High removal rate chemical mechanical polishing for ophthalmic polishing
By using an aqueous dispersion polishing preparation containing a mixture of α alumina and θ alumina, combined with surfactant, the problems of high viscosity and abrasive properties are solved, and ophthalmic lens polishing with low viscosity and high removal rate is achieved, avoiding alumina The scratching problems caused by increased hardness of abrasive particles provide an efficient polishing effect.
Patent Information
- Application Number
- CN202380033417.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-26
- Filing Date
- 2023-04-17
- Publication Date
- 2024-11-22
AI Technical Summary
The existing ophthalmic lens polishing preparations cannot adapt to the new digital polishing instruments under high viscosity, and cannot maintain abrasive performance and low viscosity at the same time after dilution. The hardness of alumina abrasive particles increases after sintering, which easily scratches the plastic lenses.
Using an aqueous dispersion polishing formulation containing a crystalline alumina and a θ alumina mixture, combined with a surfactant, viscosity between 1 cP and 25 cP, total solids content 15% to 40%, and at least 8 mg/ is achieved in a conventional lens polisher Minute removal rate.
While maintaining low viscosity, it improves the removal rate of the polishing preparation, avoids scratching problems caused by the increase in hardness of the alumina abrasive particles after sintering, and provides an efficient polishing effect suitable for plastic ophthalmic lenses.
Smart Images

Figure CN119013362A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates generally to ophthalmic polishing formulations. More specifically, the present disclosure relates to an ophthalmic lens polishing formulation that provides enhanced or high levels of removal rate while maintaining low viscosity. Background Art
[0002] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.
[0003] When polishing plastic (e.g., polycarbonate) lenses, controlling the viscosity exhibited by ophthalmic lens polishes without negatively affecting abrasive performance becomes an important issue. In conventional lens polishers, high viscosity formulations are not a problem as long as the formulation remains fluid enough to pass through the pump and system at a reasonable rate. Formulations with viscosities as high as 400 centipoise (cP) can be run on conventional polishing instruments without problems. However, newer digital polishing instruments cannot accommodate such viscous formulations, and when the viscosity is too high, negative effects on performance of all metrics have been observed. In addition, simple dilution cannot maintain abrasive performance while reducing viscosity. Instead, simple dilution will reduce viscosity to the point where the concentration of abrasive and active components is too low to provide adequate performance.
[0004] Another challenge in developing ophthalmic lens polishing formulations for polishing plastic lenses is finding a suitable abrasive component. Those skilled in the art understand that most formulations use alpha-alumina (α-Al2O3) as the abrasive grain. However, when alumina sinters to form the α phase, it acquires hardness, and even poor alumina abrasive grains can become hard enough to scratch the surface of relatively soft plastic lenses. Summary of the invention
[0005] The present disclosure generally provides a formulation comprising an aqueous dispersion of abrasive particles and a surfactant configured for polishing the outer surface of a plastic ophthalmic lens. The polishing formulation may have a viscosity of about 1 cP to about 25 cP and a total solids content of about 15 wt % to about 40 wt %. The abrasive particles comprise a mixture of crystalline alpha alumina and theta alumina; the alpha alumina is present in an amount of 50 wt % to 80 wt % relative to the total weight of the abrasive particles, and the theta alumina is present in an amount of 50 wt % to 20 wt % relative to the total weight of the abrasive particles. When desired, the formulation may also include one or more water-dispersible boehmite, a defoamer, aluminum nitrate, and a rinse aid.
[0006] According to one aspect of the present disclosure, the surface area of the abrasive particles is about 10 m 2 / g to about 35m 2 The abrasive particles may also have an average particle size (D) of about 1 micrometer (μm) to about 5 μm.50 ).
[0007] Abrasive grains can be present in a concentration of about 15% to about 30% by weight relative to the gross weight of the formulation. The amount of alpha alumina can be about 60% to about 70% by weight relative to the gross weight of the abrasive grains, and the amount of theta alumina is about 40% to about 30% by weight relative to the gross weight of the abrasive grains. When desired, the abrasive grains can also include <1% by weight of gamma phase alumina or delta phase alumina.
[0008] According to another aspect of the present disclosure, the formulation may have a pH of about 3 to about 5 and a viscosity range of about 1 cP to about 10 cP. The surfactant present in the formulation may include a carboxyl-functionalized or carboxylated polymer or a copolymer thereof.
[0009] In addition, the boehmite may have an average particle size (D 50 ), and is present in an amount up to 10% by weight relative to the total weight of the formulation. The defoaming agent may be a water-soluble silica-based defoaming agent, which is present in a concentration of up to 1% by weight relative to the total weight of the formulation.
