A combined depressant for low basicity zinc-sulfur sulfide ore flotation separation
The selective separation of zinc-sulfide ores was achieved under low alkalinity conditions by using a combination of lime and o-phenanthroline inhibitors. This solved the problems of mud formation and foaming caused by using lime at high alkalinity, reduced lime consumption and improved recovery rate, and realized green and environmentally friendly separation of zinc-sulfide ores.
Patent Information
- Application Number
- CN202411256081.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-09-09
AI Technical Summary
Existing technologies for separating zinc-sulfide ores suffer from problems such as mud formation, foam sticking, equipment corrosion, environmental pollution, and impact on the recovery of rare and precious metals due to the use of lime with high alkalinity. Furthermore, inorganic inhibitors are toxic, while organic inhibitors are costly and difficult to control.
A combination of lime and o-phenanthroline as a depressant was used in the flotation of zinc-sulfur sulfide ores under low alkalinity conditions. Through the complexation reaction of o-phenanthroline with the surface of pyrite, the amount of lime used was reduced and the collection effect of butyl xanthate on sphalerite was enhanced, thus achieving selective separation.
The system achieves efficient separation of zinc and sulfur sulfide ores under low alkalinity, reduces lime usage by 60-80%, solves environmental pollution and equipment problems caused by high alkalinity, improves recovery rate and reduces processing costs.
Smart Images

Figure CN119016186B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a combined depressant for the flotation separation of low-alkalinity zinc-sulfide ores, belonging to the field of mineral processing technology. Background Technology
[0002] Sphalerite is one of the main sources of zinc; however, pyrite often occurs in association with sphalerite, and the two are usually separated by flotation.
[0003] Lime, with its low cost and good inhibition effect, is often used as a pyrite inhibitor in zinc-sulfur separation. Although the high-alkali process has a good effect, it also brings a series of problems: (1) When the mineral has a high mud content, the use of a large amount of lime leads to severe mudification during the flotation process, sticky flotation foam, more impurities, and poor concentrate quality, which makes it difficult to stabilize the production process. (2) The use of a large amount of lime leads to easy slurry agglomeration, which causes blockage of transportation pipelines, corrosion of equipment, increased maintenance costs, and unnecessary economic losses. (3) The high-alkali environment affects the recovery of associated rare and precious metals such as Au, Ag, Ge, and In. In addition, pyrite inhibited by high alkali is difficult to activate. (4) The addition of a large amount of lime leads to a large amount of calcium ions and a high pH value in the mineral processing wastewater, causing environmental pollution and high water treatment costs. Therefore, the research on efficient pyrite inhibitors and sphalerite collectors has become one of the current hot issues.
[0004] In recent years, inhibitors for pyrite have been extensively studied, and they are further divided into inorganic and organic inhibitors. Inorganic inhibitors mainly consist of cyanide, lime, sulfur oxides, and some oxidants, but these inhibitors often involve large dosages, toxicity, and serious environmental pollution. Organic inhibitors mainly include dextrin, modified starch, humic acids, tannic acid, and lignin. Organic inhibitors are effective in small dosages, but they are costly and difficult to control during production.
[0005] Under the aforementioned conditions, the separation of sphalerite and pyrite mostly requires the use of copper sulfate as an activator for sphalerite, which increases beneficiation costs. Therefore, it is essential to find a selective and environmentally friendly pyrite inhibitor that can achieve the separation of sphalerite and pyrite without the use of copper sulfate as an activator. Summary of the Invention
[0006] To address the shortcomings of existing technologies, one objective of this invention is to provide a novel combined inhibitor that requires a small dosage, is environmentally friendly, and has strong adaptability to solve the aforementioned problems. This combined inhibitor is used to suppress pyrite in the flotation separation of zinc-sulfur ore under low-alkali conditions, with minimal impact on the flotation of sphalerite. Compared to "high-alkali sulfur suppression," this method reduces lime usage by approximately 60-80%, resolving a series of problems associated with "high-alkali sulfur suppression." Furthermore, the inhibitor of this invention is environmentally friendly, requires a small dosage, and has strong applicability.
