mm. The molding conditions were set to a cylinder temperature of 350°C and a mold temperature of 140°C (molding condition I).

[0370] For the full-scale test pieces (Examples 7, 8, Comparative Example 4), the polycarbonate resin pellets were dried in a ventilation dryer at 120°C for 4 hours and then injection molded using an injection molding machine (J75EII manufactured by Nippon Steel Works, Ltd.) at a mold temperature of 90°C to obtain a plate-shaped molded body having a thickness of 3 mm, a length of 60 mm, and a width of 60 mm. The molding conditions were set to a barrel temperature of 280°C, a molding cycle of 37 seconds, and a screw speed of 90 rpm (molding condition II).

[0371] The obtained plate-shaped molded body was treated at 120° C. and saturated vapor pressure for 100 hours using an autoclave while being suspended in the gas phase.

[0372] The viscosity average molecular weight (Mv) of the polycarbonate resin before and after the treatment was measured by the above method, and the molecular weight reduction rate after the treatment was calculated by the following formula.

[0373] Molecular weight reduction rate =

[0374] (viscosity average molecular weight before treatment - viscosity average molecular weight after treatment) / viscosity average molecular weight before treatment × 100

[0375] The haze of the plate-shaped molded body before and after the treatment was measured using a haze meter (NDH2000 manufactured by Nippon Denshoku Industries) with a D65 light source in accordance with JIS K7105 (1981), and Δhaze was determined from the difference in haze values ​​before and after the treatment.

[0376] (9) Hue evaluation (particle YI)

[0377] The YI value (yellowness index) of the polycarbonate resin pellets in reflected light was measured and evaluated as follows in accordance with ASTM D1925. The apparatus used was a spectrophotometer CM-5 manufactured by Konica Minolta, Inc., and the measurement conditions were a measurement diameter of 30 mm and SCE.

[0378] The calibration glass CM-A212 for petri dish measurement was inserted into the measurement unit, and the zero calibration box CM-A124 was placed on top to perform zero calibration, and then the built-in white calibration plate was used for white calibration. The measurement was performed using the white calibration plate CM-A210, and it was confirmed that L* was 99.40±0.05, a* was 0.03±0.01, b* was -0.43±0.01, and YI was -0.58±0.01.

[0379] The YI value was measured by filling the pellets to a depth of about 40 mm in a cylindrical glass container having an inner diameter of 30 mm and a height of 50 mm. The pellets were taken out of the glass container and measured again, and this operation was repeated twice, and the average value of the three measured values ​​was used.

[0380] The smaller the YI value, the less yellowish the resin is, which means the color tone is better.

[0381] [Abbreviation symbol]

[0382] The abbreviations of the compounds and the like used in the following Examples and Comparative Examples are as follows.

[0383] DPC: diphenyl carbonate

[0384] BPA: Bisphenol A

[0385] MeDPC: Methylphenyl carbonate

[0386] o-MeDPC: o-Methylphenyl carbonate

[0387] PC: Polycarbonate resin

[0388] [Example 1]

[0389] Into a 150 mL glass reactor equipped with a reactor stirrer, a reactor heater, and a reactor pressure regulator, 116.71 g of BPA (about 0.51 mol), 117.29 g of DPC (about 0.55 mol, MeDPC concentration in DPC: 70 mass ppm), and 0.35 g of o-MeDPC were charged, and cesium carbonate was added as an ester exchange catalyst so as to be 0.5 μmol per 1 mol of BPA to prepare a mixture.

[0390] Next, the pressure in the glass reactor was reduced to about 100 Pa (0.75 Torr), and then restored to atmospheric pressure with nitrogen. This operation was repeated three times to replace the interior of the reactor with nitrogen. After nitrogen replacement, the external temperature of the reactor was set to 220°C, and the internal temperature of the reactor was slowly raised to dissolve the mixture. Then, the stirrer was rotated at 100 rpm. Then, the phenol produced as a by-product by the oligomerization reaction of BPA and DPC carried out inside the reactor was distilled off, and the pressure in the reactor was reduced from 101.3 kPa (760 Torr) to 13.3 kPa (100 Torr) in absolute pressure in 40 minutes.

