Nonaqueous electrolyte electricity storage element

By using solid graphite and vinyl sulfate in the nonaqueous electrolyte power storage element, the coating is formed, and the problem of high DC resistance at low temperature is solved, and the performance and durability of the battery are improved.

CN119013812APending Publication Date: 2024-11-22GS YUASA INT LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380034200.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-15
Filing Date
2023-04-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing nonaqueous electrolyte power storage components have a high DC resistance at low temperatures, especially the nonaqueous electrolyte power storage components using solid graphite, which have a problem of increased resistance.

Method used

A negative electrode active material containing solid graphite is used and a specific compound, such as vinyl sulfate, is added to the nonaqueous electrolyte, to form a high-quality coating on the surface and inside of the solid graphite to reduce resistance.

Benefits of technology

It effectively reduces the DC resistance of nonaqueous electrolyte power storage components at low temperatures, and improves the durability and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013812A_ABST
    Figure CN119013812A_ABST
Patent Text Reader

Abstract

A non-aqueous electrolyte electricity storage element according to one aspect of the present invention is provided with: a negative electrode having a negative electrode active material containing solid graphite; and a nonaqueous electrolyte containing a compound represented by formula (1). In formula (1), R1 and R2 are each independently a hydrogen atom or a hydrocarbon group. In this connection, the total number of carbon atoms in R1 and R2 is 3 or less. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a nonaqueous electrolyte storage element. Background Art

[0002] Non-aqueous electrolyte secondary batteries represented by lithium ion secondary batteries are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc. due to their high energy density. In addition, as non-aqueous electrolyte storage elements other than non-aqueous electrolyte secondary batteries, capacitors such as lithium ion capacitors and electric double layer capacitors have also been widely used.

[0003] As a non-aqueous electrolyte storage element, it is usually provided with an electrode body having a positive electrode with a positive electrode active material and a negative electrode with a negative electrode active material overlapped via a separator. Such an electrode body is accommodated in a container together with a non-aqueous electrolyte to form a non-aqueous electrolyte storage element. As a negative electrode active material, carbon materials headed by graphite are widely used (see Patent Document 1, Patent Document 2). Prior art literature Patent Literature

[0004] Patent Document 1: Japanese Patent Application Publication No. 2005-222933 Patent Document 2: Japanese Patent Application Publication No. 2017-069039 Summary of the invention Problems to be solved by the invention

[0005] As graphite that becomes the negative electrode active material of non-aqueous electrolyte storage elements, solid graphite with small or substantially no voids inside the particles has been studied. Compared with hollow graphite with large voids inside the particles, solid graphite has advantages such as excellent durability. On the other hand, non-aqueous electrolyte storage elements using solid graphite have the disadvantage of high DC resistance at low temperatures compared to non-aqueous electrolyte storage elements using hollow graphite.

[0006] An object of the present invention is to provide a nonaqueous electrolyte energy storage device having a low direct current resistance at low temperatures, the nonaqueous electrolyte energy storage device using solid graphite. Methods for solving problems

[0007] A nonaqueous electrolyte storage device according to one aspect of the present invention comprises a negative electrode having a negative electrode active material composed of solid graphite and a nonaqueous electrolyte containing a compound represented by the following formula (1). [Chemistry 1] In formula (1), R 1 and R 2 are each independently a hydrogen atom or a hydrocarbon group. 1 and R2 The total number of carbon atoms is 3 or less. Effects of the Invention

[0008] According to one aspect of the present invention, there can be provided a nonaqueous electrolyte electricity storage element having a low direct current resistance at low temperatures, the nonaqueous electrolyte electricity storage element using solid graphite. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] [ Figure 1 ] Figure 1 This is a perspective view showing one embodiment of a non-aqueous electrolyte electricity storage element. [ Figure 2 ] Figure 2 This is a schematic diagram showing one embodiment of an electricity storage device constituted by assembling a plurality of nonaqueous electrolyte electricity storage elements. DETAILED DESCRIPTION

[0010] First, the outline of the nonaqueous electrolyte energy storage device disclosed in this specification will be described.

[0011] [1] A nonaqueous electrolyte storage device according to one aspect of the present invention comprises a negative electrode having a negative electrode active material composed of solid graphite and a nonaqueous electrolyte containing a compound represented by the following formula (1). [Chemistry 2] In formula (1), R 1 and R 2 are each independently a hydrogen atom or a hydrocarbon group. 1 and R 2 The total number of carbon atoms is 3 or less.

[0012] The non-aqueous electrolyte storage element described in [1] above is a non-aqueous electrolyte storage element using solid graphite, and has low DC resistance at low temperatures. The reason for this is not certain, but the following reasons can be inferred. General graphite has voids inside the particles. Therefore, in the graphite assembled in the negative electrode of the non-aqueous electrolyte storage element, a high-quality film from the additive in the non-aqueous electrolyte is formed not only on the outer surface of the particle but also in the voids inside the particle, producing a resistance reduction effect brought about by the film. On the other hand, in the case of solid graphite, it is difficult for the additive to penetrate into the particle, and the film formation inside the particle becomes insufficient. In particular, when the molecules of the additive added to the non-aqueous electrolyte are large, it is more difficult for the additive to penetrate into the interior of the solid graphite, so it is difficult to form a film inside the particle, and the resistance reduction effect brought about by the film is reduced. In contrast, the compound represented by the above formula (1) is a smaller molecule, and it is believed that it can fully penetrate into the interior even for solid graphite to form a film. As described above, the compound represented by the formula (1) can form a high-quality film from the outer surface to the inside of the solid graphite, and therefore it is considered that the DC resistance of the non-aqueous electrolyte power storage device at low temperature is reduced.

[0013] “Graphite” refers to the average lattice spacing (d) of the (002) plane determined by X-ray diffraction before charge / discharge or in a discharged state. 002 ) is 0.33nm or more and less than 0.34nm. Here, the "discharge state" of the carbon material refers to a state in which the lithium ions that can be absorbed and released accompanying the charge and discharge are fully released from the carbon material as the negative electrode active material. For example, in a half-cell using a negative electrode containing a carbon material as a negative electrode active material as a working electrode and using metal Li as a counter electrode, it is a state in which the open circuit voltage is 0.7V or more.