[0007] The combined inhibitor of the present invention is lime and o-phenanthroline, and the mass ratio of the two is (5~20):3. The combined inhibitor is a pyrite inhibitor used for the flotation separation of sphalerite and pyrite.
[0008] One of the combination inhibitors of this invention is o-phenanthroline, whose structural formula is as follows:
[0009] A second objective of this invention is to provide an application of the inhibitor in the flotation separation of zinc-sulfide ores under low-alkali conditions, the specific steps of which are as follows:
[0010] (1) After the minerals to be selected are slurried, a combination inhibitor, butyl xanthate and No. 2 oil are added in sequence to carry out zinc roughing to obtain zinc roughing concentrate and roughing tailings;
[0011] (2) The rough tailings obtained in step (1) are subjected to two scavenging processes. Collector and No. 2 oil are added before each scavenging process, and the scavenging concentrate is returned to the previous stage in sequence to form a closed loop. The final zinc tailings are obtained after two scavenging processes.
[0012] (3) The zinc rough concentrate obtained in step (1) is subjected to two fine treatments. A combined inhibitor is added in each fine treatment. The tailings of each fine treatment are returned to the previous stage to form a closed loop. The final zinc concentrate is obtained after two fine treatments.
[0013] In step (1), the raw ore is slurry adjusted to a slurry concentration of 30-35%, the combined inhibitor dosage is 800-2300 g / t, the butyl xanthate dosage is 60-100 g / t, and the No. 2 oil dosage is 10-20 g / t.
[0014] The dosage of reagents for the two scavenging operations in step (2) is as follows: for scavenging operation 1, the dosage of butyl xanthate is 30~50 g / t and the dosage of No. 2 oil is 8~15 g / t; for scavenging operation 2, the dosage of butyl xanthate is 15~25 g / t and the dosage of No. 2 oil is 5~10 g / t.
[0015] The dosage of the reagents used in the two selection operations in step (3) are as follows: Selection 1, the dosage of the combined inhibitor is 400~1000 g / t, and Selection 2, the dosage of the combined inhibitor is 200~500 g / t.
[0016] Based on the above technical solutions, the advantages, principles, and beneficial effects of this invention are as follows:
[0017] This invention addresses the flotation separation process of zinc-sulfide ores by developing a combined depressant and flotation scheme. Under low alkalinity conditions, it achieves selective recovery of sphalerite and selective suppression of pyrite. When using this combined depressant in the separation of zinc-sulfide ores, the performance indicators remain stable. This combined depressant reduces lime usage by 60-80%, solves a series of problems caused by "high alkalinity sulfur suppression," and enables effective separation of zinc-sulfide ores under low alkalinity conditions.
[0018] The combined inhibitor of this invention comprises lime and o-phenanthroline, primarily utilizing the synergistic, highly efficient, and selective inhibition of pyrite by lime and o-phenanthroline. o-phenanthroline is a bidentate heterocyclic ligand with two nitrogen-containing functional groups, exhibiting strong chelating activity with metal ions, particularly Fe. 2+ Formation of stable [Fe(phen)3] 2+ Under weakly alkaline conditions, o-phenanthroline undergoes a complexation reaction with the surface of pyrite to form [Fe(phen)3]. 2+ Butyl xanthate adsorbs onto the surface of pyrite, hindering the interaction between butyl xanthate and the pyrite surface, thus inhibiting pyrite formation. However, the complexing ability of o-phenanthroline with zinc is much weaker than its complexing ability with iron. This results in less adsorption of o-phenanthroline on the sphalerite surface. Furthermore, the adsorption of a small amount of o-phenanthroline enhances the adsorption of butyl xanthate on the sphalerite surface, thereby strengthening the collecting effect of butyl xanthate on sphalerite and reducing the use of copper sulfate.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0020] (1) The inhibitor for low-alkali zinc-sulfur sulfide mineral flotation separation provided by the present invention can achieve green and efficient separation of sphalerite and pyrite at pH 7.5 to 10, solving a series of problems such as environmental pollution and foam adhesion caused by traditional "high-alkali sulfur suppression".
