Preparation method of high-purity tantalum powder

Through vacuum drying, activation and reduction treatment, high-purity tantalum powder was prepared, which solved the problems of high metal impurities, high oxygen content and high labor intensity in the prior art, and achieved high melting point and high pineapple of high purity tantalum powder The installation density meets the requirements of sputtering targets and reduces safety risks.

CN119016737APending Publication Date: 2024-11-26CONGHUA TANTALUM & NIOBIUM SMELTERY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411160953.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing tantalum powder preparation methods have problems such as high metal impurities, high oxygen content, low loose density, high labor intensity for workers and safety hazards.

Method used

A high-purity tantalum powder preparation method is adopted, including vacuum drying, activation, reduction tank mixing and stirring, water washing, pickling, drying and sintering, etc., switching tanks and handling are replaced by cantilever cranes to control temperature and pressure , wash with deionized water and mixed acid to ensure high purity and low impurity content of tantalum powder.

Benefits of technology

It has achieved low content of high-melting point metal impurities, low oxygen content and high loose density in high purity tantalum powder, meeting the requirements for sputtering targets, and reducing the labor intensity and safety risks of workers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016737A_ABST
    Figure CN119016737A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of high-purity tantalum powder. The preparation method comprises the following steps of S1, material preparation, S2, feeding, S3, vacuum activation and drying, S4, discharging, S5, canning, S6, argon filling and heating, S7, heating and stirring, S8, stirring for sodium reduction, S9, heat preservation, S10, cooling, S11, can opening, S12, leaching for sodium removal, S13, reduction product crushing, S14, water washing, S15, acid pickling, S16, acid washing and S17, drying. The preparation method has the beneficial effects that the tantalum powder prepared by adopting the preparation method disclosed by the invention is low in content of high-melting-point metal impurities W, Mo and Nb and common metal impurities, low in oxygen content and high in apparent density, and completely meets the requirements of high-apparent-density and high-purity tantalum powder for manufacturing sputtering target materials; and the cantilever crane is used for replacing manual operation for tank opening, closing and carrying, the labor intensity of workers is reduced, and the safety risk of the workers is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tantalum powder manufacturing, and in particular to a method for preparing high-purity tantalum powder. Background Art

[0002] Tantalum is a rare special material with excellent properties such as high melting point, corrosion resistance, good electrical and thermal conductivity, high chemical stability, and large dielectric constant of metal surface oxide film. However, the tantalum powder used in sputtering targets has extremely high purity requirements.

[0003] In the production process of tantalum powder, the traditional production method is: first activate potassium fluorotantalate at a temperature of 200-350℃, crush it into powder particles of uniform size to increase its surface activity and reduce the corrosion of free hydrofluoric acid carried by it to the activation tank and reduction tank and other equipment; heat the diluent to 100-350℃ and dry it to remove its moisture, then add it to the reduction tank in a certain proportion, and then hang the reduction tank into the reduction furnace to heat, melt and stir, and then inject liquid metal sodium for reduction. After the reduction is completed, the tank body is cooled, the material in the tank body is crushed and transported to the water washing process. After water washing, it is pickled, acid washed, dried, screened, vacuum heat treated, screened, mixed, and packaged to obtain metallurgical grade tantalum powder products.

[0004] Chinese patent CN103447544A provides a method for preparing high-purity tantalum powder with a centrally controlled particle size distribution. The method is to make the tantalum powder into a high-purity tantalum ingot, then hydrogenate it into powder, and dehydrogenate it into high-purity tantalum powder. The method has a long process and requires a lot of energy consumption. At the same time, hydrogen is used, which poses a safety hazard.

[0005] Chinese patent CN104148654A provides a method for preparing target-grade high-purity tantalum powder and Chinese patent CN114749655B provides a method for preparing high-purity tantalum powder and a method for preparing the same. Both methods require high-temperature treatment, and the subsequent treatment of the tantalum powder after high-temperature treatment is difficult. In addition, oxygen treatment is required, which increases costs and introduces new impurities such as magnesium.

[0006] Chinese patent CN110315088B provides a method for preparing coral-shaped high-purity tantalum powder. This method has a long production cycle. The injected liquid sodium is above the material. During the heating process, the sodium evaporates to the tank cover and cannot completely neutralize the acidic atmosphere of the reduction tank. The impurity content is still high. Summary of the invention

[0007] The purpose of the present invention is to overcome the problems of high metal impurities, high oxygen content, low bulk density, high labor intensity and danger of workers in the prior art, and to provide a method for preparing high-purity tantalum powder.

[0008] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0009] A method for preparing high-purity tantalum powder comprises the following steps:

[0010] S1. Material preparation: After cleaning the outer package of potassium fluorotantalate with compressed air, open the outer package of potassium fluorotantalate and add the potassium fluorotantalate into the potassium fluorotantalate raw material bin; after cleaning the outer package of diluent with compressed air, open the outer package of diluent and add the diluent into the diluent raw material bin;

[0011] S2, loading: using a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, starting the first bucket elevator to add the potassium fluorotantalate in the potassium fluorotantalate raw material bin to the first vacuum dryer, starting the second bucket elevator to add the diluent in the diluent raw material bin to the second vacuum dryer, and then using the cantilever crane to cover the covers of the first vacuum dryer and the second vacuum dryer respectively;

[0012] S3, vacuum activation and drying: start the first vacuum dryer to vacuum activate potassium fluorotantalate for 2-6 hours at a temperature of 250-350°C, a pressure of -0.1-0.08Mpa, and a speed of 3-8r / min, and start the second vacuum dryer to dry the diluent for 3-8 hours at a temperature of 120-180°C, a pressure of -0.1-0.08Mpa, and a speed of 3-8r / min;

[0013] S4, discharging: using a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, putting the potassium fluorotantalate vacuum-activated in the first vacuum dryer into the potassium fluorotantalate loading bin, putting the diluent dried in the second vacuum dryer into the diluent loading bin, and discharging the potassium fluorotantalate in the potassium fluorotantalate loading bin and the diluent in the diluent loading bin into the screw feeder at a weight ratio of potassium fluorotantalate to diluent of 1.5-3:1, the amount of potassium fluorotantalate is 100-400kg;

[0014] S5. Canning: Use a cantilever crane to open the cover of the reduction tank, mix potassium tantalate and diluent and add them into the reduction tank through a screw feeder, and cut 0.5-3 kg of sodium blocks into several pieces and evenly scatter them in the reduction tank. After canning is completed, use a cantilever crane to cover the cover of the reduction tank and drop the reduction tank into the reduction furnace, connect the cooling water pipe, argon pipe and sodium injection pipe of the reduction tank, and pass cooling water with a flow rate greater than 2 kg / min into the jacket of the reduction tank. Check whether the sensors on the reduction tank are normal;

[0015] S6, argon filling and heating: when the pressure is 0.05-0.08Mpa, start the vacuum pump to evacuate the reduction tank, and then fill the reduction tank with argon when the pressure is -0.1-0.08Mpa. After the vacuuming and argon filling cycles are repeated 1-2 times, the reduction tank is heated at a heating rate of 10-20℃ / min, and the reduction tank is continuously vacuumed until the temperature of the material in the reduction tank rises to 150℃. Then, the vacuuming and argon filling cycles are repeated once again. After the argon filling replacement, the pressure in the reduction tank is maintained between 0.02Mpa-0.1Mpa;