[0010] According to yet another aspect of the present disclosure, the formulation provides a removal rate of at least 8 mg / minute when measured using an uncut plastic ophthalmic lens in a conventional lens polisher.The plastic ophthalmic lens may comprise polycarbonate.
[0011] According to another aspect of the present disclosure, a method for polishing the outer surface of a plastic ophthalmic lens is provided. The plastic ophthalmic lens may comprise polycarbonate. The method generally comprises the following steps:
[0012] (a) providing a plurality of abrasive particles, wherein the abrasive particles have an average particle size (D 50 ) is a mixture of crystalline alpha alumina and theta alumina having a diameter of about 1 micron (μm) to about 5 μm; the alpha alumina is present in an amount of 50% to 80% by weight relative to the total weight of the abrasive grains, and the theta alumina is present in an amount of 50% to 20% by weight relative to the total weight of the abrasive grains;
[0013] (b) preparing a formulation comprising an aqueous dispersion of abrasive particles and a surfactant; wherein the polishing formulation has a viscosity of about 1 cP to about 25 cP and a total solids content of about 15 wt % to about 40 wt %;
[0014] (c) applying the formulation to the outer surface of the plastic ophthalmic lens;
[0015] (d) mechanically rubbing the formulation on an outer surface of the plastic ophthalmic lens to remove a layer of plastic material from the outer surface; and
[0016] (e) removing the formulation from the outer surface to obtain a polished surface.
[0017] In this method, abrasive particles can be present in the formulation at a concentration of about 15% to about 30% by weight relative to the total weight of the formulation, wherein the formulation is configured to remove plastic material at a rate of at least 8 mg / minute when measured using an uncut polycarbonate ophthalmic lens in a conventional lens polisher. Mechanical abrasion of the formulation on the outer surface of the plastic ophthalmic lens can be accomplished using conventional mechanical or manual polishing equipment, digital polishers, or manual polishing.
[0018] According to another aspect of the present disclosure, in the method, the step of providing a plurality of abrasive particles further comprises the following steps:
[0019] (a) preparing an aqueous mixture comprising 5 to 30 wt% of uncrystallized boehmite and 0.5 to 4 wt% of nitric acid, relative to the total weight of the mixture;
[0020] (b) placing the aqueous mixture into a sealed reaction vessel;
[0021] (c) heating the sealed reaction vessel to a temperature of 120° C. to 200° C. for 4 to 24 hours to form a slurry;
[0022] (d) collecting and drying the slurry to obtain a powder; and
[0023] (e) calcining the powder at a temperature of 1,000° C. to 1,200° C. for about 1 hour to about 20 hours to form a mixture of crystalline alpha alumina and theta alumina.
[0024] When desired, the mixture of crystallized alpha alumina and theta alumina can be further reduced in particle size using a grinding operation. The abrasive particles can also contain <1 wt % of gamma alumina or delta alumina. The amount of alpha alumina is about 60 wt % to about 70 wt % relative to the total weight of the abrasive particles, and the amount of theta alumina is about 40 wt % to about 30 wt % relative to the total weight of the abrasive particles. The formulation can also contain one or more water-dispersible boehmite, a defoamer, aluminum nitrate, and a rinse aid. When present, the average particle size (D 50 ) is less than about 0.5 μm and is present in an amount up to 10% by weight relative to the total weight of the formulation. When present, the defoaming agent is a water-soluble silica-based defoaming agent, which is present in a concentration of up to 1% by weight relative to the total weight of the formulation.
[0025] Further areas of applicability will become apparent from the description provided herein.It should be understood that the description and specific examples are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] For a better understanding of the present disclosure, its various forms given by way of example will now be described with reference to the accompanying drawings. The components in each of the drawings are not necessarily drawn to scale, emphasis instead being placed upon illustrating the principles of the present invention.
[0027] Figure 1 is a graphical representation of X-ray diffraction (XRD) patterns measured for abrasive particles used in the formulations of Experimental Examples (R-1, R-2) and Comparative Example (C-2) prepared according to the teachings of the present disclosure.
[0028] Figure 2 Graph showing the XRD patterns of the abrasive particles used in the formulations of Comparative Examples (C-1, C-2).
[0029] Figure 3 is a flow chart of a method for polishing an outer surface of a plastic ophthalmic lens according to the teachings of the present disclosure.
[0030] Figure 4 for Figure 3 Flow chart of a method for preparing abrasive particles used in the illustrated method.
