Hydrocracking catalyst as well as preparation method and application thereof

By using a combination of composite acidic material support and modified Y molecular sieve and ZSM-22 molecular sieve, the conversion performance of hydrocracking catalysts to polycyclic cyclic hydrocarbons and long-chain hydrocarbons is improved, and the existing catalysts are solved in the production of API Class III base oils The problem of large loss of viscosity index is that the generated base oil has high isomer hydrocarbon content and low polycyclic cyclic hydrocarbon content, which is suitable as a high-quality isomerial dewaxing raw material.

CN119016098APending Publication Date: 2024-11-26CHINA NAT OFFSHORE OIL CORP +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310606761.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

When the existing hydrocracking catalysts produce API III base oils with low viscosity and high viscosity index, it is difficult to effectively convert polycyclic cyclic hydrocarbons and long-chain alkanes, resulting in large losses in the viscosity index of the base oil, and the catalysts for long-chain hydrocarbons. Insufficient heterogeneous performance.

Method used

Using composite acidic material support, including phthalidaeite powder, amorphous silicon-aluminum powder and composite molecular sieve, the combination of modified Y molecular sieve and ZSM-22 molecular sieve is used to serve as the acidic material support of the catalyst, and secondary pores are added through calcination treatment to promote The ring-opening of polycyclic cyclic hydrocarbons and the isomerization of long-chain hydrocarbons improve the activity and selectivity of the catalyst.

Benefits of technology

The generated hydrogenated base oil has a high isomeric hydrocarbon content and a low polycyclic cyclic hydrocarbon content. It is suitable as a high-quality raw material for isomeric dewaxed units, which improves the viscosity index and yield of the base oil and reduces the isomeric decoagulation process. loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004250825100000161
    Figure BDA0004250825100000161
  • Figure BDA0004250825100000171
    Figure BDA0004250825100000171
Patent Text Reader

Abstract

The present invention provides a hydrocracking catalyst and a preparation method and application thereof, the hydrocracking catalyst comprises a composite acidic material carrier and a metal oxide active component loaded on the surface of the composite acidic material carrier, the composite acidic material carrier comprises pseudo-boehmite powder, amorphous silica-alumina powder and a composite molecular sieve, the composite molecular sieve comprises a ZSM-22 molecular sieve and a modified Y molecular sieve, the catalyst provided by the invention has high ring-opening activity on polycyclic naphthenic hydrocarbon and good isomerization performance on paraffin, and the obtained hydrogenated base oil has the characteristics of high isoparaffin content and low polycyclic naphthenic hydrocarbon content, and is high-quality isomerization dewaxing raw oil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation, and relates to a hydrocracking catalyst and a preparation method and application thereof. Background Art

[0002] The increasing requirements for energy conservation and environmental protection and the need to improve engine performance will continue to drive the development of the global base oil market. Automotive lubricant base oils are shifting towards low-viscosity, high-viscosity index API III base oils. The full hydrogenation process is the main process technology for producing API III base oils, including three process units: hydrocracking-isomerization dewaxing-hydrogenation refining. The hydrocracking unit mainly undergoes desulfurization, denitrogenation, aromatic saturation, polycyclic cycloalkanes ring opening, and paraffin isomerization reactions, which determine the feed properties of the isomerization dewaxing unit and have an important impact on the viscosity index, viscosity, and yield of the base oil in the entire process.

[0003] Cycloalkanes and chain alkanes are two key components of base oils. The efficient conversion of polycyclic cycloalkanes and long carbon chain alkanes is the key to producing API Class III base oils, which can significantly improve the properties of base oils. The ring-opening cracking of polycyclic cycloalkanes determines the properties and selectivity of base oils, and the structure of chain alkanes has an important influence on the viscosity index and pour point of base oils. The structure and composition of chain alkanes in hydrocracking products have a significant effect on the viscosity index loss of the isomerization depressant unit: the viscosity index of the base oil products produced by isomerization depressant from two hydrocracking products with the same viscosity index and chain alkanes content differs by 8 units. Among them, the hydrocracking products with a higher ratio of isoparaffin carbon content to normal paraffin carbon content have a higher viscosity index of the base oil products obtained by isomerization depressant. This shows that the higher the content of isomerized chain alkanes in the isomerization depressant feedstock, the smaller the viscosity index loss of the base oil after isomerization depressant. In the past, the research and development of hydrocracking catalysts at home and abroad focused on strengthening the ring-opening performance of catalysts, but paid little attention to the conversion of long-chain alkanes by catalysts. In the hydrocracking unit, in response to the production needs of low-viscosity and high-viscosity index API III base oils, high-performance hydrocracking catalysts are studied and developed to improve the cracking ring-opening performance of catalysts for polycyclic cycloalkanes and the isomerization performance for long-chain alkanes, providing high-quality raw materials for the isomerization depressant unit.

[0004] The ring-opening cracking of polycyclic cycloalkanes and the isomerization of long-chain alkanes are two types of reactions, and the requirements for acidity are different. For the ring-opening cracking of polycyclic cycloalkanes, amorphous silica-alumina and Y molecular sieve are the two main acidic materials. When used as a carrier in practice, they are often modified according to the needs of the reaction to maximize the target product. In the hydrocracking section, one of the main chemical reactions for improving the viscosity index of lubricating base oil is the hydro-ring-opening cracking of polycyclic aromatic hydrocarbons and the selective ring-opening of polycyclic cycloalkanes. For Y molecular sieve, since the molecules of polycyclic aromatic hydrocarbons and polycyclic cycloalkanes with side chains are larger, they exceed the micropore pore size of Y molecular sieve and will not be able to enter the micropores for reaction. Y molecular sieve is used as a carrier for hydrocracking of lubricating base oil, and the selection and modification of molecular sieves are very critical: on the one hand, the acidity should be adjusted to improve the selectivity of selective ring opening, and on the other hand, the micropore volume should be reduced to reduce the probability of cracking of paraffins.