[0014] The "solid" in solid graphite means that the inside of the graphite particles is filled with no voids. More specifically, "solid" means that in the cross-section of the particles observed in the SEM image obtained using a scanning electron microscope (SEM), the area ratio (void ratio) of the voids in the particles relative to the area of ​​the entire particle is 2% or less. The "area ratio of voids within the particle to the area of ​​the entire particle (void ratio)" in the graphite particle can be determined by the following procedure. (1) Preparation of test samples The negative electrode to be measured is fixed with a thermosetting resin. For the negative electrode fixed with the resin, the cross section is exposed by using a cross-section polisher to prepare a sample for measurement. It should be noted that the negative electrode to be measured is prepared by the following steps. In the case where the negative electrode before assembling the non-aqueous electrolyte storage element can be prepared, it is used directly. In the case of preparing from an assembled non-aqueous electrolyte storage element, first, the non-aqueous electrolyte storage element is discharged at a constant current of 0.1C to the discharge termination voltage during normal use to become a discharged state. The non-aqueous electrolyte storage element in the discharged state is disassembled, the negative electrode is taken out, and after being thoroughly cleaned with dimethyl carbonate, it is dried under reduced pressure at room temperature. The operations from the disassembly of the non-aqueous electrolyte storage element to the preparation of the negative electrode to be measured are carried out in a dry air atmosphere with a dew point below -40°C. “In normal use” refers to the case where the nonaqueous electrolyte storage element is used using the charge and discharge conditions recommended or specified for the nonaqueous electrolyte storage element. When equipment for using the nonaqueous electrolyte storage element is prepared, it refers to the case where the nonaqueous electrolyte storage element is used using the equipment. (2) Acquisition of SEM images In obtaining the SEM image (cross-sectional SEM image), JSM-7001F (manufactured by JEOL Ltd.) was used as a scanning electron microscope. The SEM image is an observation of secondary electron images. The accelerating voltage is set to 15 kV. The observation magnification is set to a magnification that makes the number of graphite particles appearing in one field of view more than 3 and less than 15. The obtained SEM image is saved as an image file. In addition, the conditions such as spot diameter, working distance, irradiation current, brightness, and focusing are appropriately set in a manner that the outline of the graphite particles becomes clear. (3) Shearing of graphite particle contours The contour of the graphite particles was cut from the obtained SEM image using the image cutting function of the image editing software Adobe Photoshop Elements 11. The contour cutting was performed by selecting the outer side from the contour of the graphite particles using the quick selection tool and editing the part other than the graphite particles to a black background. At this time, if the number of graphite particles successfully cut to the contour was less than 3, the SEM image was obtained again until the number of graphite particles successfully cut to the contour became 3 or more. (4) Binarization The image of the first graphite particle among the cut graphite particles was binarized using the image analysis software PopImaging 6.00, with a concentration 20% less than the concentration with the highest intensity set as a threshold. The area on the side with a higher concentration was calculated by binarization, and this was used as the "area S1 of the voids within the particle". Next, the same first graphite particle image as before was binarized using a concentration of 10% as a threshold value. The outer edge of the graphite particle was determined by binarization, and the area inside the outer edge was calculated as the "area S0 of the entire particle". The ratio of S1 to S0 (S1 / S0) is calculated using S1 and S0 calculated above, thereby calculating the "area ratio R1 of the voids within the particle to the area of ​​the entire particle" in the first graphite particle. The above binarization process is also performed on the images of the second and subsequent graphite particles among the cut graphite particles to calculate the areas S1 and S0. Based on the calculated areas S1 and S0, the area ratios R2, R3, ... of the voids of each graphite particle are calculated. (5) Determination of the area ratio of voids By calculating the average value of the area ratios R1, R2, R3, ... of all the voids calculated by the binarization process, "the area ratio of the voids in the particle to the area of ​​the entire particle (void ratio)" is determined. It should be noted that, instead of the scanning electron microscope used in the above-mentioned "obtaining the SEM image", the image editing software used in the "cutting of the outline of the graphite particles", and the image analysis software used in the "binarization processing", it is also possible to use a device and software that can perform the same measurements, image editing, and image analysis as them.

[0015] [2] In the nonaqueous electrolyte storage element described in [1] above, the nonaqueous electrolyte may further contain a difluorophosphate.

[0016] The nonaqueous electrolyte energy storage device described in [2] above has a lower DC resistance at low temperatures.

[0017] [3] In the non-aqueous electrolyte storage element described in any one of [1] and [2] above, in a cross-sectional SEM image of the negative electrode, the area ratio occupied by the solid graphite relative to the area occupied by the negative electrode active material may be greater than 50%.

[0018] Regarding the non-aqueous electrolyte storage element described in [3] above, since solid graphite becomes the main negative electrode active material in the negative electrode, the DC resistance reduction effect of the non-aqueous electrolyte storage element at low temperature is particularly significant. In addition, solid graphite becomes the main negative electrode active material, thereby improving durability, etc. The cross-sectional SEM image of the above-mentioned negative electrode is obtained by the same steps as the SEM image when determining the "area ratio (void ratio) of the voids within the particles relative to the area of ​​the entire particle" in the graphite particles. The area occupied by the negative electrode active material is set to the area of ​​the entire particle of the negative electrode active material (also including the area of ​​the voids). It should be noted that the cross-sectional SEM image of the particles containing more than 10 negative electrode active materials in one field of view is used to obtain the area ratio occupied by solid graphite relative to the area occupied by the negative electrode active material (area occupied by solid graphite / area occupied by negative electrode active material).

[0019] [4] In the nonaqueous electrolyte storage element according to any one of [1] to [3] above, the solid graphite may be natural graphite.

[0020] The nonaqueous electrolyte energy storage device described in the above [4] has a lower DC resistance at low temperature.

[0021] [5] In the non-aqueous electrolyte storage element described in any one of [1] to [4] above, in the cross-section of the solid graphite particles observed in the SEM image obtained using a scanning electron microscope (SEM), the area ratio of the voids within the particles relative to the area of ​​the entire particle (void ratio) can be greater than 0.01% and less than 0.5%.

[0022] The nonaqueous electrolyte energy storage device described in the above [5] has a lower DC resistance at low temperatures.

[0023] [6] In the nonaqueous electrolyte storage element described in any one of [1] to [5] above, the content of the compound represented by the above formula (1) in the above nonaqueous electrolyte may be greater than 0 mass % and not more than 5 mass %.

[0024] The nonaqueous electrolyte energy storage device described in the above [6] has a lower DC resistance at low temperature.

[0025] A non-aqueous electrolyte storage element, a storage device, a method for manufacturing a non-aqueous electrolyte storage element, and other embodiments of one embodiment of the present invention are described in detail. It should be noted that the names of the constituent components (constituent elements) used in each embodiment are sometimes different from the names of the constituent components (constituent elements) used in the background art.

[0026] <Non-aqueous electrolyte storage element> A nonaqueous electrolyte storage element according to one embodiment of the present invention comprises: an electrode body having a positive electrode, a negative electrode and a separator; a nonaqueous electrolyte; and a container for accommodating the electrode body and the nonaqueous electrolyte. The electrode body is generally a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are stacked with a separator therebetween, or a wound type in which a positive electrode and a negative electrode are wound with a separator therebetween. The nonaqueous electrolyte exists in a state of being impregnated in the positive electrode, the negative electrode and the separator. As an example of a nonaqueous electrolyte storage element, a nonaqueous electrolyte secondary battery (hereinafter also referred to as a "secondary battery") is described.

[0027] (positive electrode) The positive electrode includes a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer.

[0028] The positive electrode substrate has electrical conductivity. Whether it has "electrical conductivity" is determined by measuring the volume resistivity measured in accordance with JIS-H-0505 (1975) with a value of 10 -2 Ω·cm is used as the threshold value for judgment. As the material of the positive electrode substrate, metals such as aluminum, titanium, tantalum, stainless steel, or their alloys are used. Among them, from the viewpoint of potential resistance, high conductivity and cost, aluminum or aluminum alloys are preferred. As the positive electrode substrate, foil, vapor-deposited film, mesh, porous material, etc. can be listed. From the viewpoint of cost, foil is preferred. Therefore, as the positive electrode substrate, aluminum foil or aluminum alloy foil is preferred. As aluminum or aluminum alloy, A1085, A3003, A1N30, etc. specified in JIS-H-4000 (2014) or JIS-H-4160 (2006) can be exemplified.