[0021] (2) The inhibitor used in this invention can chelate with dissolved metal ions, effectively reducing the cost of treating mineral processing wastewater. Attached Figure Description
[0022] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation
[0023] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the content described.
[0024] Example 1: The inhibitor used in this invention is a combination inhibitor, which is a combination of lime and o-phenanthroline, with a mass ratio of 5:3.
[0025] Application of the combined inhibitor in the flotation separation of low-alkalinity zinc-sulfide ores: In the lead-zinc sulfide ore tailings from a mine in Yunnan, the Zn grade was 1.37% and the S grade was 1.98%, with Zn mainly in sphalerite and S mainly in pyrite. Using this tailings as the target mineral, a flotation process of one rougher, two scavengers, and two cleaners was employed for separation. The process is as follows: Figure 1 As shown.
[0026] (1). Roughing operation: Add water to the above minerals to adjust the slurry to a mass concentration of 30%. Add 800 g / t of combined inhibitor (including 500 g / t of lime and 300 g / t of o-phenanthroline) and act for 3 min. At this time, the pH of the slurry is measured to be 7.5. Then add 60 g / t of butyl xanthate and act for 3 min. Finally, add 10 g / t of No. 2 oil and act for 2 min. After flotation for 4 min, zinc roughing concentrate and roughing tailings are obtained.
[0027] (2). Scavenging operation: Add 30 g / t of butyl xanthate to the roughing tailings and act for 3 min, then add 8 g / t of No. 2 oil and act for 2 min. After flotation for 3.5 min, the first scavenging concentrate and the first scavenging tailings are obtained. Return the first scavenging concentrate to the roughing operation. Add 15 g / t of butyl xanthate to the first scavenging tailings and act for 3 min, then add 5 g / t of No. 2 oil and act for 2 min. After flotation for 3 min, the second scavenging concentrate and the final zinc tailings are obtained. Then return the second scavenging concentrate to the first scavenging operation in sequence.
[0028] (3). Cleaning operation: Add 400 g / t (i.e., 250 g / t lime and 150 g / t o-phenanthroline) of depressant to the rougher concentrate for 3 min, and float for 3 min to obtain the first cleaned concentrate and the first cleaned tailings. Return the first cleaned tailings to the rougher, add 200 g / t (i.e., 125 g / t lime and 75 g / t o-phenanthroline) of depressant to the first cleaned concentrate for 3 min, and float for 2.5 min to obtain the second cleaned tailings and the final zinc concentrate. Then return the second cleaned tailings to the first cleaning operation.
[0029] The flotation reagent regime for the above flotation separation method is shown in Table 1, and the experimental results are shown in Table 2.
[0030] Comparative Example 1
[0031] Comparative Example 1 uses the above flotation process, except that the inhibitor will be entirely lime with the same dosage. The reagent formulation is shown in Table 1, and the experimental results are shown in Table 2.
[0032] Comparative Example 2
[0033] Comparative Example 2 still uses the above flotation process, but the difference is that the inhibitor will be entirely lime and the dosage will be changed. The reagent formulation is shown in Table 1, and the experimental results are shown in Table 2.
[0034] Table 1. Pharmaceutical formulations for Example 1, Comparative Example 1, and Comparative Example 2, in g / t.