[0005] CN103551186A discloses a medium oil type hydrocracking catalyst and a preparation method thereof, wherein the active ingredient is amorphous SiO2-Al2O3 as a carrier and a composite molecular sieve as an acidic component, and the composite molecular sieve includes a modified Y molecular sieve and a modified ZSM-23 molecular sieve. The modified Y molecular sieve has been deeply dealuminated and has the characteristics of high crystallinity, large specific surface area, high silicon-aluminum ratio, small unit cell constant, rich secondary pores, low acid center density, and high proportion of medium-strength acid centers. The modified ZSM-23 molecular sieve has unobstructed pores, a small number of acid centers, and outstanding isomerization performance, and is suitable for use as a medium oil type hydrocracking catalyst.

[0006] CN107344109A discloses a hydrocracking catalyst for producing high-quality hydrocracking tail oil and a preparation method thereof. The catalyst uses a modified Y / ZSM-48 composite molecular sieve as an acidic component, and the catalyst has the characteristics of high hydrocracking activity and good isomerization performance. The composite of modified Y / ZSM-48 in the invention is firstly to add unsaturated olefins in an inert gas to roast the Y molecular sieve to form carbon deposits, and then to perform a desiliconization treatment, and then, the modified Y molecular sieve is added to the template solution system for synthesizing ZSM-48 for crystallization treatment, which is a complex process and high cost. Summary of the invention

[0007] The object of the present invention is to provide a hydrocracking catalyst and a preparation method and application thereof. The catalyst of the present invention has high ring-opening activity for polycyclic cycloalkanes and good isomerization performance for paraffins. The obtained hydrogenated base oil has the characteristics of high isoparaffin content and low polycyclic cycloalkanes content, and is a high-quality isomerized dewaxing raw oil.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a hydrocracking catalyst, which comprises a composite acidic material carrier and a metal oxide active component loaded on the surface of the composite acidic material carrier, wherein the composite acidic material carrier comprises pseudo-boehmite powder, amorphous silica-alumina powder and a composite molecular sieve, and the composite molecular sieve comprises a ZSM-22 molecular sieve and a modified Y molecular sieve.

[0010] The present invention adopts different types of acidic materials as carriers in view of the reaction characteristics of base oil hydrocracking, can provide suitable reaction channels and acidic centers for different types of reaction molecules, is suitable for the hydrocracking process of various vacuum wax oils, and the generated oil has low polycyclic cycloalkanes content and high isoparaffins content.

[0011] The modified Y molecular sieve of the present invention has more secondary pores than the traditional Y molecular sieve, which promotes the cracking and ring opening of polycyclic cycloalkanes. Mixing it with the ZSM-22 molecular sieve with more regular pores to obtain a composite molecular sieve is beneficial to improving the isomerization selectivity of long-chain alkanes.

[0012] Preferably, the mass ratio of the pseudo-boehmite powder, amorphous silica-alumina powder and composite molecular sieve is (30-40):40:(20-30), for example: 30:40:30, 35:40:25, 32:40:28, 38:40:22 or 40:40:20, etc.

[0013] Preferably, the surface area of ​​the pseudo-boehmite powder is 180 to 360 m 2 / g, for example: 180m 2 / g, 200m 2 / g, 250m 2 / g、300m 2 / g or 360m 2 / g, etc., preferably 220 to 300 m 2 / g.

[0014] Preferably, the pore volume of the pseudo-boehmite powder is 0.4 to 1.2 mL / g, for example, 0.4 mL / g, 0.5 mL / g, 0.8 mL / g, 1 mL / g or 1.2 mL / g, etc., preferably 0.85 to 1.10 mL / g.

[0015] Preferably, the Na2O weight content of the pseudo-boehmite powder is ≤0.1%.

[0016] Preferably, the SO4 2- Weight content ≤2.0%.

[0017] Preferably, the weight content of SiO2 in the amorphous silicon aluminum powder is 20-50%, for example: 20%, 25%, 30%, 40% or 50%, etc., preferably 30-45%.

[0018] Preferably, the pore volume of the amorphous silicon aluminum powder is 0.8 to 1.0 mL / g, for example, 0.8 mL / g, 0.85 mL / g, 0.9 mL / g, 0.95 mL / g or 1.0 mL / g.

[0019] Preferably, the specific surface area of ​​the amorphous silicon aluminum powder is 400 to 600 m 2 / g, for example: 400m 2 / g, 450m 2 / g、500m 2 / g, 550m 2 / g or 600m 2 / g, etc.

[0020] Preferably, the mass ratio of the ZSM-22 molecular sieve to the modified Y molecular sieve is 2:8 to 5:5, for example, 2:8, 3:7, 4:6 or 5:5.

[0021] Preferably, the molar ratio of SiO2 / Al2O3 in the ZSM-22 molecular sieve is 50 to 70:1, for example, 50:1, 55:1, 60:1, 65:1 or 70:1.