[0029] The average thickness of the positive electrode substrate is preferably 3 μm or more and 50 μm or less, more preferably 5 μm or more and 40 μm or less, further preferably 8 μm or more and 30 μm or less, and particularly preferably 10 μm or more and 25 μm or less. By setting the average thickness of the positive electrode substrate to the above range, the strength of the positive electrode substrate can be improved, and the energy density per unit volume of the non-aqueous electrolyte storage element can be improved.

[0030] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode active material layer. The intermediate layer reduces the contact resistance between the positive electrode substrate and the positive electrode active material layer by including a conductive agent such as carbon particles. The composition of the intermediate layer is not particularly limited, and for example, includes a binder and a conductive agent.

[0031] The positive electrode active material layer contains a positive electrode active material and may contain any component such as a conductive agent, a binder, a thickener, and a filler as required.

[0032] As the positive electrode active material, it can be appropriately selected from known positive electrode active materials. As the positive electrode active material for lithium ion secondary batteries, materials that can absorb and release lithium ions are generally used. As the positive electrode active material, for example, lithium transition metal composite oxides having an α-NaFeO2 type crystal structure, lithium transition metal composite oxides having a spinel type crystal structure, polyanion compounds, chalcogen compounds, sulfur, etc. can be listed. As lithium transition metal composite oxides having an α-NaFeO2 type crystal structure, for example, Li[Li x Ni (1-x) ]O2(0≤x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O2(0≤x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Co (1-x) ]O2(0≤x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O2(0≤x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O2(0≤x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1-x-γ-β), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O2 (0≤x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1-x-γ-β), etc. As lithium transition metal composite oxides having a spinel crystal structure, Li x Mn2O4、Li x Ni γ Mn (2-γ) O4, etc. As polyanion compounds, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc. can be listed. As chalcogen compounds, titanium disulfide, molybdenum disulfide, molybdenum dioxide, etc. can be listed. The atoms or polyanions in these materials can be partially replaced by atoms or anions composed of other elements. The surfaces of these materials can also be coated with other materials. In the positive electrode active material layer, one of these materials can be used alone, or two or more of them can be mixed and used.

[0033] The positive electrode active material is usually a particle (powder). The average particle size of the positive electrode active material is preferably, for example, not less than 0.1 μm and not more than 20 μm. By making the average particle size of the positive electrode active material above the above lower limit, the manufacture or handling of the positive electrode active material becomes easy. By making the average particle size of the positive electrode active material below the above upper limit, the electronic conductivity of the positive electrode active material layer is improved. It should be noted that when a composite of the positive electrode active material and other materials is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material. "Average particle size" refers to the value when the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50%, based on the particle size distribution measured by the laser diffraction-scattering method for the diluted solution obtained by diluting the particles with a solvent in accordance with JIS-Z-8825 (2013).

[0034] In order to obtain a powder with a predetermined particle size, a pulverizer, a classifier, etc. can be used. As a pulverization method, for example, a method using a mortar, a ball mill, a sand mill, a vibrating ball mill, a planetary ball mill, a jet mill, a reverse jet mill, a rotating airflow jet mill, or a sieve can be cited. When pulverizing, wet pulverization coexisting with an organic solvent such as water or hexane can also be used. As a classification method, a sieve, a wind classifier, etc. can be used together with a dry method or a wet method as needed.

[0035] The content of the positive electrode active material in the positive electrode active material layer is preferably 50 mass % or more and 99 mass % or less, more preferably 70 mass % or more and 98 mass % or less, further preferably 80 mass % or more and 95 mass % or less. By setting the content of the positive electrode active material to the above range, it is possible to take into account the high energy density and manufacturability of the positive electrode active material layer.

[0036] The conductive agent is not particularly limited as long as it is a material with conductivity. Examples of such conductive agents include carbonaceous materials, metals, conductive ceramics, etc. Examples of carbonaceous materials include graphite, non-graphite carbon, graphene-based carbon, etc. Examples of non-graphite carbon include carbon nanofibers, pitch-based carbon fibers, carbon black, etc. Examples of carbon black include furnace black, acetylene black, Ketjen black, etc. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, etc. Examples of the shape of the conductive agent include powder, fiber, etc. Examples of the conductive agent include one of these materials alone, or a mixture of two or more. In addition, these materials may be used in a composite form. For example, a material obtained by compositeing carbon black with CNT may also be used. Among them, from the viewpoint of electronic conductivity and coating properties, carbon black is preferred, and acetylene black is preferred.

[0037] The content of the conductive agent in the positive electrode active material layer is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. By setting the content of the conductive agent in the above range, the energy density of the nonaqueous electrolyte storage element can be increased.

[0038] As adhesives, for example, thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic acid, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc.

[0039] The content of the binder in the positive electrode active material layer is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. By setting the content of the binder within the above range, the positive electrode active material can be stably retained.

[0040] As the thickener, for example, polysaccharide polymers such as carboxymethyl cellulose (CMC) and methyl cellulose can be cited. When the thickener has a functional group that reacts with lithium or the like, the functional group can be deactivated in advance by methylation or the like. In the case where the positive electrode active material layer contains a thickener, the content of the thickener in the positive electrode active material layer can be set to, for example, 0.1% by mass or more and 10% by mass or less. The content of the thickener in the positive electrode active material layer can be 5% by mass or less, 1% by mass or less, or 0% by mass.

[0041] Filler is not particularly limited. As filler, polyolefins such as polypropylene and polyethylene, silica, aluminum oxide, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, inorganic oxides such as aluminosilicate, hydroxides such as magnesium hydroxide, calcium hydroxide, aluminum hydroxide, carbonates such as calcium carbonate, calcium fluoride, barium fluoride, barium sulfate and other insoluble ionic crystals, nitrides such as aluminum nitride and silicon nitride, talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, mica and other mineral resources or their man-made objects can be listed. In the case where the positive electrode active material layer contains filler, the content of the filler in the positive electrode active material layer can be, for example, 0.1% by mass or more and 10% by mass or less. The content of the filler in the positive electrode active material layer can be 5% by mass or less, 1% by mass or less, or 0% by mass.

[0042] The positive electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, I, typical metal elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, Ba, and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.

[0043] The preparation of the positive electrode can be carried out, for example, by applying a positive electrode mixture paste directly or through an intermediate layer on the positive electrode substrate and drying it. After drying, pressing can be performed as needed. The positive electrode mixture paste contains the positive electrode active material and various components constituting the positive electrode active material layer such as a conductive agent and a binder as arbitrary components. The positive electrode mixture paste usually also contains a dispersion medium.

[0044] (negative electrode) The negative electrode comprises a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The structure of the intermediate layer is not particularly limited, and can be selected from the structures exemplified for the positive electrode described above.

[0045] The negative electrode substrate has conductivity. As the material of the negative electrode substrate, metals such as copper, nickel, stainless steel, nickel-plated steel, or their alloys, carbonaceous materials, etc. can be used. Among them, copper or copper alloys are preferred. As the negative electrode substrate, foil, vapor-deposited film, mesh, porous material, etc. can be listed. From the perspective of cost, foil is preferred. Therefore, as the negative electrode substrate, copper foil or copper alloy foil is preferred. As examples of copper foil, rolled copper foil, electrolytic copper foil, etc. can be listed.