[0031] The drawings described herein are for illustration purposes only and are not intended to limit the scope of the present disclosure in any way. It should be understood that throughout the specification and drawings, corresponding reference numerals indicate the same or corresponding parts and features. DETAILED DESCRIPTION
[0032] The following description is merely exemplary in nature and is not intended to limit the present disclosure or its application or use in any way. The present disclosure generally provides an ophthalmic lens polishing formulation that exhibits improved removal rates while maintaining low viscosity. The polishing formulation generally comprises a water-soluble carboxyl-functionalized copolymer and a mixture of crystalline alpha alumina and transition phase alumina.
[0033] For the purposes of this disclosure, the terms "about" and "substantially" as used herein in connection with measurable values and ranges refer to expected variations known to those skilled in the art (eg, limitations and variability of measurements).
[0034] For purposes of this disclosure, the terms "at least one" and "one or more" elements are used interchangeably and may have the same meaning. These terms are intended to include a single element or multiple elements, and may also be indicated by the suffix "(s)" at the end of the element. For example, "at least one surfactant," "one or more surfactants," and "surfactant(s)" are used interchangeably and are intended to have the same meaning.
[0035] According to one aspect of the present disclosure, an objective is to identify additives that can reduce the viscosity of a polishing formulation without negatively affecting performance (e.g., surface quality or removal rate). This objective is achieved by introducing one or more surfactants configured to interact with the abrasive particles and reduce the viscosity of the polishing formulation. It was surprisingly found that the type of surfactant significantly affects the performance of the formulation. The type of surfactant that can provide low viscosity and has a negligible effect on the grinding performance of the polishing formulation is a carboxyl-functionalized or carboxylated polymer or copolymer, such as, but not limited to, short alkyl chain polyethylene glycol ether carboxylates, carboxylic acid triblock surfactants, carboxymethyl cellulose, and polycarboxylates. Examples of commercially available surfactants of this type include, but are not limited to K-XP 228 (Lubrizol Corp., Westlake, Ohio). The surfactant may be present in an amount of 0.1 wt % to 5 wt %; or, about 0.5 wt % to about 3 wt %; or, about 1 wt % to about 2 wt % relative to the total weight of the polishing formulation. More than one carboxyl-functionalized or carboxylated polymeric or copolymeric surfactant or dispersant may be used in combination as a blend or mixture without exceeding the scope of the present disclosure.
[0036] The viscosity of the polishing formulation suitable for polishing plastic lenses is less than 30 centipoise (cP) and greater than 0.5 cP; alternatively, from about 1 cP to about 25 cP; alternatively, from about 1 cP to about 10 cP. The viscosity of the formulation can be measured by any method known in the art, including but not limited to using a rotational rheometer with parallel plate geometry, cone-plate geometry, coaxial cylinder (coquette) cell geometry, spindle (da spindle) (e.g., Brookfield viscometer); viscosity cup; or vibration viscometer.
[0037] According to another aspect of the present disclosure, another object is to determine suitable abrasive components for polishing formulations that overcome the deficiencies of the prior art. It was surprisingly found that alumina containing a mixture of structural phases or transition phases provided higher performance than pure alpha alumina having comparable surface area and phases. As previously described, as the hardness of all-alpha alumina particles increases after calcination, they have a tendency to scratch the surface of plastic lenses. However, milder calcined alumina particles having both alpha and theta phase characteristics provide ideal hardness for polishing plastic lenses. The various alumina phases can be quantitatively measured by X-ray diffraction (XRD). The combination of alpha and theta phases provides an abrasive medium that is soft enough to make scratching of plastic lenses difficult, yet hard enough to provide sufficient grinding to polish the lens surface.
[0038] In the context of the present disclosure, the term α / θ phase alumina refers to a mixture of alumina particles in which a portion of the particles are present in the α phase and a portion of the particles are present in the θ phase. α-alumina particles generally exhibit a high density (i.e., 3.98 g / cm 3 ), and consist essentially of single crystals. On the other hand, θ-alumina particles generally exhibit a lower density (e.g., <3.98 g / cm 3 ) and low crystallinity.
[0039] When aluminum oxide (Al2O3), i.e., alumina, is obtained by thermal dehydration of aluminum hydroxide such as gibbsite Al(OH)3 or boehmite AlO(OH), various structural phases or transition phases are formed as the temperature increases. For example, when boehmite is used as a raw material, the alumina structural phases encountered generally follow the order of γ-alumina (γ) → Δ-alumina (δ) → θ-alumina (θ) → α-alumina (α). As the structural water is removed, boehmite is converted to γ-Al2O3 transition alumina in the temperature range of 500-550°C. The transformation of θ-Al2O3 to α-Al2O3 generally occurs upon prolonged exposure to temperatures above 1050°C.