[0016] S7, heating and stirring: continue to heat the reduction tank at a heating rate of 10-20°C / min, and when the temperature in the reduction tank rises to 700-800°C, stir the stirring paddle at a stirring rate of 40-60r / min;

[0017] S8, stirring sodium reduction: continue to heat the reduction tank at a heating rate of 10-20°C / min, stop heating when the temperature in the reduction tank rises to 810-850°C, stir with a stirring paddle at a stirring rate of 60-100r / min, inject sodium into the reduction tank at a rate of 1-4kg / min, the amount of sodium injected is 30% of the weight of potassium fluorotantalate, and control the temperature in the reduction tank to be lower than 1100°C during the sodium injection;

[0018] S9, heat preservation: after the sodium injection is completed, the reduction tank is controlled to be kept at a temperature of 880-930°C for 0.5-2h, then the stirring paddle is stopped and lifted to the top of the inner side of the reduction tank;

[0019] S10, cooling: using a cantilever crane to lift the reduction tank out of the reduction furnace, starting the exhaust system to exhaust air until the temperature in the reduction tank is lower than 100°C and then stopping the exhaust;

[0020] S11, opening the tank: use a cantilever crane to lift the reduction tank to the furnace unloading room, start the waste gas collection system in the furnace unloading room, and then use the cantilever crane to open the tank cover of the reduction tank. At this time, the stirring paddle and the tank cover are lifted out together, and then the cantilever crane is used to pour the reduction product in the reduction tank into the leaching silo;

[0021] S12, elution and sodium removal: use a spray system to slowly spray deionized water into the elution silo to remove residual sodium in the reduction product;

[0022] S13, crushing the reduced product: start the jaw crusher, put the reduced product in the leaching silo into the jaw crusher, and crush it into product fragments with a particle size of less than 2 cm, which fall into the transfer vehicle;

[0023] S14, water washing: transferring the product fragments in the transfer vehicle into a water washing tank and washing them with cold deionized water and hot deionized water in sequence;

[0024] S15, pickling: transferring the washed product fragments to a pickling tank, and pickling the product fragments with a mixed acid for 4-12 hours;

[0025] S16, acid washing: transferring the product fragments after acid washing to a water washing tank, and using deionized water to wash away the mixed acid remaining on the product fragments;

[0026] S17, drying: the product fragments after acid washing are transferred to a drying box for drying, the dried product fragments are sieved, and the sieved material is sent to a vacuum heat treatment furnace for sintering at a temperature of 1050-1200° C. for 0.5-3 h to obtain tantalum powder.

[0027] Among them, the high melting point metal impurities W, Mo, and Nb in the potassium fluorotantalate in S1 are ≤1ppm.

[0028] Wherein, the diluent in S1 is sodium chloride or potassium chloride.

[0029] Among them, the second bucket elevator in S2 is blown clean with compressed air after completing the lifting operation.

[0030] Wherein, weight sensors for monitoring weight changes are respectively installed at the bottom of the potassium fluorotantalate loading bin and the bottom of the diluent loading bin.

[0031] Wherein, the insertion depth of the stirring paddle of the reduction tank is 1 / 3-1 / 2 of the height below the top surface of the material.

[0032] The specific process of water washing in S14 is as follows: first, use cold deionized water to wash away the metallic sodium, potassium tantalate, diluent, and reaction by-products in the product fragments, until the pH value of the washing liquid discharged from the washing tank is neutral, then use hot deionized water for washing, and stop using hot deionized water for washing until the conductivity of the washing liquid discharged from the washing tank is ≤60us / cm.

[0033] The mixed acid in S15 is formed by mixing 5%-20% nitric acid, 0.5-5% hydrogen peroxide, and 0.1%-1% hydrofluoric acid in equal volumes.

[0034] Wherein, the drying box in S17 is dried for 12-20 hours under the conditions of vacuum degree of -0.08Mpa and temperature of 80-120°C.

[0035] The beneficial effects of the present invention are as follows: the tantalum powder prepared by the preparation method of the present invention has low contents of high-melting-point metal impurities W, Mo, Nb and common metal impurities, low oxygen content and high bulk density, which fully meets the requirements of high-bulk ratio high-purity tantalum powder for manufacturing sputtering targets; a cantilever crane is used to replace manual work for opening and closing the tank and carrying work, thereby reducing the labor intensity of workers and reducing the safety risks of workers. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0037] Figure 1 is a flow chart of the preparation method of the present invention;

[0038] Figure 2 It is a schematic diagram of the structure of some devices used in the preparation method of the present invention;

[0039] Explanation of the numbers in the figure: potassium fluorotantalate raw material bin 1, diluent raw material bin 2, cantilever crane 3, first vacuum dryer 4, second vacuum dryer 5, first bucket elevator 6, second bucket elevator 7, potassium fluorotantalate loading bin 8, diluent loading bin 9, screw feeder 10, reduction tank 11, spray system 12, leaching bin 13, jaw crusher 14, transfer vehicle 15. DETAILED DESCRIPTION

[0040] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments.

[0041] like Figure 1 and Figure 2 As shown, a method for preparing high-purity tantalum powder comprises the following steps:

[0042] S1. Prepare materials: After cleaning the outer package of potassium fluorotantalate with compressed air, open the outer package of potassium fluorotantalate and add the potassium fluorotantalate into potassium fluorotantalate raw material bin 1. The high melting point metal impurities W, Mo, and Nb in potassium fluorotantalate are ≤1ppm. After cleaning the outer package of the diluent with compressed air, open the outer package of the diluent and add the diluent into the diluent raw material bin 2. The diluent is sodium chloride or potassium chloride.

[0043] S2, loading: use the cantilever crane 3 to open the covers of the first vacuum dryer 4 and the second vacuum dryer 5 respectively, start the first bucket elevator 6 to add the potassium fluorotantalate in the potassium fluorotantalate raw material bin into the first vacuum dryer 4, start the second bucket elevator 7 to add the diluent in the diluent raw material bin into the second vacuum dryer 5, and then use the cantilever crane 3 to cover the covers of the first vacuum dryer 4 and the second vacuum dryer 5 respectively; after the second bucket elevator 6 completes the lifting operation, use compressed air to blow it clean.

[0044] S3, vacuum activation and drying: start the first vacuum dryer to vacuum activate potassium fluorotantalate for 2-6 hours at a temperature of 250-350°C, a pressure of -0.1-0.08Mpa, and a speed of 3-8r / min, and start the second vacuum dryer to dry the diluent for 3-8 hours at a temperature of 120-180°C, a pressure of -0.1-0.08Mpa, and a speed of 3-8r / min;

[0045] S4, discharging: using the cantilever crane 3 to open the covers of the first vacuum dryer 4 and the second vacuum dryer 5 respectively, putting the potassium fluorotantalate vacuum-activated in the first vacuum dryer 4 into the potassium fluorotantalate loading bin 8, and putting the diluent dried in the second vacuum dryer 5 into the diluent loading bin 9; the potassium fluorotantalate in the potassium fluorotantalate loading bin 8 and the diluent in the diluent loading bin are discharged into the screw feeder 10 in a weight ratio of potassium fluorotantalate to diluent of 1.5-3:1, and the amount of potassium fluorotantalate is 100-400kg.