[0046] The average thickness of the negative electrode substrate is preferably 2 μm or more and 35 μm or less, more preferably 3 μm or more and 30 μm or less, further preferably 4 μm or more and 25 μm or less, and particularly preferably 5 μm or more and 20 μm or less. By making the average thickness of the negative electrode substrate within the above range, the strength of the negative electrode substrate can be improved, and the energy density per unit volume of the non-aqueous electrolyte storage element can be improved.

[0047] The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer contains any component such as a conductive agent, a binder, a thickener, and a filler as needed. Any component such as a conductive agent, a binder, a thickener, and a filler can be selected from the materials exemplified for the positive electrode. However, the graphite contained in the negative electrode active material layer is not contained in the conductive agent.

[0048] The negative electrode active material includes solid graphite. The non-aqueous electrolyte storage element has excellent durability because the negative electrode active material of the negative electrode includes solid graphite. For example, a non-aqueous electrolyte storage element using solid graphite in the negative electrode active material tends to have a high capacity retention rate after charge and discharge cycles. In addition, the non-aqueous electrolyte storage element has a low DC resistance at low temperatures by using solid graphite in the negative electrode active material and the non-aqueous electrolyte including the compound represented by the above formula (1).

[0049] Solid graphite can be artificial graphite or natural graphite. Artificial graphite is a general term for graphite manufactured artificially, and natural graphite is a general term for graphite collected from natural minerals. As natural graphite, specifically, flaky graphite (scaly graphite), blocky graphite, earthy graphite, etc. can be exemplified. Solid graphite can be natural graphite in a flat scaly shape or spheroidized natural graphite obtained by spheroidizing the flaky graphite. Solid graphite can be graphite particles with a coating (such as an amorphous carbon coating) applied to the surface. Solid graphite can be manufactured by compressing hollow graphite, etc.

[0050] Solid graphite is sometimes preferably natural graphite (solid natural graphite). Natural graphite can show four peaks in the range of diffraction angle 2θ of 40° to 50° in an X-ray diffraction pattern using CuKα rays measured before charge and discharge or in a discharged state. These four peaks are two peaks from a hexagonal crystal structure and two peaks from a rhombohedral crystal structure. In the case of artificial graphite, usually only two peaks from a hexagonal crystal structure appear. In the X-ray diffraction pattern, the ratio of the peak intensity derived from the (012) plane to the peak intensity derived from the (100) plane ((012) / (100)) is preferably greater than 0.3, and more preferably greater than 0.4. The above peak intensity ratio ((012) / (100)) is preferably less than 0.6. Here, the (100) plane is derived from the structure of the hexagonal crystal system, and the (012) plane is derived from the structure of the rhombohedral crystal system.

[0051] The upper limit of the porosity in the above SEM image (cross-sectional SEM image) of solid graphite is 2%, preferably 1%, more preferably 0.7%, and further preferably 0.5%. In addition, the lower limit of the above porosity may be, for example, 0% or 0.01%, but is sometimes preferably 0.05%, 0.1% or 0.2%. For example, the above porosity may be 0% or more and 2% or less, 0% or more and 1% or less, 0% or more and 0.7% or less, or 0% or more and 0.5% or less. In addition, the above porosity may be 0.01% or more and 2% or less, 0.01% or more and 1% or less, 0.01% or more and 0.7% or less, or 0.01% or more and 0.5% or less. In addition, the above porosity may be 0.05% or more and 2% or less, 0.05% or more and 1% or less, 0.05% or more and 0.7% or less, or 0.05% or more and 0.5% or less. In addition, the above-mentioned porosity can be 0.1% to 2%, 0.1% to 1%, 0.1% to 0.7%, or 0.1% to 0.5%. In addition, the above-mentioned porosity can be 0.2% to 2%, 0.2% to 1%, 0.2% to 0.7%, or 0.2% to 0.5%. Due to the presence of tiny voids in solid graphite, a film is sometimes formed inside, which significantly produces a resistance reduction effect.

[0052] The average particle size of the solid graphite is, for example, preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 50 μm or less, further preferably 3 μm or more and 30 μm or less, and further preferably 5 μm or more and 20 μm or less. By making the average particle size of the solid graphite within the above range, the resistance reduction effect brought about by the film formation can be more fully produced.

[0053] The negative electrode active material may include other negative electrode active materials other than solid graphite. Examples of other negative electrode active materials include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li4Ti5O 12 、LiTiO 2、 Titanium-containing oxides such as TiNb2O7; polyphosphate compounds; silicon carbide; graphite other than solid graphite, non-graphite carbon (graphitizable carbon or non-graphitizable carbon) and other carbon materials; and the like.

[0054] “Non-graphite carbon” refers to the average lattice spacing (d ) of the (002) plane determined by X-ray diffraction before charge / discharge or in a discharged state. 002) is a carbon material having a diameter of 0.34 nm or more and 0.42 nm or less. Examples of non-graphite carbon include difficult-graphitization carbon and easy-graphitization carbon. Examples of non-graphite carbon include materials derived from resins, petroleum asphalt or materials derived from petroleum asphalt, petroleum coke or materials derived from petroleum coke, materials derived from plants, materials derived from alcohols, and the like.

[0055] "Non-graphitizable carbon" refers to the above-mentioned 002 A carbon material having a diameter of 0.36 nm or more and 0.42 nm or less.

[0056] "Graphitizable carbon" refers to the above-mentioned 002 A carbon material having a diameter of 0.34 nm or more and less than 0.36 nm.

[0057] Among all the negative electrode active materials contained in the negative electrode active material layer, solid graphite is preferably the main active material. For example, in the cross-sectional SEM image of the negative electrode, the area ratio occupied by solid graphite (area occupied by solid graphite / area occupied by negative electrode active material) is preferably greater than 50% relative to the area occupied by the negative electrode active material, and more preferably 60% or more, 70% or more, 80% or more, 90% or more, 95% or more or 100%. In addition, relative to all the negative electrode active materials contained in the negative electrode active material layer, the content of solid graphite is preferably greater than 50% by mass, and more preferably 60% or more, 70% or more, 80% or more, 90% or more, 95% or more or 100% by mass. That is, it is particularly preferred to use only solid graphite as the negative electrode active material. In such a case, the DC resistance reduction effect at low temperature of the non-aqueous electrolyte storage element is particularly significantly produced, and in addition, the durability of the non-aqueous electrolyte storage element is also improved.

[0058] The content of solid graphite in the negative electrode active material layer is also sometimes preferably 60% by mass or more and 99% by mass or less, more preferably 90% by mass or more and 98% by mass or less, and further preferably 95% by mass or more. In addition, the content of the negative electrode active material in the negative electrode active material layer is also sometimes preferably 60% by mass or more and 99% by mass or less, more preferably 90% by mass or more and 98% by mass or less, and further preferably 95% by mass or more. By setting the content of solid graphite or negative electrode active material to the above range, it is possible to take into account both the high energy density and the manufacturability of the negative electrode active material layer.

[0059] When the negative electrode active material layer contains a conductive agent, the content of the conductive agent in the negative electrode active material layer can be, for example, 1% by mass or more and 10% by mass or less. The content of the conductive agent in the negative electrode active material layer is sometimes preferably 5% by mass or less, more preferably 2% by mass or less, 1% by mass or less, 0.1% by mass or less, or 0% by mass. When the content of the conductive agent in the negative electrode active material layer is small or does not contain a conductive agent, the content of the negative electrode active material can be increased, and the energy density can be improved.