[0391] Next, the pressure in the reactor was maintained at 13.3 kPa, and the ester exchange reaction was carried out for 80 minutes while further distilling out the phenol. Then, the temperature outside the reactor was raised to 290°C, and the pressure in the reactor was reduced from 13.3 kPa (100 Torr) to 399 Pa (3 Torr) in absolute pressure in 40 minutes, and the distilled phenol was removed to the outside of the system. The absolute pressure in the reactor was further reduced to 30 Pa (about 0.2 Torr) to carry out the polycondensation reaction. When the stirrer of the reactor reached the predetermined stirring power set in advance, the polycondensation reaction was terminated.

[0392] Next, the absolute pressure in the reactor was restored to 101.3 kPa using nitrogen gas, and then butyl p-toluenesulfonate was added as a catalyst deactivator in an amount of 5 mass ppm. After stirring for 10 minutes, the pressure was increased to 0.2 MPa using nitrogen gas. The polycarbonate resin was taken out of the reactor in the form of strands, and the obtained polycarbonate resin in the form of strands was pelletized using a rotary cutter.

[0393] Table 1 shows the evaluation results of the obtained polycarbonate resins.

[0394] [Examples 2, 3, 4, 5, 6, Comparative Examples 1, 2, 3]

[0395] As shown in Table 1, each polycarbonate resin was obtained in the same manner as in Example 1 except that the amount of o-MeDPC added and the amount of DPC added were changed. Table 1 shows the evaluation results of the obtained polycarbonate resins.

[0396] [Example 7]

[0397] In a nitrogen atmosphere, a molten mixture at 140° C. prepared by mixing BPA and DPC (MeDPC concentration: 100 ppm) at a certain molar ratio (DPC / BPA molar ratio = 1.070) was continuously supplied to a 13.3×10 3 Pa, 220 ° C in the first vertical reactor, the valve opening of the polymer discharge line provided at the bottom of the reactor was controlled so that the average residence time was 60 minutes, and the liquid level was kept constant. In addition, at the same time as the above raw material supply was started, cesium carbonate was added in an amount of 0.6×10 -6 The cesium carbonate aqueous solution as a catalyst is continuously supplied at a flow rate of 0.6 μmol / 1 mol of BPA. The generated distillates such as phenol are continuously liquefied and recovered by a heat exchanger provided in the distillation line of the first vertical reactor. The reaction liquid discharged from the first vertical reactor is then continuously introduced into the second and third vertical reactors and the fourth horizontal reactor.

[0398] The operating conditions of each reactor are as follows, and the temperature and vacuum are increased as the reaction proceeds.

[0399] Second vertical reactor: 260°C, 4.00×10 3 Pa, 75rpm

[0400] The third vertical reactor: 270°C, 200Pa, 75rpm

[0401] Horizontal reactor No. 4: outlet resin temperature 288°C, 75Pa, 4rpm

[0402] During the reaction, the liquid level was controlled so that the average residence time in the second and third vertical reactors was 60 minutes and the average residence time in the fourth horizontal reactor was 90 minutes, and by-produced phenol was removed by distillation.

[0403] Next, the polymer melt taken out from the fourth horizontal reactor was introduced into a twin-screw extruder with a vent having a three-stage vent and a three-stage supply port (screw diameter 46 mm, partially intermeshing screw type, rotating in the same direction), and butyl p-toluenesulfonate as a catalyst deactivator and tri(2,4-di-tert-butylphenyl)phosphate as a heat stabilizer were supplied in such a manner that the concentrations were 5 mass ppm and 100 mass ppm, respectively, relative to the polycarbonate resin. After devolatilization at each vent (exit temperature of the twin-screw extruder with a vent: 330° C.), the polymer was filtered using a leaf disk type polymer filter (135 leaf disks made of a woven gold mesh with an absolute filtration accuracy of 40 μm were mounted on a center column), and then water-cooled and pelletized.

[0404] Table 2 shows the evaluation results of the obtained polycarbonate resin.

[0405] [Example 8, Comparative Example 4]

[0406] As shown in Table 2, the same procedures as in Example 7 were carried out except that the MeDPC concentration of the raw material DPC, the DPC / BPA molar ratio, the amount of catalyst, the resin temperature at the outlet of the fourth horizontal reactor, the vacuum degree in the fourth horizontal reactor, and the amount of catalyst deactivator added were changed. The evaluation results of the obtained polycarbonate resin are shown in Table 2.