[0046] S5, canning: use the cantilever crane 3 to open the cover of the reduction tank 11, and add the potassium fluorotantalate and the diluent mixture into the reduction tank 11 through the screw feeder 10. At the same time, cut the 0.5-3 kg sodium block into several portions and evenly scatter them in the reduction tank 11. After the canning is completed, use the cantilever crane 3 to cover the cover of the reduction tank 11 and drop the reduction tank into the reduction furnace. Connect the cooling water pipe, argon pipe and sodium injection pipe of the reduction tank 11, and let the cooling water with a flow rate greater than 2 kg / min pass through the jacket of the reduction tank. Check whether the sensors on the reduction tank 11 are normal.

[0047] S6. Filling with argon and heating: When the pressure is 0.05-0.08Mpa, start the vacuum pump to evacuate the reduction tank, and then fill the reduction tank with argon when the pressure is -0.1-0.08Mpa. After repeating the vacuum pumping and argon filling cycle 1-2 times, heat the reduction tank at a heating rate of 10-20℃ / min, and continue to evacuate the reduction tank until the temperature of the material in the reduction tank rises to 150℃, then repeat the vacuum pumping and argon filling cycle once more, and keep the pressure in the reduction tank between 0.02Mpa-0.1Mpa after argon replacement.

[0048] S7. Heating and stirring: Continue to heat the reduction tank at a heating rate of 10-20°C / min. When the temperature in the reduction tank rises to 700-800°C, stir the agitator at a stirring rate of 40-60r / min.

[0049] S8. Stirring sodium reduction: continue to heat the reduction tank at a heating rate of 10-20°C / min. When the temperature in the reduction tank rises to 810-850°C, stop heating. Stir the agitator at a stirring rate of 60-100r / min. Add sodium to the reduction tank at a rate of 1-4kg / min. The amount of sodium added is 30% of the weight of potassium tantalate. When injecting sodium, control the temperature in the reduction tank to be lower than 1100°C.

[0050] S9. Insulation: After the sodium injection is completed, the reduction tank is kept at a temperature of 880-930°C for 0.5-2h, and then the stirring paddle is stopped and lifted to the top of the inner side of the reduction tank.

[0051] S10, cooling: Use a cantilever crane to lift the reduction tank out of the reduction furnace, start the exhaust system to exhaust air until the temperature in the reduction tank is lower than 100°C and then stop exhausting.

[0052] S11, opening the tank: using a cantilever crane to lift the reduction tank to the furnace unloading room, start the waste gas collection system in the furnace unloading room, and then use the cantilever crane to open the tank cover of the reduction tank. At this time, the stirring paddle and the tank cover are lifted out together, and then the cantilever crane is used to pour the reduction product in the reduction tank into the leaching silo 13.

[0053] S12, eluting to remove sodium: using the spray system 12 to slowly spray deionized water into the elution silo 13 to remove the residual sodium in the reduction product.

[0054] S13, crushing the reduced product: starting the jaw crusher, putting the reduced product in the leaching silo into the jaw crusher 14 and crushing it into product fragments with a particle size of less than 2 cm, which fall into the transfer vehicle 15.

[0055] S14, water washing: transfer the product fragments in the transfer vehicle into a water washing tank and wash them with cold deionized water and hot deionized water in turn. The specific process is: first use cold deionized water to wash away the metallic sodium, potassium tantalate, diluent, and reaction by-products in the product fragments, until the pH value of the washing liquid discharged from the washing tank is neutral, then switch to hot deionized water for washing, and stop washing with hot deionized water when the conductivity of the washing liquid discharged from the washing tank is ≤60us / cm.

[0056] S15, pickling: the washed product fragments are transferred to a pickling tank, and the product fragments are pickled for 4-12 hours using a mixed acid, wherein the mixed acid is a mixture of 5%-20% nitric acid, 0.5-5% hydrogen peroxide, and 0.1%-1% hydrofluoric acid in equal volumes.

[0057] S16, acid washing: the product fragments after acid washing are transferred to a water washing tank, and deionized water is used to wash away the mixed acid remaining on the product fragments.

[0058] S17, drying: the product fragments after acid washing are transferred to a drying box, and dried in the drying box at a vacuum degree of -0.08Mpa and a temperature of 80-120°C for 12-20h. The dried product fragments are sieved, and the sieved material is sent to a vacuum heat treatment furnace and sintered at a temperature of 1050-1200°C for 0.5-3h to obtain tantalum powder.

[0059] The first vacuum dryer and the second vacuum dryer are both rotary vacuum dryers.

[0060] In order to conveniently control the weight of potassium tantalate fluoroate and diluent discharged into the screw feeder, weight sensors for monitoring weight changes are respectively installed at the bottom of the potassium tantalate fluoroate loading bin and the bottom of the diluent loading bin.

[0061] The insertion depth of the agitator paddle of the reduction tank is 1 / 3-1 / 2 of the height below the top surface of the material.

[0062] When injecting sodium, the temperature in the reduction tank is controlled below 1100°C by evacuating the wall of the reduction tank and controlling the sodium injection speed.

[0063] Embodiment 1: A method for preparing high-purity tantalum powder comprises the following steps:

[0064] S1. Prepare materials: Use compressed air to clean the outer package of potassium fluorotantalate, open the outer package of potassium fluorotantalate and add the potassium fluorotantalate into the potassium fluorotantalate raw material bin. The high melting point metal impurities W, Mo, and Nb in potassium fluorotantalate are ≤1ppm. Use compressed air to clean the outer package of the diluent, open the outer package of the diluent and add the diluent into the diluent raw material bin. The diluent is sodium chloride.

[0065] S2. Loading: Use a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, start the first bucket elevator to add the potassium fluorotantalate in the potassium fluorotantalate raw material bin to the first vacuum dryer, start the second bucket elevator to add the diluent in the diluent raw material bin to the second vacuum dryer, and then use the cantilever crane to cover the covers of the first vacuum dryer and the second vacuum dryer respectively; after the second bucket elevator completes the lifting operation, use compressed air to blow it clean.

[0066] S3, vacuum activation and drying: start the first vacuum dryer to vacuum activate potassium tantalate at 320°C, -0.1Mpa, and 5r / min for 5 hours, and start the second vacuum dryer to dry the diluent at 150°C, -0.1Mpa, and 5r / min for 5 hours.

[0067] S4. Discharging: Use a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, put the potassium tantalate vacuum-activated in the first vacuum dryer into the potassium tantalate loading bin, and put the diluent dried in the second vacuum dryer into the diluent loading bin; discharge the potassium tantalate in the potassium tantalate loading bin and the diluent in the diluent loading bin into the screw feeder at a weight ratio of 2.5:1 between potassium tantalate and diluent, the amount of potassium tantalate is 200kg.