[0060] The content of the binder in the negative electrode active material layer is preferably 0.1% by mass or more and 10% by mass or less, and more preferably 1% by mass or more and 5% by mass or less. By setting the content of the binder within the above range, the negative electrode active material can be stably retained.

[0061] The content of the thickener in the negative electrode active material layer is preferably 0.1 mass % or more and 5 mass % or less.

[0062] When the negative electrode active material layer contains fillers, the content of the fillers in the negative electrode active material layer can be set to, for example, 0.1% by mass or more and 10% by mass or less. The content of the fillers in the negative electrode active material layer can be 5% by mass or less, 1% by mass or less, or 0% by mass. When the content of the fillers in the negative electrode active material layer is small or does not contain fillers, the content of the negative electrode active material can be increased, and the energy density can be improved.

[0063] The negative electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, I, typical metal elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, Ba, and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.

[0064] The negative electrode active material layer may also be a laminated structure of two or more layers each consisting of different compositions, but is preferably a single-layer structure. When negative electrode active material layers are provided on both sides of the negative electrode substrate, each negative electrode active material layer is also preferably a single-layer structure. A negative electrode having such a negative electrode active material layer has advantages such as excellent productivity.

[0065] The production of the negative electrode can be carried out, for example, by applying a negative electrode mixture paste directly or through an intermediate layer on the negative electrode substrate and drying it. After drying, pressing can be performed as needed. The negative electrode mixture paste contains a negative electrode active material containing solid graphite and various components constituting the negative electrode active material layer such as a conductive agent and a binder as arbitrary components. The negative electrode mixture paste usually also contains a dispersion medium.

[0066] (Diaphragm) The separator can be appropriately selected from known separators. As the separator, for example, a separator consisting only of a substrate layer, a separator having a heat-resistant layer including heat-resistant particles and a binder formed on one or both sides of the substrate layer, etc. can be used. As the shape of the substrate layer of the separator, for example, woven fabrics, non-woven fabrics, porous resin films, etc. can be cited. Among these shapes, porous resin films are preferred from the viewpoint of strength, and non-woven fabrics are preferred from the viewpoint of liquid retention of non-aqueous electrolytes. As the material of the substrate layer of the separator, from the viewpoint of the shutdown function, polyolefins such as polyethylene and polypropylene are preferred, and from the viewpoint of resistance to oxidative decomposition, for example, polyimides, aromatic polyamides, etc. are preferred. As the substrate layer of the separator, a material compounded with these resins can be used.

[0067] The heat-resistant particles contained in the heat-resistant layer preferably have a mass reduction of 5% or less when the temperature is raised from room temperature to 500°C in an air atmosphere of 1 atmosphere, and more preferably have a mass reduction of 5% or less when the temperature is raised from room temperature to 800°C. As materials whose mass reduction is below a predetermined value, inorganic compounds can be cited. As inorganic compounds, for example, oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminum silicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; insoluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalently bonded crystals such as silicon and diamond; talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, mica, and other mineral resources or their artificial products. As inorganic compounds, monomers or complexes of these substances can be used alone, or two or more can be mixed and used. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of safety of the nonaqueous electrolyte storage element.

[0068] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and preferably 20% by volume or more from the viewpoint of discharge performance. Here, the “porosity” refers to a value based on volume, and refers to a value measured by a mercury porosimeter.

[0069] As a separator, a polymer gel composed of a polymer and a non-aqueous electrolyte can be used. As a polymer, for example, polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinyl pyrrolidone, polyvinylidene fluoride, etc. can be cited. When a polymer gel is used, it has an effect of suppressing leakage. As a separator, a porous resin film or a nonwoven fabric as described above can be used together with a polymer gel.

[0070] (Non-aqueous electrolyte) The non-aqueous electrolyte contains the compound represented by the above formula (1). The non-aqueous electrolyte may be a non-aqueous electrolyte solution. The non-aqueous electrolyte solution contains a non-aqueous solvent, an electrolyte salt dissolved in the non-aqueous solvent, and the compound represented by the above formula (1).

[0071] As nonaqueous solvent, it can be suitably selected from known nonaqueous solvents. As nonaqueous solvent, cyclic carbonate, linear carbonate, carboxylate, phosphoric acid ester, sulfonic acid ester, ether, amides, nitrile etc. can be enumerated. As nonaqueous solvent, it is possible to use the material that a part of the contained hydrogen atom in these compounds is replaced by halogen.

[0072] Examples of the cyclic carbonate include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Among them, EC is preferred.

[0073] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among them, EMC is preferred.

[0074] As the non-aqueous solvent, preferably a cyclic carbonate or a chain carbonate is used, and more preferably a cyclic carbonate and a chain carbonate are used in combination. By using a cyclic carbonate, the dissociation of the electrolyte salt can be promoted to improve the ion conductivity of the non-aqueous electrolyte. By using a chain carbonate, the viscosity of the non-aqueous electrolyte can be suppressed to a lower level. In the case of using a cyclic carbonate and a chain carbonate in combination, the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate: chain carbonate) is preferably in the range of 5:95 to 50:50, for example.

[0075] The electrolyte salt may be appropriately selected from known electrolyte salts. Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, and onium salts. Among them, lithium salts are preferred.

[0076] As lithium salts, inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiN(SO2F)2, lithium oxalate salts such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium oxalate salts such as bis(oxalate)difluorophosphate (LiFOP), and lithium salts having halogenated hydrocarbon groups such as LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3, and LiC(SO2C2F5)3 can be cited. Among them, inorganic lithium salts are preferred, and LiPF6 is more preferred.

[0077] The content of the electrolyte salt in the non-aqueous electrolyte is preferably 0.1 mol / dm 3 Above and 2.5 mol / dm 3 Below, more preferably 0.3 mol / dm 3 Above and 2.0 mol / dm 3 Below, more preferably 0.5 mol / dm 3 Above 1.7 mol / dm 3 Below, particularly preferably 0.7 mol / dm 3 Above and 1.5 mol / dm 3 By setting the content of the electrolyte salt to the above range, the ion conductivity of the non-aqueous electrolyte can be improved.

[0078] In the compound represented by the above formula (1), R in the above formula (1) 1 and R 2 are independently a hydrogen atom or a hydrocarbon group. 1 and R 2 The total number of carbon atoms of is 3 or less. 1 and R 2 The hydrocarbon group represented by may be an alkyl group such as a methyl group, an ethyl group, a propyl group, or an alkenyl group such as a vinyl group, and an alkyl group is preferred. 1 and R 2 At least one of them is a hydrogen atom, and more preferably R 1 and R 2 Both of these are hydrogen atoms.

[0079] Examples of the compound represented by the above formula (1) include: 1 and R 2 Vinyl sulfate, R 1 is a hydrogen atom and R 2 2,3-Propylene sulfate, R 1 is a hydrogen atom and R 2 The compound represented by the above formula (1) may be used alone or in combination of two or more.