[0035]
[0036] Table 2. Flotation test results of Example 1, Comparative Example 1 and Comparative Example 2
[0037]
[0038] The experimental results above show that under low alkalinity conditions, i.e., compared with Example 1 and Comparative Example 1, the absence of o-phenanthroline is insufficient to suppress pyrite, resulting in unsatisfactory concentrate indicators. Comparing Example 1 and Comparative Example 2 (which only added lime) at high alkalinity, the flotation results are similar, both effectively suppressing pyrite to achieve flotation separation of zinc-sulfide ores. However, Example 1 with o-phenanthroline added has an 84% lower lime content compared to Comparative Example 2 (which only added lime). The fact that a lower lime content still yields good flotation indicators indicates that this inhibitor is effective for the flotation separation of zinc-sulfide ores.
[0039] Example 2
[0040] A method for flotation separation of low-alkalinity zinc-sulfide ores, wherein the inhibitor is lime and o-phenanthroline in a mass ratio of 10:3.
[0041] In a lead-zinc sulfide ore in Inner Mongolia, the Pb grade is 1.89%, the Zn grade is 1.83%, and the S grade is 2.17%. After lead-preferential flotation, lead tailings with a Zn grade of 1.67% and an S grade of 2.04% were obtained. Using these tailings as the target minerals, a flotation process of one rougher, two scavengers, and two cleaners was employed for separation. The process is as follows: Figure 1 As shown.
[0042] (1). Roughing operation: Add water to the above-mentioned minerals to adjust the slurry to a mass concentration of 33%. Add 1300 g / t of inhibitor (including 1000 g / t of lime and 300 g / t of o-phenanthroline) and act for 3 min. At this time, the pH of the slurry is measured to be 8.8. Then add 80 g / t of butyl xanthate and act for 3 min. Finally, add 15 g / t of No. 2 oil and act for 2 min. After flotation for 4 min, zinc roughing concentrate and roughing tailings are obtained.
[0043] (2). Scavenging operation: Add 40 g / t butyl xanthate to the rougher tailings and react for 3 min, then add 10 g / t No. 2 oil and react for 2 min. After flotation for 3.5 min, the first scavenging concentrate and the first scavenging tailings are obtained. Return the first scavenging concentrate to the rougher, add 20 g / t butyl xanthate to the first scavenging tailings and react for 3 min, then add 8 g / t No. 2 oil and react for 2 min. After flotation for 3 min, the second scavenging concentrate and the final zinc tailings are obtained. Then, return the second scavenging concentrate to the first scavenging operation.
[0044] (3). Cleaning operation: Add 800 g / t (i.e., 615 g / t lime and 185 g / t o-phenanthroline) of depressant to the rougher concentrate for 3 min, and float for 3 min to obtain the first cleaned concentrate and the first cleaned tailings. Return the first cleaned tailings to the rougher, add 300 g / t (i.e., 230 g / t lime and 70 g / t o-phenanthroline) of depressant to the first cleaned concentrate for 3 min, and float for 2.5 min to obtain the second cleaned tailings and the final zinc concentrate. Then return the second cleaned tailings to the first cleaning operation.
[0045] The flotation reagent regime for the above flotation separation method is shown in Table 3, and the experimental results are shown in Table 4.
[0046] Comparative Example 3
[0047] Comparative Example 3 adopted the above flotation process, except that the inhibitor was entirely lime with the same dosage. The reagent formulation is shown in Table 3, and the experimental results are shown in Table 4.
[0048] Comparative Example 4
[0049] Comparative Example 4 still uses the above flotation process, but the difference is that the inhibitor will be entirely lime and the dosage will be changed. The reagent system is shown in Table 3, and the experimental results are shown in Table 4.
[0050] Table 3. Pharmaceutical formulations for Example 2, Comparative Example 3, and Comparative Example 4, in g / t.
[0051]
[0052] Table 4. Flotation test results of Example 2, Comparative Example 3 and Comparative Example 4
[0053]
[0054] The results above show that under low-alkali conditions, the addition of o-phenanthroline is beneficial for sulfur suppression, ensuring concentrate quality while also improving recovery rate. The flotation results of using o-phenanthroline as a depressant for pyrite under low-alkali conditions are slightly better than under high-alkali conditions. The addition of o-phenanthroline not only reduces lime consumption but also solves a series of problems associated with high alkali conditions in production, which is beneficial for improving economic efficiency.