[0407] In Examples 1 to 8 and Comparative Examples 1 to 4, in any of the examples, the terminal groups (1) possessed by the polycarbonate resin were all o-cresol terminals, and terminal groups (1) other than o-cresol terminals did not exist.

[0408] [Table 1]

[0409]

[0410] [Table 2]

[0411]

[0412] According to Tables 1 and 2, the polycarbonate resin having a terminal group (1) / total terminal group ratio in the range of 0.024 to 4.0 mol% has a reduced odor due to a small amount of residual non-volatile impurities such as phenol, BPA and DPC. In addition, the Δ haze and molecular weight reduction rate after treatment at 120°C and saturated water vapor for 100 hours are small, and the heat resistance (wet heat stability) is also excellent.

[0413] On the other hand, in Comparative Examples 1, 2, and 4 in which the ratio of terminal group (1) to all terminal groups was less than 0.024 mol % and Comparative Example 3 in which the ratio of terminal group (1) to all terminal groups exceeded 4.0 mol %, the residual phenol amount, the residual BPA amount, and the residual DPC amount were large, there was an odor problem, and the heat resistance (wet heat stability) was also poor.

[0414] Although the present invention has been described in detail using specific embodiments, it will be apparent to one skilled in the art that various modifications can be made therein without departing from the spirit and scope of the present invention.

[0415] Explanation of symbols

[0416] 11a, 11b, 11c vertical reactor

[0417] 11d Horizontal Reactor

[0418] 12 Heat exchanger

[0419] 13 Phenol tank

[0420] A. Raw material mixture

[0421] B Aromatic polycarbonate resin.

Claims

1. A polycarbonate resin having a terminal group represented by the following formula (1), wherein the ratio of the terminal group represented by the following formula (1) to all terminal groups is 0.024 to 4.0 mol%. [Chemistry 1] In the above formula (1), X 1 ~X 5 may be the same or different, and each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, in, X in formula (1) 1 ~X 5 At least one of them is an alkyl group having 1 to 3 carbon atoms, and * represents a bond with a polycarbonate resin chain. 2 . The polycarbonate resin according to claim 1 , wherein the ratio of the terminal groups represented by the formula (1) to all terminal groups of the polycarbonate resin is 0.024 to 2.0 mol %. 3 . The polycarbonate resin according to claim 2 , wherein the ratio of the terminal groups represented by the formula (1) to all terminal groups of the polycarbonate resin is 0.030 to 2.0 mol %. 4 . The polycarbonate resin according to claim 1 , wherein the terminal group represented by the formula (1) is a methylphenoxy group. The polycarbonate resin according to claim 1 , which is a transesterification product of a dihydroxy compound and a carbonic acid diester, wherein the dihydroxy compound comprises at least one selected from the group consisting of aromatic dihydroxy compounds, aliphatic dihydroxy compounds and alicyclic dihydroxy compounds. The polycarbonate resin according to claim 5 , wherein the aromatic dihydroxy compound is bisphenol A.

7. The polycarbonate resin according to any one of claims 1 to 6, wherein the total amount of the compounds represented by the following formulae (A) to (E) in a hydrolyzate obtained by hydrolyzing the polycarbonate resin is 500 to 6,000 ppm by mass based on the polycarbonate resin, [Chemistry 2] In the above formula (A), R 1 , R in formula (B) 2 , R in formula (C) 3 , R 4 and R in formula (D) 5 , R 6 Each independently represents a hydrogen atom or a methyl group. 8 . The polycarbonate resin according to claim 7 , wherein the total amount of the compounds represented by the formulae (A) to (E) in a hydrolyzate obtained by hydrolyzing the polycarbonate resin is 2,000 to 6,000 ppm by mass based on the polycarbonate resin. 9 . The polycarbonate resin according to claim 8 , wherein the total amount of the compounds represented by the formulae (A) to (E) obtained by hydrolyzing the polycarbonate resin is 3,000 to 6,000 ppm by mass based on the polycarbonate resin. 10 . The polycarbonate resin according to claim 1 , wherein a terminal hydroxyl group concentration of the polycarbonate resin is 1000 ppm by mass or less. 11 . The polycarbonate resin according to claim 10 , wherein a terminal hydroxyl group concentration of the polycarbonate resin is 700 ppm by mass or less. 12 . The polycarbonate resin according to claim 1 , which has a viscosity average molecular weight of 14,000 to 30,000.