[0080] The content of the compound shown in the above formula (1) in the non-aqueous electrolyte (non-aqueous electrolyte) can be, for example, greater than 0% by mass and less than 5% by mass, can be greater than 0.01% by mass and less than 3% by mass, or can be greater than 0.1% by mass and less than 2% by mass. In addition, the above content can be, for example, greater than 0% by mass and less than 5% by mass, can be greater than 0% by mass and less than 3% by mass, or can be greater than 0% by mass and less than 2% by mass. In addition, the above content can be, for example, greater than 0.01% by mass and less than 5% by mass, can be greater than 0.01% by mass and less than 3% by mass, or can be greater than 0.01% by mass and less than 2% by mass. In addition, the above content can be, for example, greater than 0.1% by mass and less than 5% by mass, can be greater than 0.1% by mass and less than 3% by mass, or can be greater than 0.1% by mass and less than 2% by mass. The compound shown in the above formula (1) is usually decomposed during the initial charge and discharge, forming a film on the outer surface and inside of solid graphite. Therefore, in the assembled non-aqueous electrolyte storage element, if even a trace amount of the compound represented by the above formula (1) remains in the non-aqueous electrolyte, a film derived from the compound represented by the above formula (1) has already been formed on the outer surface and inside of the solid graphite, and the effect based on the compound represented by the above formula (1) can be exerted.

[0081] The non-aqueous electrolyte (non-aqueous electrolyte) preferably further comprises a difluorophosphate. When the non-aqueous electrolyte comprises a compound represented by the above formula (1) and also comprises a difluorophosphate, the DC resistance of the non-aqueous electrolyte storage element at low temperature becomes lower. As difluorophosphate, lithium difluorophosphate, sodium difluorophosphate, etc. can be cited, preferably lithium difluorophosphate. One difluorophosphate can be used alone, or two or more can be used in combination.

[0082] The content of difluorophosphate in nonaqueous electrolyte (nonaqueous electrolyte) can be, for example, greater than 0 mass % and less than 3 mass %, can be more than 0.01 mass % and less than 1.8 mass %, or can be more than 0.1 mass % and less than 1.6 mass %. Difluorophosphate is the same as the compound shown in the above formula (1), usually decomposes during initial charge and discharge, and forms a film on the outer surface and inside of solid graphite. Therefore, in the assembled nonaqueous electrolyte storage element, if there is a trace of difluorophosphate in the nonaqueous electrolyte, a film from difluorophosphate has been formed on the outer surface and inside of solid graphite together with the compound shown in the above formula (1), and the effect based on difluorophosphate can be exerted.

[0083] In addition to the non-aqueous solvent, electrolyte salt, the compound represented by the above formula (1) and difluorophosphate, the non-aqueous electrolyte may also contain other additives. Examples of other additives include aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partial hydrogenation of terphenyl, cyclohexylbenzene, tert-butylbenzene, tert-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; vinylene carbonate, methyl vinylene carbonate, ethyl vinylene carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaric anhydride, itaconic anhydride, cyclohexanedicarboxylic anhydride, dimethyl sulfite, methyl methanesulfonate, white Sulfamethoxybenzene, methyl toluenesulfonate, dimethyl sulfate, vinyl sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathialane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathialane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propylene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, tetrakis(trimethylsilyl)titanate, etc. These other additives may be used alone or in combination of two or more.

[0084] The content of other additives contained in the nonaqueous electrolyte is preferably 0.01 mass % or more and 10 mass % or less relative to the mass of the entire nonaqueous electrolyte, more preferably 0.1 mass % or more and 7 mass % or less, further preferably 0.2 mass % or more and 5 mass % or less, particularly preferably 0.3 mass % or more and 3 mass % or less. By setting the content of other additives to the above range, it is possible to improve the capacity maintenance performance or cycle performance after high temperature storage, or further improve safety.

[0085] A solid electrolyte may be used as the non-aqueous electrolyte, or a non-aqueous electrolyte solution and a solid electrolyte may be used in combination.

[0086] The solid electrolyte can be selected from any material that has ion conductivity and is solid at room temperature (e.g., 15° C. to 25° C.), such as lithium, sodium, and calcium. Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes.

[0087] In the case of lithium ion secondary batteries, examples of sulfide solid electrolytes include Li2S-P2S5, LiI-Li2S-P2S5, Li10 Ge-P2S 12 wait.

[0088] The shape of the nonaqueous electrolyte storage element of the present embodiment is not particularly limited, and examples thereof include cylindrical batteries, square batteries, flat batteries, coin batteries, and button batteries.

[0089] Figure 1 A non-aqueous electrolyte storage element 1 is shown as an example of a square battery. It should be noted that this figure is a perspective view of the inside of a container. An electrode body 2 having a positive electrode and a negative electrode wound with a separator interposed therebetween is housed in a square container 3. The positive electrode is electrically connected to a positive terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative terminal 5 via a negative electrode lead 51.

[0090] <Electrical Storage Device> The non-aqueous electrolyte storage element of the present embodiment can be used as a storage unit (battery module) composed of a plurality of non-aqueous electrolyte storage elements assembled and mounted on a power supply for automobiles such as electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), a power supply for electronic devices such as personal computers and communication terminals, or a power supply for power storage, etc. In this case, it is sufficient to apply the technology of the present invention to at least one non-aqueous electrolyte storage element included in the storage unit.

[0091] Figure 2 An example of an electric storage device 30 is shown in which an electric storage unit 20 composed of two or more electrically connected non-aqueous electrolyte storage elements 1 is further assembled. The electric storage device 30 may also include a bus bar (not shown) electrically connecting the two or more non-aqueous electrolyte storage elements 1, a bus bar (not shown) electrically connecting the two or more electric storage units 20, etc. The electric storage unit 20 or the electric storage device 30 may also include a state monitoring device (not shown) that monitors the state of one or more non-aqueous electrolyte storage elements.

[0092] <Method for Manufacturing Non-Aqueous Electrolyte Storage Element> The manufacturing method of the non-aqueous electrolyte storage element of the present embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, preparing an electrode body; preparing a non-aqueous electrolyte; and storing the electrode body and the non-aqueous electrolyte in a container. Preparing the electrode body includes: preparing a positive electrode and a negative electrode; and forming the electrode body by stacking or winding the positive electrode and the negative electrode through a separator.

[0093] The operation of storing the non-aqueous electrolyte in the container can be appropriately selected from known methods. For example, when a non-aqueous electrolyte solution is used as the non-aqueous electrolyte, the non-aqueous electrolyte solution can be injected from an injection port formed in the container and then the injection port can be sealed.

[0094] The content of the compound represented by the above formula (1) in the prepared nonaqueous electrolyte is preferably 0.1% by mass or more and 5% by mass or less, more preferably 0.2% by mass or more and 2% by mass or less. In addition, when the nonaqueous electrolyte contains difluorophosphate, the content of the difluorophosphate in the prepared nonaqueous electrolyte is preferably 0.1% by mass or more and 3% by mass or less, more preferably 0.2% by mass or more and 1.8% by mass or less.

[0095] <Other Implementation Methods> It should be noted that the nonaqueous electrolyte storage element of the present invention is not limited to the above-mentioned embodiment, and various changes can be made without departing from the scope of the present invention. For example, the structure of other embodiments can be added to the structure of a certain embodiment, and in addition, a part of the structure of a certain embodiment can be replaced with the structure of other embodiments or known technology. Furthermore, a part of the structure of a certain embodiment can be deleted. In addition, known technology can be added to the structure of a certain embodiment.