[0040] The abrasive component in the polishing preparation of the present disclosure generally includes α / θ phase alumina, which contains a mixture of 50 wt% to 80 wt% of α-alumina and 50 wt% to 20 wt% of θ-alumina, consists of a mixture of 50 wt% to 80 wt% of α-alumina and 50 wt% to 20 wt% of θ-alumina, or consists essentially of a mixture of 50 wt% to 80 wt% of α-alumina and 50 wt% to 20 wt% of θ-alumina. Alternatively, in the abrasive component of the polishing preparation, α-Al2O3 is present in an amount of 55 wt% to 75 wt%, and θ-Al2O3 is present in an amount of about 45 wt% to about 25 wt%. Alternatively, in the abrasive component of the polishing preparation, α-Al2O3 is present in an amount of 60 wt% to 70 wt%, and θ-Al2O3 is present in an amount of about 40 wt% to about 30 wt%. Alternatively, the amount of α / θ phase alumina present in the abrasive component of the polishing formulation is provided by a ratio of α-Al2O3 to θ-Al2O3 of 1:1 to 4:1, or a ratio of about 1.25:1 to about 3:1, or a ratio of about 1.5:1 to about 2.25:1. The amount of other alumina phases in the abrasive component, such as γ-alumina or Δ-alumina, is negligible; alternatively, any other alumina phase is present in an amount of ≤0.5 wt%, or ≤1.0 wt%, relative to the weight of the abrasive component.
[0041] The amount of each phase present in the alpha / theta alumina comprising the abrasive grain can be quantitatively determined using X-ray diffraction (XRD) measurements. Quantitative phase analysis refers to the measurement of the relative proportions of elemental components or phases using X-ray diffraction (XRD) patterns, calibrated against internal or external standards. The intensity of the diffraction lines for a particular phase in a mixture depends on the relative amount of that phase in the mixture. Reference Figure 1 and Figure 2 , by measuring the θ-Al2O3 peak at ~33 degrees (see Figure 1 point T in the figure) and the α-Al2O3 peak measured at ~38 degrees (see Figure 1 and Figure 2 The phase ratio between the α phase and the θ phase is determined by the intensity ratio between the points A in the figure. Figure 1 As shown, the abrasive particles used in the polishing formulations of Experimental Examples R-1 and R-2 and Comparative Example C-2 appear to contain a mixture of α-alumina and θ-alumina phases. Figure 2 As shown, the abrasive grains in the polishing formulations used in Comparative Examples C-1 and C-2 contained only the α alumina phase.
[0042] The average particle size of the abrasive particles (D 50) is from 0.5 micrometers (μm) to 7.5 μm; or, from about 1 μm to about 5 μm; or, from about 1.5 μm to about 3 μm. The average particle size and particle size distribution can be measured using any conventional technique, such as screening, microscopy, Coulter counting, dynamic light scattering, or particle imaging analysis, to name a few. Alternatively, a laser particle analyzer is used to determine the average particle size and its corresponding particle size distribution.
[0043] Abrasive particles also show 5m 2 / g to 40m 2 / g surface area; or, about 10m 2 / g to about 35m 2 / g surface area; or, about 15m 2 / g to about 30m 2 The surface area of the abrasive particles can be measured using any known technique, including but not limited to microscopy, small angle x-ray scattering, mercury porosimetry, and Brunauer, Emmett and Teller (BET) analysis. Alternatively, the surface area can be determined using Brunauer, Emmett and Teller (BET) analysis.
[0044] When desired, the polishing formulation may incorporate one or more of water-dispersible boehmite, defoamers, aluminum nitrate, and rinse aids. The amount of boehmite incorporated into the polishing formulation may be from greater than 0 wt% to 12 wt%; or, up to 10 wt%; or, less than or equal to 5 wt%. The average particle size of the boehmite particles may be less than 0.75 μm; or, about 0.5 μm or less; or, not greater than 0.25 μm.
[0045] The optional defoamer in the polishing formulation may include, but is not limited to, a water-soluble silica-based defoamer, present in a concentration of greater than 0 wt % to 1.5 wt %, or not greater than 1 wt %. The optional rinse aid incorporated into the formulation may include any commercially available or known rinse aid, including but not limited to polyvinylpyrrolidone (PVP).
[0046] The resulting polishing formulation comprises an aqueous dispersion of abrasive particles as described above and a surfactant, which has been found to be effective in polishing the outer surface of a plastic ophthalmic lens. The polishing formulation comprises a total solids content of 10% to 50% by weight; alternatively, a total solids content of about 15% to about 40% by weight; alternatively, a total solids content of about 20% to about 35% by weight. The amount of abrasive particles present in the polishing formulation is 10% to 35% by weight; alternatively, about 15% to about 30% by weight; alternatively, about 20% to about 30% by weight.