[0068] S5. Canning: Use a cantilever crane to open the cover of the reduction tank, mix potassium tantalate and diluent and add them into the reduction tank through a screw feeder, and cut 1 kg of sodium block into several portions and scatter them evenly in the reduction tank. After canning is completed, use a cantilever crane to cover the cover of the reduction tank and drop the reduction tank into the reduction furnace, connect the cooling water pipe, argon pipe and sodium injection pipe of the reduction tank, and pass cooling water with a flow rate greater than 2 kg / min into the jacket of the reduction tank. Check whether the sensors on the reduction tank are normal.

[0069] S6. Filling with argon and heating: When the pressure is 0.05-0.08Mpa, start the vacuum pump to evacuate the reduction tank, and then fill the reduction tank with argon when the pressure is -0.1-0.08Mpa. After repeating the vacuum pumping and argon filling cycle twice, heat the reduction tank at a heating rate of 15℃ / min. At the same time, continue to evacuate the reduction tank until the temperature of the material in the reduction tank rises to 150℃, and then repeat the vacuum pumping and argon filling cycle once again. After argon filling and replacement, the pressure in the reduction tank is maintained between 0.02Mpa-0.1Mpa.

[0070] S7. Heating and stirring: continue to heat the reduction tank at a heating rate of 15°C / min. When the temperature in the reduction tank rises to 800°C, the stirring paddle is stirred at a stirring rate of 60r / min.

[0071] S8. Stirring sodium reduction: continue to heat the reduction tank at a heating rate of 15°C / min. When the temperature in the reduction tank rises to 840°C, stop heating. Stir the agitator at a stirring rate of 80r / min. Add sodium to the reduction tank at a rate of 4kg / min. The amount of sodium added is 30% of the weight of potassium tantalate. When injecting sodium, control the temperature in the reduction tank to be lower than 1100°C.

[0072] S9. Insulation: After the sodium injection is completed, the reduction tank is kept at a temperature of 900°C for 1 hour, then the stirring paddle is stopped and lifted to the top of the inner side of the reduction tank.

[0073] S10, cooling: Use a cantilever crane to lift the reduction tank out of the reduction furnace, start the exhaust system to exhaust air until the temperature in the reduction tank is lower than 100°C and then stop exhausting.

[0074] S11, tank opening: Use a cantilever crane to lift the reduction tank to the furnace unloading room, start the waste gas collection system in the furnace unloading room, and then use the cantilever crane to open the tank cover of the reduction tank. At this time, the stirring paddle and the tank cover are lifted out together, and then the cantilever crane is used to pour the reduction product in the reduction tank into the leaching silo.

[0075] S12. Elution to remove sodium: Use a spray system to slowly spray deionized water into the elution silo to remove residual sodium in the reduction product.

[0076] S13, crushing the reduced product: start the jaw crusher, put the reduced product in the leaching silo into the jaw crusher and crush it into product fragments with a particle size less than 2 cm and fall into the transfer vehicle.

[0077] S14, water washing: transfer the product fragments in the transfer vehicle into a water washing tank and wash them with cold deionized water and hot deionized water in turn. The specific process is: first use cold deionized water to wash away the metallic sodium, potassium tantalate, diluent, and reaction by-products in the product fragments, until the pH value of the washing liquid discharged from the washing tank is neutral, then switch to hot deionized water for washing, and stop washing with hot deionized water when the conductivity of the washing liquid discharged from the washing tank is ≤60us / cm.

[0078] S15, pickling: the washed product fragments are transferred to a pickling tank, and the product fragments are pickled for 6 hours using a mixed acid, wherein the mixed acid is a mixture of 5%-20% nitric acid, 0.5-5% hydrogen peroxide, and 0.1%-1% hydrofluoric acid in equal volumes.

[0079] S16, acid washing: the product fragments after acid washing are transferred to a water washing tank, and deionized water is used to wash away the mixed acid remaining on the product fragments.

[0080] S17, drying: the product fragments after acid washing are transferred to a drying box, and dried in the drying box at a vacuum degree of -0.08Mpa and a temperature of 120°C for 15 hours. The dried product fragments are sieved, and the sieved materials are sent to a vacuum heat treatment furnace and sintered at a temperature of 1100°C for 1 hour to obtain tantalum powder 1.

[0081] Comparative Example 1: A method for preparing high-purity tantalum powder, comprising the following steps:

[0082] S1. Prepare materials: Use compressed air to clean the outer package of potassium fluorotantalate, open the outer package of potassium fluorotantalate and add the potassium fluorotantalate into the potassium fluorotantalate raw material bin. The high melting point metal impurities W, Mo, and Nb in potassium fluorotantalate are ≤1ppm. Use compressed air to clean the outer package of the diluent, open the outer package of the diluent and add the diluent into the diluent raw material bin. The diluent is sodium chloride.

[0083] S2. Loading: Use a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, start the first bucket elevator to add the potassium fluorotantalate in the potassium fluorotantalate raw material bin to the first vacuum dryer, start the second bucket elevator to add the diluent in the diluent raw material bin to the second vacuum dryer, and then use the cantilever crane to cover the covers of the first vacuum dryer and the second vacuum dryer respectively; after the second bucket elevator completes the lifting operation, use compressed air to blow it clean.

[0084] S3, vacuum activation and drying: start the first vacuum dryer to vacuum activate potassium tantalate at 320°C, -0.1Mpa, and 5r / min for 5 hours, and start the second vacuum dryer to dry the diluent at 150°C, -0.1Mpa, and 5r / min for 5 hours.

[0085] S4. Discharging: Use a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, put the potassium tantalate vacuum-activated in the first vacuum dryer into the potassium tantalate loading bin, and put the diluent dried in the second vacuum dryer into the diluent loading bin; discharge the potassium tantalate in the potassium tantalate loading bin and the diluent in the diluent loading bin into the screw feeder at a weight ratio of 2.5:1 between potassium tantalate and diluent, the amount of potassium tantalate is 200kg.

[0086] S5. Canning: Use a cantilever crane to open the cover of the reduction tank, mix potassium tantalate and diluent and add them into the reduction tank through a screw feeder, and cut 1 kg of sodium block into several portions and scatter them evenly in the reduction tank. After canning is completed, use a cantilever crane to cover the cover of the reduction tank and drop the reduction tank into the reduction furnace, connect the cooling water pipe, argon pipe and sodium injection pipe of the reduction tank, and pass cooling water with a flow rate greater than 2 kg / min into the jacket of the reduction tank. Check whether the sensors on the reduction tank are normal.

[0087] S6. Heating and stirring: The reduction tank is heated at a heating rate of 15°C / min. When the temperature in the reduction tank rises to 800°C, the stirring paddle is stirred at a stirring rate of 60r / min.

[0088] S7. Stirring sodium reduction: continue to heat the reduction tank at a heating rate of 15°C / min. When the temperature in the reduction tank rises to 840°C, stop heating. Stir the agitator at a stirring rate of 80r / min. Add sodium to the reduction tank at a rate of 4kg / min. The amount of sodium added is 30% of the weight of potassium tantalate. When injecting sodium, control the temperature in the reduction tank to be lower than 1100°C.