[0055] Example 3
[0056] A method for flotation separation of low-alkalinity zinc-sulfide ores, wherein the inhibitor is lime and o-phenanthroline in a mass ratio of 20:3.
[0057] A copper-lead-zinc polymetallic sulfide ore in Yunnan Province, after copper-lead flotation and zinc-sulfur flotation, yielded a zinc-sulfur mixed concentrate with a Zn grade of 2.85% and a S grade of 6.21%. Using this zinc-sulfur concentrate as the target mineral, further processing was carried out... Figure 1 The flotation process shown here is for zinc and sulfur separation. The specific steps are as follows:
[0058] (1). Roughing operation: Add water to the above-mentioned minerals to adjust the slurry to a mass concentration of 35%. Add 2300 g / t of inhibitor (including 2000 g / t of lime and 300 g / t of o-phenanthroline) for 3 min. At this time, the pH of the slurry is measured to be 10. Then add 100 g / t of butyl xanthate for 3 min. Finally, add 20 g / t of No. 2 oil for 2 min. After flotation for 4 min, zinc roughing concentrate and roughing tailings are obtained.
[0059] (2) Scavenging operation: Add 50 g / t butyl xanthate to the rougher tailings and react for 3 min, then add 15 g / t No. 2 oil and react for 2 min. After flotation for 3.5 min, the first scavenging concentrate and the first scavenging tailings are obtained. Return the first scavenging concentrate to the rougher, add 25 g / t butyl xanthate to the first scavenging tailings and react for 3 min, then add 10 g / t No. 2 oil and react for 2 min. After flotation for 3 min, the second scavenging concentrate and the final zinc tailings are obtained. Then, return the second scavenging concentrate to the first scavenging operation.
[0060] (3) Cleaning operation: Add 1000 g / t (i.e., 870 g / t lime and 130 g / t o-phenanthroline) of depressant to the rougher concentrate for 3 min, and float for 3 min to obtain the first cleaned concentrate and the first cleaned tailings. Return the first cleaned tailings to the rougher, add 500 g / t (i.e., 385 g / t lime and 115 g / t o-phenanthroline) of depressant to the first cleaned concentrate for 3 min, and float for 2.5 min to obtain the second cleaned tailings and the final zinc concentrate. Then return the second cleaned tailings to the first cleaning operation in sequence.
[0061] The above flotation experimental reagent system is shown in Table 5, and the flotation results are shown in Table 6.
[0062] Comparative Example 5
[0063] Comparative Example 5 adopted the above flotation process, except that the inhibitor was entirely lime with the same dosage. The reagent formulation is shown in Table 5, and the experimental results are shown in Table 6.
[0064] Comparative Example 6
[0065] Comparative Example 6 still uses the above flotation process, but the difference is that the inhibitor will be entirely lime and the dosage will be changed. The reagent system is shown in Table 5, and the experimental results are shown in Table 6.
[0066] Table 5. Pharmaceutical formulations for Example 3, Comparative Example 5, and Comparative Example 6, in g / t.
[0067]
[0068] Table 6. Flotation test results of Example 3, Comparative Example 5 and Comparative Example 6
[0069]
[0070] The results above show that under low-alkali conditions, the addition of o-phenanthroline is beneficial for sulfur inhibition, ensuring concentrate quality while also improving recovery rate. The flotation results of using o-phenanthroline as a depressant for pyrite under low-alkali conditions are slightly better than under high-alkali conditions. This also indicates that using o-phenanthroline can not only reduce lime usage but also improve recovery rate while ensuring concentrate quality, thereby increasing production efficiency.