[0047] Typically, the pH of the polishing formulation is acidic in nature, ie, pH <7; alternatively, the pH range is about 3 to 5; alternatively, the pH range is about 3 to about 4.
[0048] The plastic lens whose surface is polished by the formulation can be any standard plastic poly(allyl diglycol carbonate) lens (e.g., CR-39), polycarbonate lens, Tribrid lens, Trivex lens, high refractive index or ultra-high refractive index plastic lens for ophthalmic applications. Alternatively, the plastic lens is a polycarbonate lens.
[0049] According to yet another aspect of the present disclosure, a method for polishing the outer surface of a plastic ophthalmic lens is provided. Figure 3 The method 100 generally comprises the following steps. First, 110 provides a plurality of abrasive particles, wherein the abrasive particles have an average particle size (D 50 ) is a mixture of crystalline α-alumina and θ-alumina having a particle size of about 1 micron (μm) to about 5 μm, and having an average particle size (D 50 ) is about 1 micrometer (μm) to about 5 μm of crystalline alpha alumina and theta alumina mixture, or consists essentially of an average particle size (D 50 ) is a mixture of crystalline alpha alumina and theta alumina of about 1 micron (μm) to about 5 μm. The alpha alumina is present in an amount of 50% to 80% by weight relative to the total weight of the abrasive particles, and the theta alumina is present in an amount of 50% to 20% by weight relative to the total weight of the abrasive particles. As defined above and further described herein, 120 prepares a polishing formulation. The formulation generally comprises an aqueous dispersion of these abrasive particles and a surfactant. The polishing formulation has a viscosity of about 1 cP to about 25 cP and a total solids content of about 15% to about 40% by weight. 130 The formulation is applied to the outer surface of a plastic ophthalmic lens, and then 140 mechanically rubbed on the outer surface of the plastic ophthalmic lens to remove a layer of plastic material from the outer surface. Finally, 150 removes the formulation from the outer surface to obtain a polished surface.
[0050] As used herein, the phrase "to polish" or the term "polishing" refers to making the surface of an ophthalmic lens smoother by removing material to eliminate the appearance of scratches and the resulting haze. In other words, smoothing the surface of an ophthalmic lens helps to hide or eliminate the appearance of surface defects and reduce the magnitude of any diffuse reflections.
[0051] Figure 3The mechanical rubbing 140 or polishing of the outer surface described in the embodiment can be accomplished by any polishing method known for ophthalmic lenses. Several examples of such polishing methods include, but are not limited to, conventional mechanical or manual polishing machines or polishing equipment, digital polishing machines, or manual polishing. In order to effectively polish the lens surface, the average amount of plastic material removed from the lens surface during the polishing process is 8 mg / min to about 11 mg / min; or, about 9 mg / min to about 10 mg / min, while maintaining a low viscosity as described above.
[0052] Reference Figure 4 , the step 110 of providing a plurality of abrasive particles may include the following steps. 111 An aqueous mixture containing 5 wt % to 30 wt % of uncrystallized boehmite and 0.5 wt % to 4 wt % of nitric acid relative to the total weight of the mixture may be prepared. 113 The aqueous mixture is placed in a sealed reaction vessel and then 115 heated to a temperature of 120° C. to 200° C. for 4 to 24 hours to form a slurry. 117 The slurry is collected and dried to obtain a powder. Finally, 119 the powder is calcined at a temperature of 1000° C. to 1200° C. for about 1 hour to about 20 hours to form a mixture of crystallized α alumina and θ alumina particles. When desired, the step 110 of providing a plurality of abrasive particles may include a step 122 of reducing the particle size of the mixture of crystallized α alumina and θ alumina using a grinding operation. Such a grinding operation may include, but is not limited to, using a sand mill, a vertical ball mill, and a horizontal bead mill.
[0053] Example
[0054] The specific examples provided in this disclosure are given for the purpose of illustrating multiple embodiments of the present invention and should not be construed as limiting the scope of the present disclosure. The embodiments have been described in a manner that enables a clear and concise description to be written, but it is intended and should be understood that the embodiments can be combined or separated in various ways without departing from the present invention. For example, it should be understood that all preferred features described herein are applicable to all aspects of the present invention described herein.
[0055] All of the aluminas used in the polishing formulations prepared according to the teachings of the present disclosure, as well as those used as comparative examples, exhibited an average particle size (D 50 ) range. Having such an average particle size (D 50 ) was obtained by grinding aluminum oxide at 40% by volume in water at 2000 rpm for about 2 hours using 1.25 mm yttria-stabilized zirconium oxide grinding beads in a horizontal bead mill. The particle size distribution was measured every 15 to 30 minutes until the average particle size (D 50 ) within the prescribed scope.