13. The polycarbonate resin according to any one of claims 1 to 6, It is characterized in that The total amount of the compound represented by the following formula (2) in the hydrolyzate obtained by hydrolyzing the polycarbonate resin is 4 to 1,500 ppm by mass based on the polycarbonate resin, [Chemistry 3] In the above formula (2), X 1 ~X 5 respectively with X in the formula (1) 1 ~X 5 Synonymous.

14. The polycarbonate resin according to any one of claims 1 to 6, wherein the polycarbonate resin is molded under the following molding condition I, and the molded article has a Δ haze of 4.3 or less after 100 hours at 120°C under saturated water vapor. Forming conditions I: The polycarbonate resin pellets were dried at 120° C. for 4 hours and then injection molded using an injection molding machine at a cylinder temperature of 350° C. and a mold temperature of 140° C. to obtain a plate-shaped molded body having a thickness of 3 mm, a length of 25 mm, and a width of 25 mm. 15 . A polycarbonate resin composition comprising the polycarbonate resin according to claim 1 . 16 . The polycarbonate resin composition according to claim 15 , wherein the content of the aromatic monohydroxy compound in the polycarbonate resin composition is 20 ppm by mass or less.

17. A method for producing a polycarbonate resin, It is characterized in that include: A reaction step of obtaining the polycarbonate resin according to any one of claims 1 to 6 by subjecting a dihydroxy compound to an ester exchange reaction with a carbonic acid diester, The carbonic acid diester includes a carbonic acid diester represented by the following formula (3): [Chemistry 4] In the above formula (3), X 1A ~X 5A and X 1B ~X 5B may be the same or different, and each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, wherein X in formula (3) 1A ~X 5A and X 1B ~X 5B At least one of the groups is an alkyl group having 1 to 3 carbon atoms.

18. The method for producing a polycarbonate resin according to claim 17, It is characterized in that The carbonic acid diester further includes diphenyl carbonate, and the ratio of the amount of the carbonic acid diester represented by the formula (3) to the amount of the diphenyl carbonate is 80 to 35,000 mass ppm.

19. The method for producing a polycarbonate resin according to claim 17, It is characterized in that The carbonic acid diester represented by the formula (3) is methylphenylphenyl carbonate.

20. The method for producing a polycarbonate resin according to claim 17, It is characterized in that The dihydroxy compound includes at least one selected from the group consisting of aromatic dihydroxy compounds, aliphatic dihydroxy compounds, and alicyclic dihydroxy compounds.

21. The method for producing a polycarbonate resin according to claim 20, It is characterized in that The dihydroxy compound is bisphenol A.

22. The method for producing a polycarbonate resin according to claim 17, It is characterized in that Further including: After the reaction step, a step of devolatilizing the polycarbonate resin using a twin-screw extruder with a vent is performed.

23. The method for producing a polycarbonate resin according to claim 17, It is characterized in that In the reaction step, The reaction treatment is carried out in the presence of an ester exchange catalyst, After the reaction treatment, a catalyst deactivation treatment is further performed by adding 5 to 15 molar equivalents of a catalyst deactivator based on 1 mole of the transesterification catalyst. 24 . A hollow container which is a blow-molded article of the polycarbonate resin according to claim 1 . 25 . A hollow container which is a blow-molded product of the polycarbonate resin composition according to claim 15 .

26. The hollow container according to claim 24, which is a dairy product bottle, a refreshing drink bottle or a water bottle. 27 . A sheet which is a molded product of the polycarbonate resin according to claim 1 . 28 . A sheet which is a molded product of the polycarbonate resin composition according to claim 15 .

Citation Information

Patent Citations

  • Polycarbonate resin, production method therefor, and film

    CN108291016A

  • Aromatic polycarbonate and method for producing the same

    JP2004250551A

  • Aromatic polycarbonate resin and method for manufacturing the same

    JP2013213105A

  • Aromatic polycarbonate composition having improved thermal stability, and method for producing the same

    US5912289A