[0096] In the above embodiment, the case where the nonaqueous electrolyte storage element is used as a nonaqueous electrolyte secondary battery (e.g., a lithium ion secondary battery) capable of charge and discharge is described, but the type, shape, size, capacity, etc. of the nonaqueous electrolyte storage element are arbitrary. The present invention can also be applied to capacitors such as various secondary batteries, double-layer capacitors, or lithium ion capacitors.

[0097] In the above embodiment, the electrode body is described as a positive electrode and a negative electrode stacked with a separator interposed therebetween, but the electrode body may not have a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state where a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode. Example

[0098] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to the following Examples.

[0099] [Example 1] (Production of positive electrode) LiNi is used as the positive electrode active material 1 / 3 Co 1 / 3 Mn 1 / 3 The positive electrode mixture paste is prepared by using O2, acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a dispersion medium. It should be noted that the mass ratio of the positive electrode active material, AB, and PVDF is set to 93:4:3 (solid content conversion). The positive electrode mixture paste is applied to one side of the aluminum foil as the positive electrode substrate and dried. Then, roll pressing is performed to obtain a positive electrode.

[0100] (Production of negative electrode) A negative electrode mixture paste is prepared by mixing solid natural graphite as a negative electrode active material, styrene-butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and water as a dispersion medium. It should be noted that the mass ratio of solid natural graphite, SBR and CMC is set to 98:1:1 (solid content conversion). The negative electrode mixture paste is applied to one side of a copper foil as a negative electrode substrate and dried. Then, roller pressing is performed to obtain a negative electrode. The porosity of solid natural graphite obtained by the above method is 0.49%, and the average particle size is 7.7μm. In addition, since only solid natural graphite is used as the negative electrode active material, in the cross-sectional SEM image of the negative electrode, the area occupied by solid graphite is 100% relative to the area occupied by the negative electrode active material.

[0101] (Non-aqueous electrolyte) In a solvent prepared by mixing ethylene carbonate and ethyl methyl carbonate at a volume ratio of 30:70, 1.2 mol / dm 3 LiPF6 was dissolved at a concentration of 0.5 mass %, and vinyl sulfate (R in the above formula (1)) as a compound represented by the above formula (1) was dissolved at a concentration of 0.5 mass % 1 and R 2 All of them are compounds containing hydrogen atoms, and compound A) is used as an additive to obtain a non-aqueous electrolyte.

[0102] (Diaphragm) A polyolefin microporous film was used as the separator.

[0103] (Assembly of non-aqueous electrolyte storage element) The positive electrode, negative electrode and separator were used to obtain a stacked electrode body. The electrode body was placed in a container, a non-aqueous electrolyte was injected and the container was sealed. Thus, the non-aqueous electrolyte storage element of Example 1 was obtained.

[0104] [Example 2] A nonaqueous electrolyte storage device of Example 2 was obtained in the same manner as in Example 1 except that the following nonaqueous electrolyte solution was used. In a solvent prepared by mixing ethylene carbonate and ethyl methyl carbonate at a volume ratio of 30:70, 1.2 mol / dm 3 LiPF6 is dissolved in a concentration of 0.5 mass %, and further vinyl sulfate (compound A) and lithium difluorophosphate (LiPO2F2) are dissolved in a concentration of 0.5 mass % as additives to obtain a non-aqueous electrolyte.

[0105] [Comparative Example 1] A nonaqueous electrolyte storage device of Comparative Example 1 was obtained in the same manner as in Example 1 except that a nonaqueous electrolyte solution containing 4,4′-bis(2,2-dioxo-1,3,2-dioxathiapentane) (Compound B represented by the following formula (2)) was used as an additive instead of vinyl sulfate (Compound A).

[0106] [Chemistry 3]

[0107] [Reference Example 1] A nonaqueous electrolyte storage element of Reference Example 1 was obtained in the same manner as in Comparative Example 1 except that hollow natural graphite (porosity: 7.69%) was used as the negative electrode active material instead of solid natural graphite.

[0108] [Reference Example 2] A nonaqueous electrolyte storage element of Reference Example 2 was obtained in the same manner as in Example 1 except that hollow natural graphite (porosity: 7.69%) was used as the negative electrode active material instead of solid natural graphite.

[0109] [Reference Example 3] A nonaqueous electrolyte storage element of Reference Example 3 was obtained in the same manner as in Example 2 except that hollow natural graphite (porosity: 7.69%) was used as the negative electrode active material instead of solid natural graphite.

[0110] (Evaluation: Low temperature DCR) For each non-aqueous electrolyte storage element of Example 1, Example 2, Comparative Example 1 and Reference Examples 1 to 3, first, constant current charging is performed at 25°C with a current of 0.2C to 4.1V, and then constant voltage charging is performed at 4.1V. The end condition of charging is set to when the charging current reaches 0.01C. After a 10-minute rest after charging, constant current discharge is performed at 25°C with a current of 1.0C to 2.75V. A 10-minute rest is set after discharge. Next, constant current charging is performed at 25°C with a current of 1.0C to make the SOC 50%. After being stored in a constant temperature bath at -10°C for 4 hours, discharge is performed at a current value of 0.5C, 1.0C or 1.5C for 30 seconds respectively. After each discharge is completed, constant current charging is performed with a current of 0.2C to make the SOC 50%. The relationship between the current value in each discharge and the voltage at the tenth second after the start of discharge is plotted, and the low-temperature direct current resistance (low-temperature DCR) is calculated based on the slope of the straight line obtained by plotting the three points. The obtained low-temperature DCR is shown in Table 1. In addition, the relative values ​​of the low-temperature DCR based on the case of using compound B as an additive are also shown in Table 1. That is, the low-temperature DCR (relative value) of Comparative Example 1 and Examples 1 and 2 are values ​​based on Comparative Example 1 (100%), and Reference Examples 1 to 3 are values ​​based on Reference Example 1 (100%).

[0111] [Table 1] Compound A: Vinyl sulfate Compound B::4,4'-bis(2,2-dioxo-1,3,2-dioxathiapentane)

[0112] [Reference Example 4] (Production of positive electrode) LiNi is used as the positive electrode active material 1 / 3 Co 1 / 3 Mn 1 / 3 The positive electrode mixture paste is prepared by using O2, acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a dispersion medium. It should be noted that the mass ratio of the positive electrode active material, AB, and PVDF is set to 93:4:3 (solid content conversion). The positive electrode mixture paste is applied to both sides of the aluminum foil as the positive electrode substrate and dried. Then, roll pressing is performed to obtain a positive electrode.

[0113] (Production of negative electrode) The negative electrode mixture paste is prepared by mixing hollow natural graphite (porosity 7.69%) as a negative electrode active material, styrene-butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and water as a dispersion medium. It should be noted that the mass ratio of hollow natural graphite, SBR and CMC is set to 98:1:1 (solid content conversion). The negative electrode mixture paste is applied to both sides of the copper foil as the negative electrode substrate and dried. Then, roll pressing is performed to obtain a negative electrode.

[0114] (Non-aqueous electrolyte) In a solvent prepared by mixing ethylene carbonate and ethyl methyl carbonate at a volume ratio of 30:70, 1.2 mol / dm 3 LiPF6 is dissolved in a concentration of to obtain a non-aqueous electrolyte.