[0089] S8. Insulation: After the sodium injection is completed, the reduction tank is kept at a temperature of 900° C. for 1 hour, then the stirring paddle is stopped and lifted to the top of the inner side of the reduction tank.

[0090] S9. Cooling: Use a cantilever crane to lift the reduction tank out of the reduction furnace, start the exhaust system to exhaust air until the temperature in the reduction tank is lower than 100°C, and then stop exhausting air.

[0091] S10, opening the tank: use a cantilever crane to lift the reduction tank to the furnace unloading room, start the waste gas collection system in the furnace unloading room, and then use the cantilever crane to open the tank cover of the reduction tank. At this time, the stirring paddle and the tank cover are lifted out together, and then the cantilever crane is used to pour the reduction product in the reduction tank into the leaching silo.

[0092] S11. Elution to remove sodium: Use a spray system to slowly spray deionized water into the elution silo to remove residual sodium in the reduction product.

[0093] S12. Crushing the reduction product: start the jaw crusher, put the reduction product in the leaching silo into the jaw crusher and crush it into product fragments with a particle size less than 2 cm, which fall into the transfer vehicle.

[0094] S13, water washing: transfer the product fragments in the transfer vehicle into a water washing tank and wash them with cold deionized water and hot deionized water in turn. The specific process is: first use cold deionized water to wash away the metallic sodium, potassium tantalate, diluent, and reaction by-products in the product fragments, until the pH value of the washing liquid discharged from the washing tank is neutral, then use hot deionized water for washing, and stop using hot deionized water for washing when the conductivity of the washing liquid discharged from the washing tank is ≤60us / cm.

[0095] S14, pickling: the washed product fragments are transferred to a pickling tank, and the product fragments are pickled for 6 hours using a mixed acid, wherein the mixed acid is a mixture of 5%-20% nitric acid, 0.5-5% hydrogen peroxide, and 0.1%-1% hydrofluoric acid in equal volumes.

[0096] S15, acid washing: the product fragments after acid washing are transferred to a water washing tank, and deionized water is used to wash away the mixed acid remaining on the product fragments.

[0097] S16, drying: the product fragments after acid washing are transferred to a drying box, and dried in the drying box at a vacuum degree of -0.08Mpa and a temperature of 120°C for 15 hours. The dried product fragments are sieved, and the sieved materials are sent to a vacuum heat treatment furnace and sintered at a temperature of 1100°C for 1 hour to obtain tantalum powder II.

[0098] Comparative Example 2: A method for preparing high-purity tantalum powder, comprising the following steps:

[0099] S1. Prepare materials: Use compressed air to clean the outer package of potassium fluorotantalate, open the outer package of potassium fluorotantalate and add the potassium fluorotantalate into the potassium fluorotantalate raw material bin. The high melting point metal impurities W, Mo, and Nb in potassium fluorotantalate are ≤1ppm. Use compressed air to clean the outer package of the diluent, open the outer package of the diluent and add the diluent into the diluent raw material bin. The diluent is sodium chloride.

[0100] S2. Loading: Use a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, start the first bucket elevator to add the potassium fluorotantalate in the potassium fluorotantalate raw material bin to the first vacuum dryer, start the second bucket elevator to add the diluent in the diluent raw material bin to the second vacuum dryer, and then use the cantilever crane to cover the covers of the first vacuum dryer and the second vacuum dryer respectively; after the second bucket elevator completes the lifting operation, use compressed air to blow it clean.

[0101] S3, vacuum activation and drying: start the first vacuum dryer to vacuum activate potassium tantalate at 320°C, -0.1Mpa, and 5r / min for 5 hours, and start the second vacuum dryer to dry the diluent at 150°C, -0.1Mpa, and 5r / min for 5 hours.

[0102] S4. Discharging: Use a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, put the potassium tantalate vacuum-activated in the first vacuum dryer into the potassium tantalate loading bin, and put the diluent dried in the second vacuum dryer into the diluent loading bin; discharge the potassium tantalate in the potassium tantalate loading bin and the diluent in the diluent loading bin into the screw feeder at a weight ratio of 2.5:1 between potassium tantalate and diluent, the amount of potassium tantalate is 200kg.

[0103] S5. Canning: Use a cantilever crane to open the cover of the reduction tank, mix potassium tantalate and diluent and add them into the reduction tank through a screw feeder, and then place 1 kg of sodium block on the top of the potassium tantalate and diluent in the reduction tank. After the canning is completed, use a cantilever crane to cover the cover of the reduction tank and drop the reduction tank into the reduction furnace, connect the cooling water pipe, argon pipe and sodium injection pipe of the reduction tank, and pass cooling water with a flow rate greater than 2kg / min into the jacket of the reduction tank. Check whether the sensors on the reduction tank are normal.

[0104] S6. Filling with argon and heating: When the pressure is 0.05Mpa, start the vacuum pump to evacuate the reduction tank, and then fill the reduction tank with argon when the pressure is -0.1Mpa. After repeating the vacuum pumping and argon filling cycle twice, heat the reduction tank at a heating rate of 15℃ / min. At the same time, continue to evacuate the reduction tank until the temperature of the material in the reduction tank rises to 150℃, and then repeat the vacuum pumping and argon filling cycle once more. After argon filling and replacement, the pressure in the reduction tank is maintained between 0.02Mpa and 0.1Mpa.

[0105] S7. Heating and stirring: continue to heat the reduction tank at a heating rate of 15°C / min. When the temperature in the reduction tank rises to 800°C, the stirring paddle is stirred at a stirring rate of 60r / min.

[0106] S8. Stirring sodium reduction: continue to heat the reduction tank at a heating rate of 15°C / min. When the temperature in the reduction tank rises to 840°C, stop heating. Stir the agitator at a stirring rate of 80r / min. Add sodium to the reduction tank at a rate of 4kg / min. The amount of sodium added is 30% of the weight of potassium tantalate. When injecting sodium, control the temperature in the reduction tank to be lower than 1100°C.

[0107] S9. Insulation: After the sodium injection is completed, the reduction tank is kept at a temperature of 900°C for 1 hour, then the stirring paddle is stopped and lifted to the top of the inner side of the reduction tank.

[0108] S10, cooling: Use a cantilever crane to lift the reduction tank out of the reduction furnace, start the exhaust system to exhaust air until the temperature in the reduction tank is lower than 100°C and then stop exhausting.

[0109] S11, tank opening: Use a cantilever crane to lift the reduction tank to the furnace unloading room, start the waste gas collection system in the furnace unloading room, and then use the cantilever crane to open the tank cover of the reduction tank. At this time, the stirring paddle and the tank cover are lifted out together, and then the cantilever crane is used to pour the reduction product in the reduction tank into the leaching silo.

[0110] S12. Elution to remove sodium: Use a spray system to slowly spray deionized water into the elution silo to remove residual sodium in the reduction product.

[0111] S13, crushing the reduced product: start the jaw crusher, put the reduced product in the leaching silo into the jaw crusher and crush it into product fragments with a particle size less than 2 cm and fall into the transfer vehicle.