[0022] Preferably, the relative crystallinity of the ZSM-22 molecular sieve is ≥80%.

[0023] Preferably, the specific surface area of ​​the ZSM-22 molecular sieve is 150 to 350 m 2 / g, for example: 150m 2 / g, 180m 2 / g, 200m 2 / g, 250m 2 / g、300m 2 / g or 350m 2 / g, etc.

[0024] Preferably, the pore volume of the ZSM-22 molecular sieve is 0.15 to 0.35 mL / g, for example, 0.15 mL / g, 0.2 mL / g, 0.25 mL / g, 0.3 mL / g or 0.35 mL / g.

[0025] Preferably, the unit cell constant of the Y molecular sieve is 2.425-2.445 nm, for example, 2.425 nm, 2.430 nm, 2.435 nm, 2.440 nm or 2.445 nm.

[0026] Preferably, the relative crystallinity of the Y molecular sieve is 45.2-75.3%, for example, 45.2%, 50%, 55%, 60% or 75.3%.

[0027] Preferably, the specific surface area of ​​the Y molecular sieve is 350 to 600 m 2 / g, for example: 350m 2 / g, 400m 2 / g, 450m 2 / g、500m 2 / g or 600m 2 / g, etc.

[0028] Preferably, the weight content of Na2O in the Y molecular sieve is ≤0.1%.

[0029] Preferably, the metal oxide active component comprises at least one Group VIII metal oxide and at least one Group VIB metal oxide.

[0030] Preferably, the Group VIII metal oxide comprises nickel oxide and / or cobalt oxide.

[0031] Preferably, the VIB Group metal oxide includes tungsten oxide and / or molybdenum oxide.

[0032] Preferably, based on 100% of the mass of the hydrocracking catalyst, the mass fraction of the Group VIII metal oxide is 2-7%, for example, 2%, 3%, 4%, 5%, 6% or 7%.

[0033] Preferably, the mass fraction of the VIB group metal oxide is 16-32%, for example, 16%, 20%, 25%, 30% or 32%.

[0034] Preferably, the modified Y molecular sieve is prepared by calcining the Y molecular sieve in an air atmosphere.

[0035] According to the reaction characteristics of polycyclic cycloalkanes and long-chain alkanes in VGO raw materials, the invention modifies the Y molecular sieve, increases secondary pores, promotes the cracking and ring opening of polycyclic cycloalkanes, does not require dealumination, and has a simple process.

[0036] Preferably, the unit cell constant of the molecular sieve is 2.451-2.472 nm, for example, 2.451 nm, 2.455 nm, 2.46 nm, 2.465 nm or 2.472 nm.

[0037] Preferably, the molecular sieve has a Na2O weight content of ≤0.1%.

[0038] Preferably, the ratio of the volume of air introduced to the mass of the Y molecular sieve is 10 to 100 L / (kg·min), for example: 10 L / (kg·min), 20 L / (kg·min), 50 L / (kg·min), 80 L / (kg·min) or 100 L / (kg·min), etc.

[0039] Preferably, the calcination temperature is 750-1050°C, for example, 750°C, 800°C, 900°C, 1000°C or 1050°C.

[0040] Preferably, the calcination treatment time is 1 to 6 hours, for example: 1 hour, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.

[0041] In a second aspect, the present invention provides a method for preparing the hydrocracking catalyst as described in the first aspect, the preparation method comprising the following steps:

[0042] (1) Pseudo-boehmite powder, amorphous silica-alumina powder, modified Y molecular sieve, ZSM-22 molecular sieve, an extrusion aid, a peptizing agent and water are rolled and mixed, and then molded, dried and calcined to obtain a composite acidic material carrier;

[0043] (2) The composite acidic material carrier is impregnated in an active metal component impregnation solution, and the hydrocracking catalyst is obtained after drying and activation.

[0044] Preferably, the peptizing agent in step (1) comprises any one of nitric acid, acetic acid or citric acid, or a combination of at least two of them.

[0045] Preferably, the extrusion aid in step (1) includes sesbania powder and / or cellulose.

[0046] Preferably, the forming method includes any one of extrusion, sheeting or ball rolling, or a combination of at least two of them, preferably extrusion.

[0047] Preferably, the drying temperature is 80-180°C, for example, 80°C, 100°C, 120°C, 150°C or 180°C, etc., preferably 110-150°C.

[0048] Preferably, the drying time is 6 to 12 hours, for example, 6 hours, 7 hours, 8 hours, 10 hours or 12 hours.

[0049] Preferably, the calcination temperature is 500-700°C, for example, 500°C, 550°C, 600°C, 650°C or 700°C.

[0050] Preferably, the calcination time is 2 to 6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.

[0051] Preferably, the drying temperature in step (2) is 80-180°C, for example, 80°C, 100°C, 120°C, 150°C or 180°C, etc., preferably 110-150°C.

[0052] Preferably, the drying time is 6 to 12 hours, for example, 6 hours, 7 hours, 8 hours, 10 hours or 12 hours.

[0053] Preferably, the activation temperature is 250-450°C, for example, 250°C, 300°C, 350°C, 400°C or 450°C.

[0054] Preferably, the activation time is 2 to 6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.

[0055] In a third aspect, the present invention provides a use of the hydrocracking catalyst as described in the first aspect, wherein the hydrocracking catalyst is used for hydrocracking of vacuum distillate oil to produce lubricating oil base oil.