[0071] In summary, the results show that o-phenanthroline is beneficial for the flotation separation of zinc-sulfide ores, mainly in the following aspects: (1) o-phenanthroline is used at low alkalinity, reducing the amount of lime required; (2) o-phenanthroline does not require the addition of copper sulfate to activate sphalerite when separating zinc-sulfide ores, reducing reagent costs; (3) The use of o-phenanthroline solves the problems of severe mud formation and foam sticking caused by the use of large amounts of lime. These aspects are beneficial effects on the separation of zinc-sulfide ores. The combined inhibitor of this invention is stable, has good selective inhibition effect, requires small dosage, is safe to use, has strong adaptability, and has broad application prospects.
[0072] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention shall fall within the scope of the technical solution of the present invention.
Claims
1. A combined depressant for the flotation separation of low-alkalinity zinc-sulfide ores, characterized in that, The combined inhibitor is a combination of lime and o-phenanthroline, with a mass ratio of (5~20):
3. When separating zinc-sulfur sulfide ores with o-phenanthroline, it is not necessary to add copper sulfate to activate sphalerite. O-phenanthroline is a bidentate heterocyclic compound ligand with two nitrogen-containing functional groups, exhibiting a strong chelating effect with metal ions, particularly Fe. 2+ Formation of stable [Fe(phen)3] 2+ Under weakly alkaline conditions, o-phenanthroline undergoes a complexation reaction with the surface of pyrite to form [Fe(phen)3]. 2+ Adsorbed on the surface of pyrite, butyl xanthate inhibits the interaction between butyl xanthate and the pyrite surface, thus suppressing the pyrite. The complexing ability of o-phenanthroline with zinc is much weaker than its complexing ability with iron, which also results in less adsorption of o-phenanthroline on the surface of sphalerite. Furthermore, the adsorption of a small amount of o-phenanthroline enhances the adsorption of butyl xanthate on the surface of sphalerite, thereby strengthening the collecting effect of butyl xanthate on sphalerite and reducing the use of copper sulfate. One of the combination inhibitors is o-phenanthroline, whose structural formula is as follows: ; This combination of depressants is used to suppress pyrite, and the specific flotation separation steps are as follows: (1) After the minerals to be selected are slurried, a combination inhibitor, butyl xanthate and No. 2 oil are added in sequence to carry out zinc roughing to obtain zinc roughing concentrate and roughing tailings; (2) The rough tailings obtained in step (1) are subjected to two scavenging processes. Collector and No. 2 oil are added before each scavenging process, and the scavenging concentrate is returned to the previous stage in sequence to form a closed loop. The final zinc tailings are obtained after two scavenging processes. (3) The zinc rough concentrate obtained in step (1) is subjected to two fine treatments. A combined inhibitor is added in each fine treatment. The tailings of each fine treatment are returned to the previous stage to form a closed loop. The final zinc concentrate is obtained after two fine treatments. In step (1), the selected minerals are slurry adjusted to a slurry concentration of 30-35%, the combined inhibitor dosage is 800-2300 g / t, the butyl xanthate dosage is 60-100 g / t, and the No. 2 oil dosage is 10-20 g / t; The dosage of reagents for the two scavenging operations in step (2) is as follows: for scavenging operation 1, the dosage of butyl xanthate is 30~50 g / t and the dosage of No. 2 oil is 8~15 g / t; for scavenging operation 2, the dosage of butyl xanthate is 15~25 g / t and the dosage of No. 2 oil is 5~10 g / t.
2. The combined depressant for low-alkalinity zinc-sulfide ore flotation separation according to claim 1, characterized in that: The dosage of the reagents used in the two selection operations in step (3) are as follows: Selection 1, the dosage of the combined inhibitor is 400~1000 g / t, and Selection 2, the dosage of the combined inhibitor is 200~500 g / t.
Citation Information
Patent Citations
Inhibitor for zinc-sulfur sulfide ore flotation separation under low alkalinity and application of inhibitor
CN118341575A