[0112] S14, water washing: transfer the product fragments in the transfer vehicle into a water washing tank and wash them with cold deionized water and hot deionized water in turn. The specific process is: first use cold deionized water to wash away the metallic sodium, potassium tantalate, diluent, and reaction by-products in the product fragments, until the pH value of the washing liquid discharged from the washing tank is neutral, then switch to hot deionized water for washing, and stop washing with hot deionized water when the conductivity of the washing liquid discharged from the washing tank is ≤60us / cm.

[0113] S15, pickling: the washed product fragments are transferred to a pickling tank, and the product fragments are pickled for 6 hours using a mixed acid, wherein the mixed acid is a mixture of 5%-20% nitric acid, 0.5-5% hydrogen peroxide, and 0.1%-1% hydrofluoric acid in equal volumes.

[0114] S16, acid washing: the product fragments after acid washing are transferred to a water washing tank, and deionized water is used to wash away the mixed acid remaining on the product fragments.

[0115] S17, drying: the product fragments after acid washing are transferred to a drying box, and dried in the drying box at a vacuum degree of -0.08Mpa and a temperature of 120°C for 15 hours. The dried product fragments are sieved, and the sieved materials are sent to a vacuum heat treatment furnace and sintered at a temperature of 1100°C for 1 hour to obtain tantalum powder III.

[0116] Comparative Example 3: A method for preparing high-purity tantalum powder, comprising the following steps:

[0117] S1. Prepare materials: Use compressed air to clean the outer package of potassium fluorotantalate, open the outer package of potassium fluorotantalate and add the potassium fluorotantalate into the potassium fluorotantalate raw material bin. The high melting point metal impurities W, Mo, and Nb in potassium fluorotantalate are ≤1ppm. Use compressed air to clean the outer package of the diluent, open the outer package of the diluent and add the diluent into the diluent raw material bin. The diluent is sodium chloride.

[0118] S2. Loading: Use a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, start the first bucket elevator to add the potassium fluorotantalate in the potassium fluorotantalate raw material bin to the first vacuum dryer, start the second bucket elevator to add the diluent in the diluent raw material bin to the second vacuum dryer, and then use the cantilever crane to cover the covers of the first vacuum dryer and the second vacuum dryer respectively; after the second bucket elevator completes the lifting operation, use compressed air to blow it clean.

[0119] S3, vacuum activation and drying: start the first vacuum dryer to vacuum activate potassium tantalate at 320°C, -0.1Mpa, and 5r / min for 5 hours, and start the second vacuum dryer to dry the diluent at 150°C, -0.1Mpa, and 5r / min for 5 hours.

[0120] S4. Discharging: Use a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, put the potassium tantalate vacuum-activated in the first vacuum dryer into the potassium tantalate loading bin, and put the diluent dried in the second vacuum dryer into the diluent loading bin; discharge the potassium tantalate in the potassium tantalate loading bin and the diluent in the diluent loading bin into the screw feeder at a weight ratio of 2.5:1 between potassium tantalate and diluent, the amount of potassium tantalate is 200kg.

[0121] S5. Canning: Use a cantilever crane to open the cover of the reduction tank, mix potassium tantalate and diluent and add them into the reduction tank through a screw feeder, and cut 1 kg of sodium block into several portions and scatter them evenly in the reduction tank. After canning is completed, use a cantilever crane to cover the cover of the reduction tank and drop the reduction tank into the reduction furnace, connect the cooling water pipe, argon pipe and sodium injection pipe of the reduction tank, and pass cooling water with a flow rate greater than 2 kg / min into the jacket of the reduction tank. Check whether the sensors on the reduction tank are normal.

[0122] S6. Filling with argon and heating: When the pressure is 0.05Mpa, start the vacuum pump to evacuate the reduction tank, and then fill the reduction tank with argon when the pressure is -0.1Mpa. After repeating the vacuum pumping and argon filling cycle twice, heat the reduction tank at a heating rate of 15℃ / min. At the same time, continue to evacuate the reduction tank until the temperature of the material in the reduction tank rises to 150℃, and then repeat the vacuum pumping and argon filling cycle once more. After argon filling and replacement, the pressure in the reduction tank is maintained between 0.02Mpa and 0.1Mpa.

[0123] S7. Stirring sodium reduction: continue to heat the reduction tank at a heating rate of 15°C / min. When the temperature in the reduction tank rises to 740°C, stop heating. Stir the agitator at a stirring rate of 80r / min. Add sodium to the reduction tank at a rate of 4kg / min. The amount of sodium added is 30% of the weight of potassium tantalate. When injecting sodium, control the temperature in the reduction tank to be lower than 1100°C.

[0124] S8. Insulation: After the sodium injection is completed, the reduction tank is kept at a temperature of 900° C. for 1 hour, then the stirring paddle is stopped and lifted to the top of the inner side of the reduction tank.

[0125] S9. Cooling: Use a cantilever crane to lift the reduction tank out of the reduction furnace, start the exhaust system to exhaust air until the temperature in the reduction tank is lower than 100°C and stop exhausting.

[0126] S10, opening the tank: use a cantilever crane to lift the reduction tank to the furnace unloading room, start the waste gas collection system in the furnace unloading room, and then use the cantilever crane to open the tank cover of the reduction tank. At this time, the stirring paddle and the tank cover are lifted out together, and then the cantilever crane is used to pour the reduction product in the reduction tank into the leaching silo.

[0127] S11. Elution to remove sodium: Use a spray system to slowly spray deionized water into the elution silo to remove residual sodium in the reduction product.

[0128] S12. Crushing the reduction product: start the jaw crusher, put the reduction product in the leaching silo into the jaw crusher and crush it into product fragments with a particle size less than 2 cm, which fall into the transfer vehicle.

[0129] S13, water washing: transfer the product fragments in the transfer vehicle into a water washing tank and wash them with cold deionized water and hot deionized water in turn. The specific process is: first use cold deionized water to wash away the metallic sodium, potassium tantalate, diluent, and reaction by-products in the product fragments, until the pH value of the washing liquid discharged from the washing tank is neutral, then use hot deionized water for washing, and stop using hot deionized water for washing when the conductivity of the washing liquid discharged from the washing tank is ≤60us / cm.

[0130] S14, pickling: the washed product fragments are transferred to a pickling tank, and the product fragments are pickled for 6 hours using a mixed acid, wherein the mixed acid is a mixture of 5%-20% nitric acid, 0.5-5% hydrogen peroxide, and 0.1%-1% hydrofluoric acid in equal volumes.

[0131] S15, acid washing: the product fragments after acid washing are transferred to a water washing tank, and deionized water is used to wash away the mixed acid remaining on the product fragments.

[0132] S16, drying: the product fragments after acid washing are transferred to a drying box, and dried in the drying box at a vacuum degree of -0.08Mpa and a temperature of 120°C for 15 hours. The dried product fragments are sieved, and the sieved materials are sent to a vacuum heat treatment furnace and sintered at a temperature of 1100°C for 1 hour to obtain tantalum powder 4.