[0056] Before use, the hydrocracking catalyst of the present invention can be pre-sulfurized with hydrogen sulfide or sulfur-containing raw materials in the presence of hydrogen at a temperature of 140-370°C. This pre-sulfurization can be carried out outside the vessel or in situ inside the vessel to convert it into a sulfide type.

[0057] The hydrocracking catalyst of the present invention is mainly used for hydrocracking of vacuum distillate oil (VGO) and / or light deasphalted oil to produce lubricating oil base oil. The vacuum distillate oil can be, for example, various vacuum distillate oils of a refinery, such as one or more of vacuum first-line oil, vacuum second-line oil, vacuum third-line oil and vacuum fourth-line oil. The light deasphalted oil can be obtained by contacting the vacuum distillate oil with a deasphalting solvent for solvent deasphalting.

[0058] Preferably, the hydrogen partial pressure of the hydrocracking is 8 to 20 MPa, for example, 8 MPa, 10 MPa, 12 MPa, 15 MPa or 20 MPa.

[0059] Preferably, the reaction temperature of the hydrocracking is 320-410°C, for example, 320°C, 350°C, 380°C, 400°C or 410°C.

[0060] Preferably, the hydrogen-to-oil volume ratio of the hydrocracking is 800-2000:1, for example, 800:1, 1000:1, 1200:1, 1500:1 or 2000:1, etc.

[0061] Preferably, the liquid hourly volume space velocity of the hydrocracking is 0.4 to 1.8 h -1 , for example: 0.4h -1 , 0.6h -1 , 1h-1 , 1.5h -1 or 1.8h -1 wait.

[0062] Compared with the prior art, the present invention has the following beneficial effects:

[0063] (1) The present invention adopts different types of acidic materials as carriers according to the reaction characteristics of base oil hydrocracking, which can provide suitable reaction channels and acidic centers for different types of reaction molecules. It is suitable for the hydrocracking process of various vacuum wax oils, and the generated oil has a low content of polycyclic cycloalkanes and a high content of isoparaffins.

[0064] (2) The catalyst-generated oil of the present invention can be distilled under reduced pressure to obtain a fraction with a temperature of ≥350°C with a yield of 82% or more, a cycloalkane content of ≥3 rings can be less than 5.5%, and an IP / NP ratio can be greater than 0.62. DETAILED DESCRIPTION

[0065] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0066] Example 1

[0067] This embodiment provides a hydrocracking catalyst, and the preparation method of the hydrocracking catalyst is as follows:

[0068] (1) 150 g of pseudo-boehmite powder, 200 g of amorphous silicon aluminum powder, 75 g of modified Y molecular sieve and 75 g of ZSM-22 molecular sieve, an extrusion aid, a peptizing agent, water, etc. were mixed uniformly, fully rolled and mixed, and then formed, and then dried at 80° C. for 12 h and calcined at 500° C. for 6 h to obtain a carrier;

[0069] (2) preparing a metal impregnation solution of Ni and Mo, impregnating the support obtained in step (1), and then drying at 150° C. for 4 h and activating at 250° C. for 6 h to obtain the hydrocracking catalyst of the present invention, numbered SSC-1. The mass fraction of nickel oxide in the hydrocracking catalyst is 4%, and the mass fraction of molybdenum oxide is 24%.

[0070] The preparation conditions of the modified Y molecular sieve in step (1) are as follows: weigh a Y molecular sieve with a unit cell constant of 2.472 nm, place it in an air-permeable calcining furnace and calcine it at 1050° C. in a dry air atmosphere for 1 h. The modified Y molecular sieve is numbered as MY-1 with a unit cell constant of 2.425 nm, a relative crystallinity of 45.1%, and a specific surface area of ​​350 m 2 / g.

[0071] Example 2

[0072] This embodiment provides a hydrocracking catalyst, and the preparation method of the hydrocracking catalyst is as follows:

[0073] (1) 150 g of pseudo-boehmite powder, 200 g of amorphous silica-alumina powder, 100 g of modified Y molecular sieve, 50 g of ZSM-22 molecular sieve, an extrusion aid, a peptizing agent, water, etc. were mixed evenly, fully rolled and mixed, and then formed, and then dried at 110° C. for 8 h and calcined at 550° C. for 5 h to obtain a carrier.

[0074] (2) preparing a metal impregnation solution of Ni and W, impregnating the support obtained in step (1), and then drying at 120° C. for 6 h and activating at 300° C. for 5 h to obtain the hydrocracking catalyst of the present invention, numbered SSC-2. The mass fraction of nickel oxide in the hydrocracking catalyst is 5.5%, and the mass fraction of tungsten oxide is 30%.

[0075] The preparation conditions of the modified Y molecular sieve in step (1) are as follows: weigh a Y molecular sieve with a unit cell constant of 2.451 nm, place it in an air-permeable calcining furnace at 950° C. in a dry air atmosphere for 2 h, and number it as MY-2: unit cell constant 2.429 nm, relative crystallinity 49.6%, specific surface area 435 m 2 / g.

[0076] Example 3

[0077] This embodiment provides a hydrocracking catalyst, and the preparation method of the hydrocracking catalyst is as follows:

[0078] (1) 150 g of pseudo-boehmite powder, 200 g of amorphous silica-alumina powder, 120 g of modified Y molecular sieve, 30 g of ZSM-22 molecular sieve, an extrusion aid, a peptizing agent, water, etc. are mixed evenly, fully rolled and mixed to form, and then dried at 120° C. for 6 h and calcined at 600° C. for 4 h to obtain a carrier.