[0115] (Diaphragm) A polyolefin microporous film was used as the separator.

[0116] (Assembly of non-aqueous electrolyte storage element) The positive electrode, negative electrode and separator were used to obtain a wound electrode body. The electrode body was placed in a container, a non-aqueous electrolyte was injected and the container was sealed. Thus, the non-aqueous electrolyte storage element of Reference Example 4 was obtained.

[0117] [Reference Example 5] A nonaqueous electrolyte storage element of Reference Example 5 was obtained in the same manner as Reference Example 4 except that solid natural graphite (porosity: 0.49%) was used as the negative electrode active material instead of the hollow natural graphite.

[0118] (Initial charge and discharge) For each non-aqueous electrolyte storage element of Reference Examples 4 and 5, initial charge and discharge were performed according to the following procedures. After constant current charging at 25°C with a current of 0.2C to 4.1V, constant voltage charging was performed at 4.1V. The end condition of charging was set until the charging current reached 0.01C. After a 10-minute rest period after charging, constant current discharge was performed at 25°C with a current of 0.2C to 2.75V. A 10-minute rest period was set after discharging.

[0119] (Evaluation: Low temperature DCR) For each non-aqueous electrolyte storage element of reference examples 4 and 5 after the above-mentioned initial charge and discharge, constant current charging was performed at 25°C with a current of 1.0C to make the SOC 50%. After being stored in a thermostatic chamber at -10°C for 4 hours, the elements were discharged at current values ​​of 0.2C, 0.5C or 1.0C for 30 seconds respectively. After each discharge was completed, constant current charging was performed at a current of 1.0C to make the SOC 50%. The relationship between the current value in each discharge and the voltage at the tenth second after the start of the discharge was plotted, and the low-temperature direct current resistance (low-temperature DCR) was calculated based on the slope of the straight line obtained by plotting the three points. The calculated low-temperature DCR is shown in Table 2.

[0120] (Evaluation: Capacity retention rate after charge and discharge cycles) For each non-aqueous electrolyte storage element of Reference Examples 4 and 5 after the above-mentioned initial charge and discharge, a charge and discharge cycle test was performed according to the following procedures. Constant current and constant voltage charging was performed at 25°C with a charging current of 1C and a charge end voltage of 4.1V. The charge end condition was set until the charging current reached 0.01C. After a 10-minute rest after charging, constant current discharge was performed at 25°C with a discharge current of 1C and a discharge end voltage of 2.75V. The discharge capacity obtained under this condition was used as the discharge capacity before the charge and discharge cycle. Then, at 60°C, the charge condition was set to a charging current of 4C and a charge end voltage of 4.0V, and the discharge condition was set to a discharge current of 4C and a discharge end voltage of 3.4V, and a charge and discharge cycle test was performed. A 10-minute rest was set after charging and discharging. The charge and discharge were performed for 11430 cycles. Then, constant current and constant voltage charging was performed at 25°C with a charging current of 1C and a charge end voltage of 4.1V. The charge end condition was set until the charging current reached 0.01C. After charging, a 10-minute rest period was set, and then constant current discharge was performed at 25°C with a discharge current of 1C and a discharge end voltage of 2.75V. The obtained discharge capacity was taken as the discharge capacity after the charge and discharge cycle. The percentage of the discharge capacity after the charge and discharge cycle relative to the discharge capacity before the charge and discharge cycle was taken as the capacity retention rate after the charge and discharge cycle. The obtained capacity retention rate is shown in Table 2.

[0121] [Table 2]

[0122] As shown in Table 1, when comparing Comparative Example 1 and Example 1, in which solid graphite is used as the negative electrode active material, the non-aqueous electrolyte storage element of Example 1, in which the non-aqueous electrolyte contains the compound represented by formula (1), has a lower low-temperature DCR than the non-aqueous electrolyte storage element of Comparative Example 1, in which the non-aqueous electrolyte does not contain the compound represented by formula (1). Furthermore, in the non-aqueous electrolyte storage element of Example 2, in which the non-aqueous electrolyte contains the compound represented by formula (1) and the difluorophosphate, the low-temperature DCR is further reduced. On the other hand, when comparing Reference Example 1 and Reference Example 2, in which hollow graphite is used as the negative electrode active material, the non-aqueous electrolyte storage element of Reference Example 2, in which the non-aqueous electrolyte contains the compound represented by formula (1), has a higher low-temperature DCR than the non-aqueous electrolyte storage element of Reference Example 1, in which the non-aqueous electrolyte does not contain the compound represented by formula (1). It can be confirmed that the effect of reducing the low-temperature DCR of the non-aqueous electrolyte storage element by containing the compound represented by formula (1) in the non-aqueous electrolyte is a unique effect produced when solid graphite is used as the negative electrode active material. In addition, as in Reference Example 3, in a non-aqueous electrolyte storage element using hollow graphite as the negative electrode active material, when the non-aqueous electrolyte contains a compound represented by formula (1) and a difluorophosphate, the low-temperature DCR is reduced, but the effect is smaller than that of Example 2.

[0123] In addition, as shown in Table 2, it can be seen that when the non-aqueous electrolyte does not contain the compound represented by formula (1), the non-aqueous electrolyte storage element of Reference Example 5 using solid graphite as the negative electrode active material has a good capacity retention rate after charge and discharge cycles, but a high low-temperature DCR, compared with the non-aqueous electrolyte storage element of Reference Example 4 using hollow graphite as the negative electrode active material.

[0124] The present invention can be applied to power storage elements used as power sources for electronic devices such as personal computers and communication terminals, and automobiles. Description of Reference Numerals

[0125] 1: non-aqueous electrolyte storage element, 2: electrode body, 3: container, 4: positive electrode terminal, 41: positive electrode lead, 5: negative electrode terminal, 51: negative electrode lead, 20: storage unit, 30: storage device.

Claims

1. A non-aqueous electrolyte storage element comprising a negative electrode and a non-aqueous electrolyte, The negative electrode has a negative electrode active material including solid graphite, The nonaqueous electrolyte includes a compound represented by the following formula (1): [Chemistry 1] In formula (1), R 1 and R 2 are each independently a hydrogen atom or a hydrocarbon group, and R 1 and R 2 The total number of carbon atoms is 3 or less.

2. The nonaqueous electrolyte storage element according to claim 1, wherein The nonaqueous electrolyte further includes a difluorophosphate.

3. The nonaqueous electrolyte storage element according to claim 1 or 2, wherein: In a cross-sectional SEM image of the negative electrode, an area ratio of the solid graphite relative to an area occupied by the negative electrode active material is greater than 50%.

4. The nonaqueous electrolyte storage element according to claim 1 or 2, wherein The solid graphite is natural graphite.

5. The nonaqueous electrolyte storage element according to claim 1 or 2, wherein: In the cross section of the solid graphite particle observed in an SEM image obtained using a scanning electron microscope (SEM), the void ratio, which is an area ratio of voids in the particle to the area of ​​the entire particle, is 0.01% to 0.5%.

6. The nonaqueous electrolyte storage element according to claim 1 or 2, wherein: The content of the compound represented by the formula (1) in the nonaqueous electrolyte is greater than 0 mass % and 5 mass % or less.

Citation Information

Patent Citations

  • Negative electrode for power storage device, and power storage device

    JP2017069039A