[0133] Comparative Example 4: A method for preparing high-purity tantalum powder, comprising the following steps:

[0134] S1. Prepare materials: Use compressed air to clean the outer package of potassium fluorotantalate, open the outer package of potassium fluorotantalate and add the potassium fluorotantalate into the potassium fluorotantalate raw material bin. The high melting point metal impurities W, Mo, and Nb in potassium fluorotantalate are ≤1ppm. Use compressed air to clean the outer package of the diluent, open the outer package of the diluent and add the diluent into the diluent raw material bin. The diluent is sodium chloride.

[0135] S2. Loading: Use a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, start the first bucket elevator to add the potassium fluorotantalate in the potassium fluorotantalate raw material bin to the first vacuum dryer, start the second bucket elevator to add the diluent in the diluent raw material bin to the second vacuum dryer, and then use the cantilever crane to cover the covers of the first vacuum dryer and the second vacuum dryer respectively; after the second bucket elevator completes the lifting operation, use compressed air to blow it clean.

[0136] S3, vacuum activation and drying: start the first vacuum dryer to vacuum activate potassium tantalate at 320°C, -0.1Mpa, and 5r / min for 5 hours, and start the second vacuum dryer to dry the diluent at 150°C, -0.1Mpa, and 5r / min for 5 hours.

[0137] S4. Discharging: Use a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, put the potassium tantalate vacuum-activated in the first vacuum dryer into the potassium tantalate loading bin, and put the diluent dried in the second vacuum dryer into the diluent loading bin; discharge the potassium tantalate in the potassium tantalate loading bin and the diluent in the diluent loading bin into the screw feeder at a weight ratio of 2.5:1 between potassium tantalate and diluent, the amount of potassium tantalate is 200kg.

[0138] S5. Canning: Use a cantilever crane to open the cover of the reduction tank, mix potassium tantalate and diluent and add them into the reduction tank through a screw feeder, and cut 1 kg of sodium block into several portions and scatter them evenly in the reduction tank. After canning is completed, use a cantilever crane to cover the cover of the reduction tank and drop the reduction tank into the reduction furnace, connect the cooling water pipe, argon pipe and sodium injection pipe of the reduction tank, and pass cooling water with a flow rate greater than 2 kg / min into the jacket of the reduction tank. Check whether the sensors on the reduction tank are normal.

[0139] S6. Filling with argon and heating: When the pressure is 0.05Mpa, start the vacuum pump to evacuate the reduction tank, and then fill the reduction tank with argon when the pressure is -0.1Mpa. After repeating the vacuum pumping and argon filling cycle twice, heat the reduction tank at a heating rate of 15℃ / min. At the same time, continue to evacuate the reduction tank until the temperature of the material in the reduction tank rises to 150℃, and then repeat the vacuum pumping and argon filling cycle once more. After argon filling and replacement, the pressure in the reduction tank is maintained between 0.02Mpa and 0.1Mpa.

[0140] S7. Heating and stirring: continue to heat the reduction tank at a heating rate of 15°C / min. When the temperature in the reduction tank rises to 800°C, the stirring paddle is stirred at a stirring rate of 60r / min.

[0141] S8. Stirring sodium reduction: continue to heat the reduction tank at a heating rate of 15°C / min. When the temperature in the reduction tank rises to 840°C, stop heating. Stir the stirring slurry at a stirring rate of 80r / min. Inject sodium into the reduction tank at a rate of 4kg / min. The amount of sodium injected is 30% of the weight of potassium tantalate. The temperature in the reduction tank is not controlled during the sodium injection process.

[0142] S9. Insulation: After the sodium injection is completed, the reduction tank is kept at a temperature of 900°C for 1 hour, then the stirring paddle is stopped and lifted to the top of the inner side of the reduction tank.

[0143] S10, cooling: Use a cantilever crane to lift the reduction tank out of the reduction furnace, start the exhaust system to exhaust air until the temperature in the reduction tank is lower than 100°C and then stop exhausting.

[0144] S11, tank opening: Use a cantilever crane to lift the reduction tank to the furnace unloading room, start the waste gas collection system in the furnace unloading room, and then use the cantilever crane to open the tank cover of the reduction tank. At this time, the stirring paddle and the tank cover are lifted out together, and then the cantilever crane is used to pour the reduction product in the reduction tank into the leaching silo.

[0145] S12. Elution to remove sodium: Use a spray system to slowly spray deionized water into the elution silo to remove residual sodium in the reduction product.

[0146] S13, crushing the reduced product: start the jaw crusher, put the reduced product in the leaching silo into the jaw crusher and crush it into product fragments with a particle size less than 2 cm and fall into the transfer vehicle.

[0147] S14, water washing: transfer the product fragments in the transfer vehicle into a water washing tank and wash them with cold deionized water and hot deionized water in turn. The specific process is: first use cold deionized water to wash away the metallic sodium, potassium tantalate, diluent, and reaction by-products in the product fragments, until the pH value of the washing liquid discharged from the washing tank is neutral, then switch to hot deionized water for washing, and stop washing with hot deionized water when the conductivity of the washing liquid discharged from the washing tank is ≤60us / cm.

[0148] S15, pickling: the washed product fragments are transferred to a pickling tank, and the product fragments are pickled for 6 hours using a mixed acid, wherein the mixed acid is a mixture of 5%-20% nitric acid, 0.5-5% hydrogen peroxide, and 0.1%-1% hydrofluoric acid in equal volumes.

[0149] S16, acid washing: the product fragments after acid washing are transferred to a water washing tank, and deionized water is used to wash away the mixed acid remaining on the product fragments.

[0150] S17, drying: the product fragments after acid washing are transferred to a drying box, and dried in the drying box at a vacuum degree of -0.08Mpa and a temperature of 120°C for 15 hours. The dried product fragments are sieved, and the sieved materials are sent to a vacuum heat treatment furnace and sintered at a temperature of 1100°C for 1 hour to obtain tantalum powder V.

[0151] The obtained tantalum powder 1, tantalum powder 2, tantalum powder 3, tantalum powder 4 and tantalum powder 5 were tested for impurity content. The test results are shown in Table 1 below.

[0152] Table 1. Impurity content test results

[0153]

[0154]

[0155] The obtained tantalum powder 1, tantalum powder 2, tantalum powder 3, tantalum powder 4 and tantalum powder 5 were tested for bulk density. The test results are shown in Table 2 below.

[0156] Table 2. Bulk density test results

[0157]

[0158] From Table 1 and Table 2, we can see that:

[0159] In the tantalum powder prepared by the preparation method of Example 1 of the present invention, the sum of the high melting point metal impurities W, Mo, and Nb is <2ppm, the sum of the metal impurities Fe, Ni, and Cr is ≤10ppm, O≤600ppm, and the bulk density is 4.25g / cm3, which fully meets the requirements of high bulk ratio high-purity tantalum powder for manufacturing sputtering targets.

[0160] Dividing the sodium block into several equal parts and scattering them evenly in the reduction tank is more effective than simply placing them on top of potassium tantalate and diluent. It can better neutralize the acidic atmosphere in the reduction tank and prevent corrosion of the reduction tank.