[0079] (2) preparing a metal impregnation solution of Co and Mo, impregnating the support obtained in step (1), and then drying at 110° C. for 8 h and activating at 350° C. for 4 h to obtain the hydrocracking catalyst of the present invention, numbered SSC-3. The mass fraction of cobalt oxide in the hydrocracking catalyst is 4.6%, and the mass fraction of molybdenum oxide is 23%.

[0080] The preparation conditions of the modified Y molecular sieve in step (1) are as follows: weigh a Y molecular sieve with a unit cell constant of 2.458 nm, place it in an air-permeable calcining furnace and calcine it at 1000° C. in a dry air atmosphere for 1 h. The modified Y molecular sieve is numbered MY-3 with a unit cell constant of 2.428 nm, a relative crystallinity of 47.2%, and a specific surface area of ​​378 m 2 / g.

[0081] Example 4

[0082] This embodiment provides a hydrocracking catalyst, and the preparation method of the hydrocracking catalyst is as follows:

[0083] (1) 175 g of pseudo-boehmite powder, 200 g of amorphous silica-alumina powder, 62.5 g of modified Y molecular sieve and 62.5 g of ZSM-22 molecular sieve, an extrusion aid, a peptizing agent, water, etc. were mixed evenly, fully rolled and mixed to form, and then dried at 150° C. for 4 h and calcined at 650° C. for 3 h to obtain a carrier.

[0084] (2) preparing a metal impregnation solution of Ni and Mo, impregnating the support obtained in step (1), and then drying at 80° C. for 12 h and activating at 400° C. for 3 h to obtain the hydrocracking catalyst of the present invention, numbered SSC-4. The mass fraction of nickel oxide in the hydrocracking catalyst is 4%, and the mass fraction of tungsten oxide is 25%.

[0085] The preparation conditions of the modified Y molecular sieve in step (1) are as follows: weigh a Y molecular sieve with a unit cell constant of 2.467 nm, place it in an air-permeable calcining furnace at 850° C. in a dry air atmosphere for 3 h, and number it as MY-4: unit cell constant 2.438 nm, relative crystallinity 65.3%, specific surface area 547 m 2 / g.

[0086] Example 5

[0087] This embodiment provides a hydrocracking catalyst, and the preparation method of the hydrocracking catalyst is as follows:

[0088] (1) 175 g of pseudo-boehmite powder, 200 g of amorphous silica-alumina powder, 85 g of modified Y molecular sieve, 40 g of ZSM-22 molecular sieve, an extrusion aid, a peptizing agent, water, etc. are mixed evenly, fully rolled and mixed, and then formed, and then dried at 150° C. for 4 h and calcined at 700° C. for 2 h to obtain a carrier.

[0089] (2) preparing a metal impregnation solution of Ni and W, impregnating the support obtained in step (1), and then drying at 150° C. for 4 h and activating at 450° C. for 2 h to obtain the hydrocracking catalyst of the present invention, numbered SSC-5. The mass fraction of nickel oxide in the hydrocracking catalyst is 2.5%, and the mass fraction of tungsten oxide is 25%.

[0090] The preparation conditions of the modified Y molecular sieve in step (1) are as follows: weigh a Y molecular sieve with a unit cell constant of 2.463 nm, place it in an air-permeable calcining furnace at 900° C. in a dry air atmosphere for 3 h, and number it as MY-5: unit cell constant 2.432 nm, relative crystallinity 53.6%, specific surface area 524 m 2 / g.

[0091] Example 6

[0092] This embodiment provides a hydrocracking catalyst, and the preparation method of the hydrocracking catalyst is as follows:

[0093] (1) 175 g of pseudo-boehmite powder, 200 g of amorphous silica-alumina powder, 100 g of modified Y molecular sieve, 25 g of ZSM-22 molecular sieve, an extrusion aid, a peptizing agent, water, etc. were mixed evenly, fully rolled and mixed, and then formed, and then dried at 120° C. for 6 h and calcined at 700° C. for 2 h to obtain a carrier.

[0094] (2) preparing a metal impregnation solution of Co and Mo, impregnating the support obtained in step (1), and then drying at 120° C. for 6 h and activating at 450° C. for 2 h to obtain the hydrocracking catalyst of the present invention, numbered SSC-6. The mass fraction of cobalt oxide in the hydrocracking catalyst is 3.6%, and the mass fraction of molybdenum oxide is 18%.

[0095] The preparation conditions of the modified Y molecular sieve in step (1) are as follows: weigh a Y molecular sieve with a unit cell constant of 2.467 nm, place it in an air-permeable calcining furnace at 950° C. in a dry air atmosphere for 2 h, and number it as MY-6: unit cell constant 2.428 nm, relative crystallinity 48.7%, specific surface area 424 m 2 / g.

[0096] Example 7

[0097] This embodiment provides a hydrocracking catalyst, and the preparation method of the hydrocracking catalyst is as follows:

[0098] (1) 200 g of pseudo-boehmite powder, 200 g of amorphous silica-alumina powder, 50 g of modified Y molecular sieve and 50 g of ZSM-22 molecular sieve, an extrusion aid, a peptizing agent, water, etc. were mixed evenly, fully rolled and mixed, and then formed, and then dried at 110° C. for 8 h and calcined at 650° C. for 3 h to obtain a carrier.