[0056] In preparing each of the following polishing formulations, the raw materials were combined and mixed until uniformly dispersed. In each case, the raw materials were mixed together using an overhead mixer equipped with an impeller-type blade at 600 rpm for 30 to 90 minutes.
[0057] Preparation of polishing formulations according to the present disclosure - In the first experimental example (R-1), a water-based formulation was prepared, which consisted of 20 wt% abrasive grains comprising a mixture of crystalline alpha-phase alumina and theta-phase alumina, 2 wt% aluminum nitrate, 2.5 wt% surfactant (KXP-228, Lubrizol Corp., Westlake, Ohio), 0.5 wt% silica-based defoamer and 2.5 wt% water-dispersible boehmite with the balance being water. In this formulation, the alpha / theta-phase alumina abrasive grains comprised about 35 wt% theta-phase alumina and about 65 wt% alpha-phase alumina (see Figure 1 The average surface area of these abrasive particles is about 24 m 2 / g, and the pH of the preparation was measured to be 3.5.
[0058] In the second experimental example (R-2), a water-based formulation was prepared, which consisted of 20 wt% of α / θ phase alumina abrasive particles, 2 wt% of aluminum nitrate, 2.5 wt% of a surfactant (KXP-228, Lubrizol Corp., Westlake, Ohio), 0.5 wt% of a silica-based defoamer, 2.5 wt% of polyvinylpyrrolidone (PVP), and 2.5 wt% of a water-dispersible boehmite, with the balance being water. In this formulation, the α / θ phase alumina abrasive particles contained about 35 wt% of θ phase alumina and about 65 wt% of α phase alumina (see Figure 1 The average surface area of these abrasive particles is about 24 m 2 / g, the pH of the preparation was measured to be 3.9. The average molecular weight of the polyvinyl pyrrolidone (PVP) used was 10,000 gms / mole.
[0059] Preparation of Comparative Example Formulations - In Comparative Example C-1, a water-based formulation was prepared that contained 25 wt% of uncrystallized alpha alumina abrasive particles, 2 wt% of aluminum nitrate, 2.5 wt% of 1,2-propylene glycol as a surfactant, 0.5 wt% of a silica-based defoamer, 2.5 wt% of a water-dispersible boehmite, and the remainder was water. In this Comparative Example (C-1), there was no theta phase alumina (see Figure 2 ).
[0060] In Comparative Example C-2, a water-based formulation was prepared, which consisted of 20 wt% of abrasive grains comprising a mixture of crystalline α-phase alumina and θ-phase alumina, 2 wt% of aluminum nitrate, 2.5 wt% of a surfactant (1,2-propylene glycol), 0.5 wt% of a silica-based defoamer, and 2.5 wt% of a water-dispersible boehmite, with the balance being water. In this formulation, the α / θ-phase alumina abrasive grains comprised about 35 wt% of θ-phase alumina and about 65 wt% of α-phase alumina (see Figure 1 The average surface area of these abrasive particles is about 24 m 2 / g.
[0061] In Comparative Example C-3, a water-based formulation was prepared that contained 20 wt% of uncrystallized alpha alumina abrasive particles, 2 wt% of aluminum nitrate, 2 wt% of a surfactant (KXP-228, Lubrizol Corp., Westlake, Ohio), 1 wt% of a silica-based defoamer, and 1.5 wt% of a water-dispersible boehmite, with the balance being water. In this Comparative Example (C-1), there was no θ phase alumina (see Figure 2 ).
[0062] Tested Experimental Batches and Comparative Examples - The viscosity and abrasive properties (e.g., removal rates) exhibited by each polishing formulation are summarized in Table 1 below. Comparative formulation C-1 exhibited a viscosity of >300 cP, 20-35 wt% solids, and a removal rate of about 6 mg / min when tested on a conventional lens polishing machine. Comparative formulation C-2 exhibited a viscosity of >300 cP, 20-35 wt% solids, and a removal rate of about 9 mg / min. Comparative formulation C-3 exhibited a viscosity of <20 cP, 20-35 wt% solids, and a removal rate of about 7 mg / min. In contrast, experimental sample R-1 exhibited a viscosity of <20 cP, 20-35 wt% solids, and a removal rate of over 9 mg / min. Similarly, experimental sample R-2 also exhibited a viscosity of <20 cP, 20-35 wt% solids, and a removal rate of over 10 mg / min.