[0161] Evacuating the reduction tank and filling it with argon to replace the air in the reduction tank is extremely critical to reducing the oxygen content of tantalum powder.

[0162] Controlling the temperature below 1100°C during the sodium injection process can reduce the impurity content of tantalum powder.

[0163] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for preparing high-purity tantalum powder, characterized in that: The following steps are involved: S1. Material preparation: After cleaning the outer package of potassium fluorotantalate with compressed air, open the outer package of potassium fluorotantalate and add the potassium fluorotantalate into the potassium fluorotantalate raw material bin; after cleaning the outer package of diluent with compressed air, open the outer package of diluent and add the diluent into the diluent raw material bin; S2, loading: using a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, starting the first bucket elevator to add the potassium fluorotantalate in the potassium fluorotantalate raw material bin to the first vacuum dryer, starting the second bucket elevator to add the diluent in the diluent raw material bin to the second vacuum dryer, and then using the cantilever crane to cover the covers of the first vacuum dryer and the second vacuum dryer respectively; S3, vacuum activation and drying: start the first vacuum dryer to vacuum activate potassium fluorotantalate for 2-6 hours at a temperature of 250-350°C, a pressure of -0.1-0.08Mpa, and a speed of 3-8r / min, and start the second vacuum dryer to dry the diluent for 3-8 hours at a temperature of 120-180°C, a pressure of -0.1-0.08Mpa, and a speed of 3-8r / min; S4, discharging: using a cantilever crane to open the covers of the first vacuum dryer and the second vacuum dryer respectively, putting the potassium fluorotantalate vacuum-activated in the first vacuum dryer into the potassium fluorotantalate loading bin, putting the diluent dried in the second vacuum dryer into the diluent loading bin, and discharging the potassium fluorotantalate in the potassium fluorotantalate loading bin and the diluent in the diluent loading bin into the screw feeder at a weight ratio of potassium fluorotantalate to diluent of 1.5-3:1, the amount of potassium fluorotantalate is 100-400kg; S5. Canning: Use a cantilever crane to open the cover of the reduction tank, mix potassium tantalate and diluent and add them into the reduction tank through a screw feeder, and cut 0.5-3 kg of sodium blocks into several pieces and evenly scatter them in the reduction tank. After canning is completed, use a cantilever crane to cover the cover of the reduction tank and drop the reduction tank into the reduction furnace, connect the cooling water pipe, argon pipe and sodium injection pipe of the reduction tank, and pass cooling water with a flow rate greater than 2 kg / min into the jacket of the reduction tank. Check whether the sensors on the reduction tank are normal; S6, argon filling and heating: when the pressure is 0.05-0.08Mpa, start the vacuum pump to evacuate the reduction tank, and then fill the reduction tank with argon when the pressure is -0.1-0.08Mpa. After the vacuuming and argon filling cycles are repeated 1-2 times, the reduction tank is heated at a heating rate of 10-20℃ / min, and the reduction tank is continuously vacuumed until the temperature of the material in the reduction tank rises to 150℃. Then, the vacuuming and argon filling cycles are repeated once again. After the argon filling replacement, the pressure in the reduction tank is maintained between 0.02Mpa-0.1Mpa; S7, heating and stirring: continue to heat the reduction tank at a heating rate of 10-20°C / min, and when the temperature in the reduction tank rises to 700-800°C, stir the stirring paddle at a stirring rate of 40-60r / min; S8, stirring sodium reduction: continue to heat the reduction tank at a heating rate of 10-20°C / min, stop heating when the temperature in the reduction tank rises to 810-850°C, stir with a stirring paddle at a stirring rate of 60-100r / min, inject sodium into the reduction tank at a rate of 1-4kg / min, the amount of sodium injected is 30% of the weight of potassium fluorotantalate, and control the temperature in the reduction tank to be lower than 1100°C during the sodium injection; S9, heat preservation: after the sodium injection is completed, the reduction tank is controlled to be kept at a temperature of 880-930°C for 0.5-2h, then the stirring paddle is stopped and lifted to the top of the inner side of the reduction tank; S10, cooling: using a cantilever crane to lift the reduction tank out of the reduction furnace, starting the exhaust system to exhaust air until the temperature in the reduction tank is lower than 100°C and then stopping the exhaust; S11, opening the tank: use a cantilever crane to lift the reduction tank to the furnace unloading room, start the waste gas collection system in the furnace unloading room, and then use the cantilever crane to open the tank cover of the reduction tank. At this time, the stirring paddle and the tank cover are lifted out together, and then the cantilever crane is used to pour the reduction product in the reduction tank into the leaching silo; S12, elution and sodium removal: use a spray system to slowly spray deionized water into the elution silo to remove residual sodium in the reduction product; S13, crushing the reduced product: start the jaw crusher, put the reduced product in the leaching silo into the jaw crusher, and crush it into product fragments with a particle size of less than 2 cm, which fall into the transfer vehicle; S14, water washing: transferring the product fragments in the transfer vehicle into a water washing tank and washing them with cold deionized water and hot deionized water in sequence; S15, pickling: transferring the washed product fragments to a pickling tank, and pickling the product fragments with a mixed acid for 4-12 hours; S16, acid washing: transferring the product fragments after acid washing to a water washing tank, and using deionized water to wash away the mixed acid remaining on the product fragments; S17, drying: the product fragments after acid washing are transferred to a drying box for drying, the dried product fragments are sieved, and the sieved material is sent to a vacuum heat treatment furnace for sintering at a temperature of 1050-1200° C. for 0.5-3 h to obtain tantalum powder.

2. The preparation method according to claim 1, characterized in that: The high melting point metal impurities W, Mo and Nb in the potassium fluorotantalate in S1 are ≤1ppm.

3. The preparation method according to claim 1, characterized in that: The diluent in S1 is sodium chloride or potassium chloride.

4. The preparation method according to claim 1, characterized in that: After the second bucket elevator in S2 completes the lifting operation, it is blown clean with compressed air.

5. The preparation method according to claim 1, characterized in that: The bottom of the potassium fluorotantalate loading bin and the bottom of the diluent loading bin are respectively installed with weight sensors for monitoring weight changes.

6. The preparation method according to claim 1, characterized in that: The insertion depth of the stirring paddle of the reduction tank is 1 / 3-1 / 2 of the height below the top surface of the material.

7. The preparation method according to claim 1, characterized in that: The specific process of water washing in S14 is: first use cold deionized water to wash away the metallic sodium, potassium tantalate, diluent, and reaction by-products in the product fragments, until the pH value of the washing liquid discharged from the washing tank is neutral, then switch to hot deionized water for washing, and stop using hot deionized water for washing until the conductivity of the washing liquid discharged from the washing tank is ≤60us / cm.

8. The preparation method according to claim 1, characterized in that: The mixed acid in S15 is prepared by mixing 5%-20% nitric acid, 0.5%-5% hydrogen peroxide, and 0.1%-1% hydrofluoric acid in equal volumes.

9. The preparation method according to claim 1, characterized in that: In the drying box in S17, the drying is carried out for 12-20 hours under the conditions of vacuum degree of -0.08Mpa and temperature of 80-120°C.