[0099] (2) preparing a metal impregnation solution of Ni and Mo, impregnating the support obtained in step (1), and then drying at 110° C. for 8 h and activating at 350° C. for 4 h to obtain the hydrocracking catalyst of the present invention, numbered SSC-7. The mass fraction of nickel oxide in the hydrocracking catalyst is 4.6%, and the mass fraction of molybdenum oxide is 23%.

[0100] The preparation conditions of the modified Y molecular sieve in step (1) are as follows: weigh a Y molecular sieve with a unit cell constant of 2.458 nm, place it in an air-permeable calcining furnace at 850° C. in a dry air atmosphere for 4 h, and number it as MY-7: unit cell constant 2.424 nm, relative crystallinity 67.4%, specific surface area 509 m 2 / g.

[0101] Example 8

[0102] This embodiment provides a hydrocracking catalyst, and the preparation method of the hydrocracking catalyst is as follows:

[0103] (1) 200 g of pseudo-boehmite powder, 200 g of amorphous silica-alumina powder, 70 g of modified Y molecular sieve, 30 g of ZSM-22 molecular sieve, an extrusion aid, a peptizing agent, water, etc. are mixed evenly, fully rolled and mixed to form, and then dried at 120° C. for 6 h and calcined at 600° C. for 4 h to obtain a carrier.

[0104] (2) preparing a metal impregnation solution of Ni and W, impregnating the support obtained in step (1), and then drying at 80° C. for 12 h and activating at 300° C. for 5 h to obtain the hydrocracking catalyst of the present invention, numbered SSC-8. The mass fraction of nickel oxide in the hydrocracking catalyst is 4%, and the mass fraction of tungsten oxide is 30%.

[0105] The preparation conditions of the modified Y molecular sieve in step (1) are as follows: weigh a Y molecular sieve with a unit cell constant of 2.472 nm, place it in an air-permeable calcining furnace at 700° C. in a dry air atmosphere for 6 h, and number it as MY-8: unit cell constant 2.445 nm, relative crystallinity 73.7%, specific surface area 600 m 2 / g.

[0106] Example 9

[0107] This embodiment provides a hydrocracking catalyst, and the preparation method of the hydrocracking catalyst is as follows:

[0108] (1) 200 g of pseudo-boehmite powder, 200 g of amorphous silica-alumina powder, 80 g of modified Y molecular sieve, 20 g of ZSM-22 molecular sieve, an extrusion aid, a peptizing agent, water, etc. are mixed evenly, fully rolled and mixed to form, and then dried at 150° C. for 4 h and calcined at 600° C. for 4 h to obtain a carrier.

[0109] (2) preparing a metal impregnation solution of Co and Mo, impregnating the support obtained in step (1), and then drying at 150° C. for 4 hours and activating at 350° C. for 4 hours to obtain the hydrocracking catalyst of the present invention, numbered SSC-9. The mass fraction of cobalt oxide in the hydrocracking catalyst is 5.5%, and the mass fraction of molybdenum oxide is 23%.

[0110] The preparation conditions of the modified Y molecular sieve in step (1) are as follows: weigh a Y molecular sieve with a unit cell constant of 2.463 nm, place it in an air-permeable calcining furnace at 800° C. in a dry air atmosphere for 5 h, and number it as MY-9: unit cell constant 2.441 nm, relative crystallinity 71.5%, specific surface area 572 m 2 / g.

[0111] Example 10

[0112] The only difference between this embodiment and embodiment 1 is that the mass ratio of ZSM-22 molecular sieve to modified Y molecular sieve is 6:4, and other conditions and parameters are exactly the same as those in embodiment 1.

[0113] Embodiment 11

[0114] The only difference between this embodiment and embodiment 1 is that the mass ratio of ZSM-22 molecular sieve to modified Y molecular sieve is 1:9, and other conditions and parameters are exactly the same as those in embodiment 1.

[0115] Example 12

[0116] The only difference between this embodiment and embodiment 1 is that the mass fraction of nickel oxide is 1%, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0117] Embodiment 13

[0118] The only difference between this embodiment and embodiment 1 is that the mass fraction of nickel oxide is 10%, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0119] Embodiment 14

[0120] The only difference between this embodiment and embodiment 1 is that the mass fraction of molybdenum oxide is 15%, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0121] Embodiment 15

[0122] The only difference between this embodiment and embodiment 1 is that the mass fraction of molybdenum oxide is 35%, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0123] Comparative Example 1

[0124] This comparative example provides a hydrocracking catalyst, and the preparation method of the hydrocracking catalyst is as follows:

[0125] (1) 200 g of pseudo-boehmite powder, 200 g of amorphous silica-alumina powder, 50 g of Y molecular sieve (unit cell constant is 2.458 nm, unmodified), 50 g of ZSM-22 molecular sieve, an extrusion aid, a peptizing agent, water, etc. are mixed evenly, fully rolled and mixed, and then formed, and then dried at 110° C. for 8 h and calcined at 650° C. for 3 h to obtain a carrier.

[0126] (2) preparing a metal impregnation solution of Ni and Mo, impregnating the support obtained in step (1), and then drying at 110° C. for 8 h and activating at 350° C. for 4 h to obtain a hydrocracking catalyst of the present invention, numbered DBC-1. The mass fraction of nickel oxide in the hydrocracking catalyst is 4.6%, and the mass fraction of molybdenum oxide is 23%.