[0063] Table 1
[0064]
[0065] Comparative Examples C-1, C-2, and C-3 show formulations that do not include a crystallized α / θ phase (see C-1, C-3) or have a viscosity of less than 25 centipoise (see C-1, C-2). Therefore, these comparative examples provide a removal rate of less than 8 mg / minute and / or a viscosity that is too high to provide the necessary polishing of polycarbonate lenses. In contrast, experimental batches R-1 and R-2 show formulations prepared according to the teachings of the present invention, which contain a mixture of crystallized α alumina and θ alumina as abrasive particles, and a surfactant or dispersant that reduces the viscosity to less than 25 centipoise (cP). The experimental batches (R-1, R-2) provide low viscosities and removal rates in excess of 8 mg / minute, which are necessary for effective polishing of plastic lenses.
[0066] The conventional lens polisher used in these embodiments is a Satisloh Toro-X-2S system and a plurality of uncut plastic ophthalmic lenses, such as a GENTEX Optics CR39 lens. Viscosity was measured using a Brookfield DV1 viscometer, and pH was measured using a Mettler-Toledo SevenCompact pH meter. Surface area was determined using the BET method on a Micromeretics TriStar II element. X-ray diffraction patterns for phase determination were measured using a Rigaku MiniFlex II desktop X-ray diffractometer. The size reduction of the alumina abrasive particles was performed by grinding in an EMI horizontal bead mill. Particle size distribution data was measured on a Horiba LA930 particle size analyzer by a light scattering method.
[0067] The conditions used to run the Toro-X-2S were to maintain the piston pressure at 0.5 bar and the flow rate of the polishing agent high enough to keep the lens surface coated at all times during the run, with a total flow rate of about 5 L / min for the Toro-X-2S. The run will last for 6 minutes, and before and after the run, the lenses are cleaned with water and gently dried with a clean microfiber cloth. The cleaned lenses are weighed before and after polishing on a Mettler-Toledo New Classic MS balance and the mass is recorded. The change in mass before and after polishing is then divided by the number of minutes the lens is polished to determine the mass / time removal rate. This process is repeated at least 5 times to obtain an average value for each polishing formulation to ensure consistent and accurate results.
[0068] In this specification, the embodiments have been described in a manner that allows for a clear and concise description, but it is intended and should be understood that the embodiments can be combined or separated in various ways without departing from the present invention. For example, it should be understood that all preferred features described herein are applicable to all aspects of the present invention described herein.
[0069] According to the present disclosure, it will be appreciated by those skilled in the art that many changes can be made to the specific embodiments disclosed herein and still the same or similar results can be obtained without departing from or exceeding the spirit or scope of the present disclosure. It will be further appreciated by those skilled in the art that any characteristic reported herein represents a characteristic that is routinely measured and can be obtained by a variety of different methods. The method described herein represents one such method and other methods can be used without exceeding the scope of the present disclosure.
[0070] The above description of various forms of the present invention is presented for the purpose of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. In light of the above teachings, many modifications or variations are possible. The forms discussed are selected and described to provide the best illustration of the principles of the present invention and its practical application, so that one of ordinary skill in the art can utilize the present invention in various forms and make various modifications to suit the specific use contemplated. All such modifications and variations are within the scope of the present invention as determined by the appended claims when interpreted in accordance with the scope to which they are fairly, legally, and equitably entitled.
Claims
1. A formulation comprising an aqueous dispersion of abrasive particles and a surfactant configured for polishing the outer surface of a plastic ophthalmic lens; wherein the polishing formulation has a viscosity of about 1 cP to about 25 cP and a total solids content of about 15 wt % to about 40 wt %; wherein the abrasive grains comprise a mixture of crystallized alpha alumina and theta alumina; the alpha alumina is present in an amount of 50 wt % to 80 wt % relative to the total weight of the abrasive grains, and the theta alumina is present in an amount of 50 wt % to 20 wt % relative to the total weight of the abrasive grains.
2. The formulation of claim 1, further comprising one or more of water-dispersible boehmite, a defoamer, aluminum nitrate and a rinse aid.
3. The formulation of any one of claims 1 or 2, wherein the surface area of the abrasive particles is about 10 m 2 / g to about 35m 2 / g.
4. The formulation according to any one of claims 1 to 3, wherein the average particle size (D 50 ) is about 1 micrometer (μm) to about 5 μm.
5. The formulation of any one of claims 1 to 4, wherein the pH of the formulation is from about 3 to about 5.
6. The formulation of any one of claims 1 to 5, wherein the surfactant comprises a carboxyl-functionalized or carboxylated polymer or copolymer.