[0127] Comparative Example 2

[0128] This comparative example adopts Example 6 of CN103551186A to prepare a catalyst, which is numbered as DBC-2. The mass fraction of nickel oxide in the hydrocracking catalyst is 4.4%, and the mass fraction of molybdenum oxide is 20.3%.

[0129] Performance Test:

[0130] The catalyst performance evaluation is carried out on a medium-sized hydrogenation unit. Before the activity evaluation, the catalyst is first sulfurized to convert the active metal into a sulfurized state to form an active center. The present invention uses the ratio of isoparaffin carbon content IP to normal alkane carbon content NP IP / NP to indicate the isoparaffin content in the base oil. The larger the ratio, the higher the isoparaffin content. When evaluating the hydrocracking catalyst, the raw oil first passes through the hydrorefining catalyst bed R1 and then enters the hydrocracking catalyst bed R2. Raw oil property table 1:

[0131] Table 1

[0132] 100℃ 6.713 80℃ 10.70 Viscosity Index 118 <![CDATA[Density (20 °C) / (g / cm 3 )]]> 0.8611 Pour point / ℃ 48 Sulfur mass fraction / (μg / g) 1051 Nitrogen mass fraction / (μg / g) 756 Aromatics mass fraction / % 17.0 IBP / 10% 324 / 383 30% / 50% 429 / 470 70% / 90% 499 / 521 95% / FBP 530 / 553

[0133] Evaluation process conditions are shown in Table 2:

[0134] Table 2

[0135] Hydrogen partial pressure / MPa 13.0 <![CDATA[Air speed (R1 / R2) / h -1 > 1.0 / 1.5 Hydrogen to oil volume ratio 1000 Reaction temperature / ℃ 385

[0136] The generated oil was subjected to vacuum distillation and the fractions ≥350°C were collected for analysis. The results are shown in Table 3:

[0137] Table 3

[0138]

[0139]

[0140] As can be seen from Table 3, from Examples 1-9, the catalyst generated oil of the present invention can be obtained by vacuum distillation to collect the ≥350°C fraction yield of more than 92%, the ≥3-ring cycloalkanes content can be less than 5.5%, and the IP / NP can be more than 0.62.

[0141] By comparing Example 1 with Examples 10-11, it can be seen that in the hydrocracking catalyst of the present invention, the mass ratio of the ZSM-22 molecular sieve and the modified Y molecular sieve will affect its performance. When the mass ratio of the ZSM-22 molecular sieve and the modified Y molecular sieve is controlled at 2:8 to 5:5, the performance of the hydrocracking catalyst is better. If the proportion of the ZSM-22 molecular sieve is too high, the ring-opening cracking performance of the catalyst for polycyclic cycloalkanes will be weakened, and the content of polycyclic cycloalkanes in the product will increase. If the proportion of the ZSM-22 molecular sieve is too low, the degree of isomerization of the paraffin molecules in the product will be low, and the ratio of isomerized hydrocarbons to paraffins will decrease.

[0142] By comparing Example 1 with Examples 12-13, it can be seen that in the hydrocracking catalyst of the present invention, the mass fraction of the Group VIII metal oxide will affect its performance. When the mass fraction of the Group VIII metal oxide is controlled at 2-7%, the performance of the hydrocracking catalyst is better. If the mass fraction of the Group VIII metal oxide is too high or too low, the ring-opening cracking selectivity of the catalyst for polycyclic cycloalkanes will decrease, the product yield will decrease, and the viscosity index will decrease.

[0143] By comparing Example 1 with Examples 14-15, it can be seen that in the hydrocracking catalyst of the present invention, the mass fraction of the VIB Group metal oxide will affect its performance. When the mass fraction of the VIB Group metal oxide is controlled at 16-32%, the performance of the hydrocracking catalyst is better. If the mass fraction of the VIB Group metal oxide is too high, it will block the pores of part of the catalyst, reduce the accessibility of part of the acid center, reduce the ring-opening performance of the catalyst, reduce the viscosity index of the product, and increase the content of polycyclic cycloalkanes. If the mass fraction of the VIB Group metal oxide is too low, it will reduce the hydrogenation performance of the catalyst, resulting in a decrease in the ring-opening cracking performance and selectivity of the catalyst, a decrease in the viscosity index of the product, and a decrease in the yield.

[0144] By comparing the embodiments and the comparative examples, it can be obtained that, compared with the comparative example catalyst, the catalyst of the present invention has a higher yield of the fraction ≥350°C of the generated oil than the comparative example catalyst, a lower content of cycloalkanes with ≥3 rings than the comparative example catalyst, and a ratio of the isoalkane carbon content to the normal alkane carbon content IP / NP greater than that of the comparative example catalyst, indicating that the hydrocracking catalyst of the present invention has better base oil fraction selectivity, stronger ring-opening ability for polycyclic cycloalkanes, and higher isomerization performance for normal alkanes in the feedstock oil, and the generated oil is a high-quality feedstock for the isomerization dewaxing unit.

[0145] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A hydrocracking catalyst, characterized in that: The hydrocracking catalyst comprises a composite acidic material carrier and a metal oxide active component loaded on the surface of the composite acidic material carrier, wherein the composite acidic material carrier comprises pseudo-boehmite powder, amorphous silica-alumina powder and a composite molecular sieve, and the composite molecular sieve comprises a ZSM-22 molecular sieve and a modified Y molecular sieve.

2. The hydrocracking catalyst according to claim 1, characterized in that The mass ratio of the pseudo-boehmite powder, the amorphous silica-alumina powder and the composite molecular sieve is (30-40):40:(20-30); Preferably, the surface area of ​​the pseudo-boehmite powder is 180 to 360 m 2 / g, preferably 220 to 300 m 2 / g; Preferably, the pore volume of the pseudo-boehmite powder is 0.4 to 1.2 mL / g, preferably 0.85 to 1.10 mL / g; Preferably, the Na2O weight content of the pseudo-boehmite powder is ≤0.1%; Preferably, the SO4 2- Weight content ≤ 2.0%; Preferably, the SiO2 weight content in the amorphous silicon aluminum powder is 20 to 50%, preferably 30 to 45%; Preferably, the pore volume of the amorphous silicon aluminum powder is 0.8 to 1.0 mL / g; Preferably, the specific surface area of ​​the amorphous silicon aluminum powder is 400 to 600 m 2 / g.

3. The hydrocracking catalyst according to claim 1 or 2, characterized in that The mass ratio of the ZSM-22 molecular sieve to the modified Y molecular sieve is 2:8 to 5:5; Preferably, the molar ratio of SiO2 / Al2O3 in the ZSM-22 molecular sieve is 50 to 70:1; Preferably, the relative crystallinity of the ZSM-22 molecular sieve is ≥80%; Preferably, the specific surface area of ​​the ZSM-22 molecular sieve is 150 to 350 m 2 / g; Preferably, the pore volume of the ZSM-22 molecular sieve is 0.15 to 0.35 mL / g; Preferably, the unit cell constant of the Y molecular sieve is 2.425 to 2.445 nm; Preferably, the relative crystallinity of the Y molecular sieve is 45.2-75.3%; Preferably, the specific surface area of ​​the Y molecular sieve is 350 to 600 m 2 / g; Preferably, the weight content of Na2O in the Y molecular sieve is ≤0.1%.

4. The hydrocracking catalyst according to any one of claims 1 to 3, characterized in that The metal oxide active component includes at least one Group VIII metal oxide and at least one Group VIB metal oxide; Preferably, the Group VIII metal oxide comprises nickel oxide and / or cobalt oxide; Preferably, the VIB group metal element includes tungsten oxide and / or molybdenum oxide; Preferably, based on 100% of the mass of the hydrocracking catalyst, the mass fraction of the Group VIII metal oxide is 2 to 7%; Preferably, the mass fraction of the VIB group metal oxide is 16-32%.

5. The hydrocracking catalyst according to any one of claims 1 to 4, characterized in that The modified Y molecular sieve is prepared by calcining the Y molecular sieve in an air atmosphere; Preferably, the unit cell constant of the molecular sieve is 2.451 to 2.472 nm; Preferably, the molecular sieve has a Na2O weight content of ≤0.1%; Preferably, the ratio of the volume of air introduced to the mass of the Y molecular sieve is 10 to 100 L / (kg·min); Preferably, the calcination temperature is 750-1050°C; Preferably, the calcination treatment time is 1 to 6 hours.

6. A method for preparing the hydrocracking catalyst according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) Pseudo-boehmite powder, amorphous silica-alumina powder, modified Y molecular sieve, ZSM-22 molecular sieve, an extrusion aid, a peptizing agent and water are rolled and mixed, and then molded, dried and calcined to obtain a composite acidic material carrier; (2) The composite acidic material carrier is impregnated in an active metal component impregnation solution, and the hydrocracking catalyst is obtained after drying and activation.

7. The preparation method according to claim 6, characterized in that: The peptizing agent in step (1) comprises any one of nitric acid, acetic acid or citric acid or a combination of at least two thereof; Preferably, the extrusion aid includes sesbania powder and / or cellulose.

8. The preparation method according to claim 6 or 7, characterized in that: The forming method in step (1) includes any one of extrusion, sheeting or ball rolling, or a combination of at least two of them, preferably extrusion; Preferably, the drying temperature is 80 to 180°C, preferably 110 to 150°C; Preferably, the drying time is 6 to 12 hours; Preferably, the calcination temperature is 500-700°C; Preferably, the calcination time is 2 to 6 hours.

9. The preparation method according to any one of claims 6 to 8, characterized in that: The drying temperature in step (2) is 80 to 180° C., preferably 110 to 150° C.; Preferably, the drying time is 6 to 12 hours; Preferably, the activation temperature is 250-450°C; Preferably, the activation time is 2 to 6 hours.

10. Use of the hydrocracking catalyst according to any one of claims 1 to 5, characterized in that: The hydrocracking catalyst is used for producing lubricating oil base oil by hydrocracking of vacuum distillate oil; Preferably, the hydrogen partial pressure of the hydrocracking is 8 to 20 MPa; Preferably, the reaction temperature of the hydrocracking is 320-410°C; Preferably, the hydrogen to oil volume ratio of the hydrocracking is 800 to 2000:1; Preferably, the liquid hourly volume space velocity of the hydrocracking is 0.4 to 1.8 h -1 .

Citation Information

Patent Citations

  • Composite molecular sieve-containing medium oil type hydrocracking catalyst, preparation method and application thereof

    CN103551186A

  • Hydrocracking catalyst for producing high-quality hydrocracking tail oil and preparation method of hydrocracking catalyst

    CN107344109A