7. The formulation of any one of claims 1 to 6, wherein the abrasive particles are present in a concentration of about 15 wt % to about 30 wt % relative to the total weight of the formulation.
8. The formulation of any one of claims 1 to 9, wherein the amount of the alpha alumina is from about 60 wt % to about 70 wt % relative to the total weight of the abrasive grains, and the amount of the theta alumina is from about 40 wt % to about 30 wt % relative to the total weight of the abrasive grains.
9. The formulation according to claim 2, wherein the average particle size (D 50 ) is less than about 0.5 μm and is present in an amount of up to 10 wt % relative to the total weight of the formulation.
10. The formulation of claim 2, wherein the antifoaming agent is a water-soluble silica-based antifoaming agent present in a concentration of up to 1 wt% relative to the total weight of the formulation.
11. The formulation of any one of claims 1 to 10, wherein the formulation has a viscosity ranging from about 1 cP to about 10 cP.
12. The formulation of any one of claims 1 to 11, wherein the formulation provides a removal rate of at least 8 mg / minute when measured using uncut plastic ophthalmic lenses in a conventional lens polishing machine.
13. The formulation of any one of claims 1 to 12, wherein the plastic ophthalmic lens comprises polycarbonate.
14. The formulation of any one of claims 1 to 13, wherein the abrasive grains further comprise <1 wt% of gamma or delta alumina.
15. A method for polishing the outer surface of a plastic ophthalmic lens, the method comprising the steps of: A plurality of abrasive particles are provided, wherein the abrasive particles comprise an average particle size (D 50 ) is a mixture of crystalline alpha alumina and theta alumina having a diameter of about 1 micron (μm) to about 5 μm; the alpha alumina is present in an amount of 50 wt % to 80 wt % relative to the total weight of the abrasive grains, and the theta alumina is present in an amount of 50 wt % to 20 wt % relative to the total weight of the abrasive grains; Prepare a formulation comprising an aqueous dispersion of the abrasive particles and a surfactant; wherein the polishing formulation has a viscosity of about 1 cP to about 25 cP and a total solid content of about 15 wt % to about 40 wt %; applying the formulation to the outer surface of the plastic ophthalmic lens; mechanically rubbing the formulation on an outer surface of the plastic ophthalmic lens to remove a layer of plastic material from the outer surface; and The formulation is removed from the outer surface to obtain a polished surface.
16. The method of claim 15, wherein the abrasive particles are present in the formulation at a concentration of about 15 wt % to about 30 wt % relative to the total weight of the formulation; wherein the formulation is configured to remove plastic material at a rate of at least 8 mg / minute when measured using uncut polycarbonate ophthalmic lenses in a conventional lens polishing machine.
17. The method according to any one of claims 15 or 16, wherein providing a plurality of abrasive particles comprises the following steps: preparing an aqueous mixture comprising 5 to 30 wt % of uncrystallized boehmite and 0.5 to 4 wt % of nitric acid, relative to the total weight of the mixture; placing the aqueous mixture into a sealed reaction vessel; heating the sealed reaction vessel to a temperature of 120° C. to 200° C. for 4 to 24 hours to form a slurry; collecting and drying the slurry to obtain a powder; and The powder is calcined at a temperature of 1,000° C. to 1,200° C. for about 1 hour to about 20 hours to form a mixture of crystalline alpha alumina and theta alumina.
18. The method of claim 17, wherein the mixture of crystallized alpha and theta alumina is further subjected to particle size reduction using a grinding operation.
19. The method of any one of claims 15 to 18, wherein the abrasive grains further comprise <1 wt% of gamma or delta alumina.
20. The method of any one of claims 15 to 19, wherein the plastic ophthalmic lens comprises polycarbonate.
21. The method according to any one of claims 15 to 20, wherein the amount of the alpha alumina is about 60 wt% to about 70 wt% relative to the total weight of the abrasive grains, and the amount of the theta alumina is about 40 wt% to about 30 wt% relative to the total weight of the abrasive grains.
22. A method according to any one of claims 15 to 21, wherein the formulation further comprises one or more of water dispersible boehmite, a defoamer, aluminium nitrate and a rinse aid.
23. The method of claim 22, wherein when present, the average particle size (D 50 ) is less than about 0.5 μm and is present in an amount of up to 10% by weight relative to the total weight of the formulation; Wherein the antifoaming agent, when present, is a water-soluble silica-based antifoaming agent, which is present in a concentration of up to 1 wt % relative to the total weight of the formulation.
24. The method according to any one of claims 15 to 23, wherein the mechanical rubbing of the formulation on the outer surface of the plastic ophthalmic lens is accomplished by using conventional mechanical or manual polishing equipment, digital polishers or manual polishing.