Cobaltosic oxide and preparation method thereof, lithium cobalt oxide and positive pole piece
Through flash drying and suspension furnace sintering processes, the processing strength and electrochemical performance of cobalt tetraoxide are improved, and the fragility of its particles and insufficient binding capacity are solved, and the preparation of cobalt tetraoxide with high specific surface area and tap density is achieved, which improves lithium cobalt oxide Electrochemical properties.
Patent Information
- Application Number
- CN202411112229.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The processing performance of cobalt tetraoxide particles is insufficient and easy to break, and their binding capacity and electrochemical performance with lithium need to be improved. It is difficult for the existing technology to effectively improve their specific surface area and tap density.
Using flash drying and suspension furnace sintering technology, the cobalt tetroxide particles are rapidly shrinked by high temperature, and their internal bonding strength and processing strength are improved. Cobalt tetroxide with high specific surface area and tap density is prepared, and mixed with lithium source to sinter it to obtain good electrochemical Lithium cobalt oxide of performance.
The processing strength and electrochemical performance of cobalt tetroxide are improved, the discharge specific capacity of lithium cobalt oxide is increased, and the rapid shrinkage and efficient electrochemical performance of the material are achieved.
Smart Images

Figure CN119018941A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of positive electrode materials for lithium batteries, and in particular to cobalt tetroxide and a preparation method thereof, lithium cobaltate and a positive electrode sheet. Background Art
[0002] Cobalt oxide particles are layered and have weak interlayer bonding, so the particles are brittle and easily broken during processing. The prior art uses a variety of methods to improve the processing performance of cobalt oxide, such as improving the crystallinity of its outer layer, but the effect is not ideal. On the other hand, in order to improve the binding ability of cobalt oxide with lithium and the electrochemical performance of the product lithium cobaltate, it is necessary to further improve the specific surface area and tap density of cobalt oxide.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] The object of the present invention is to provide a cobalt oxide and a preparation method thereof, lithium cobalt oxide and a positive electrode plate, aiming to improve the processing strength, specific surface area and tap density of the cobalt oxide, thereby improving the electrochemical properties of the lithium cobalt oxide obtained therefrom.
[0005] The present invention is achieved in that:
[0006] In a first aspect, the present invention provides a cobalt trioxide having the following characteristics:
[0007] Feature 1: The particle size difference ΔDv5 of the cobalt tetroxide under a pressure of 7500N relative to the particle size difference ΔDv5 under zero pressure is ≤0.37 μm;
[0008] Feature 2: The particle size difference ΔDv10 of the cobalt tetroxide under a pressure of 7500N relative to the particle size difference ΔDv10 under zero pressure is ≤0.5 μm;
[0009] Feature 3: The particle size difference ΔDv50 of the cobalt tetroxide at a pressure of 7500N relative to the Dv50 at zero pressure is ≤1.95μm.
[0010] In some embodiments of the present invention, the cobalt oxide has at least one of the following characteristics:
[0011] Feature 4: The value of ΔDv5 is 0.26μm≤ΔDv5≤0.37μm; the value of ΔDv10 is 0.4μm≤ΔDv10≤0.5μm; the value of ΔDv50 is 1.85μm≤ΔDv50≤1.95μm;
[0012] Feature 5: The specific surface area of the cobalt oxide is greater than or equal to 10m 2 / g; preferably, the specific surface area is 10 to 12.6 m2 / g;
[0013] Feature 6: The tap density of the cobalt oxide is greater than or equal to 2.25 g / cm 3 Preferably, the tap density is 2.25 to 2.4 g / cm 3 .
[0014] In a second aspect, the present invention provides a method for preparing cobalt trioxide, comprising the following steps:
[0015] Step 1: sending the cobalt carbonate into a flash dryer for drying to obtain a pre-oxidized material;
[0016] Step 2: sending the pre-oxidized material into a suspension furnace for sintering, and screening and demagnetizing after cooling to obtain cobalt tetroxide.
[0017] In some embodiments of the present invention, the drying temperature in step 1 is 250-400° C. and the drying time is 10-30 seconds.
[0018] In some embodiments of the present invention, the water content of the pre-oxidation material is ≤1.5%, and the cobalt content is 60%-72.2%.
[0019] In some embodiments of the present invention, the sintering temperature in step 2 is 710-750° C. and the sintering time is 2-3 min.
[0020] In some embodiments of the present invention, the feeding rate of the cobalt carbonate into the flash dryer in step 1 is 5 to 15 kg / min.
[0021] In some embodiments of the present invention, the feeding rate of the pre-oxidized material into the suspension furnace in step 2 is 4-11 kg / min.
[0022] In a third aspect, the present invention provides a lithium cobaltate obtained by mixing the cobalt trioxide of the first aspect or the cobalt trioxide obtained from any one of the embodiments of the second aspect with a lithium source and sintering the mixture.
[0023] In a fourth aspect, the present invention provides a positive electrode plate comprising the above-mentioned lithium cobalt oxide.
[0024] In a fifth aspect, the present invention also provides a lithium battery, comprising the above-mentioned positive electrode plate.
[0025] The present invention has the following beneficial effects:
[0026] The invention provides cobalt oxide and a preparation method thereof. The cobalt oxide has good processing strength, high specific surface area and tap density. Firstly, cobalt carbonate is dehydrated and pre-oxidized at high temperature by adopting a flash drying method, and then further sintered in a suspension furnace. Both the flash drying and suspension furnace sintering processes reduce the processing time of the material, so that the material can shrink rapidly at high temperature, improve the bonding strength inside the material particles, and thus improve the tap density, specific surface area and processing strength of the material. The lithium cobalt oxide obtained by subsequent lithium addition and sintering has good discharge specific capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 The SEM images of cobalt tetroxide prepared in Example 1 (a) and Comparative Example 3 (b);
[0029] Figure 2 The SEM images of the cobalt tetroxide prepared in Example 1 (a) and Comparative Example 3 (b) after ball milling experiment;
[0030] Figure 3 The charge and discharge curves of the cobalt tetroxide prepared in Example 1 and Comparative Example 3 are shown. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0032] The present invention provides a cobalt tetraoxide having the following characteristics:
[0033] Feature 1: The particle size difference ΔDv5 of the cobalt tetroxide under a pressure of 7500N relative to the particle size difference ΔDv5 under zero pressure is ≤0.37 μm;
[0034] Feature 2: The particle size difference ΔDv10 of the cobalt tetroxide under a pressure of 7500N relative to the particle size difference ΔDv10 under zero pressure is ≤0.5 μm;
[0035] Feature 3: The particle size difference ΔDv50 of the cobalt tetroxide at a pressure of 7500N relative to the Dv50 at zero pressure is ≤1.95μm.
[0036] Dv5, Dv10, and Dv50 refer to the particle sizes corresponding to 5%, 10%, and 50% of the cumulative particle size distribution based on volume. ΔDv5, ΔDv10, and ΔDv50 refer to the changes in Dv5, Dv10, and Dv50 of cobalt oxide under a pressure of 7500N relative to zero pressure. The smaller ΔDv is, the greater the processing strength of cobalt oxide is, and the particles are not easy to break during pressing, which is beneficial to the subsequent mixed sintering with a lithium source to obtain lithium cobalt oxide with high sphericity and high tap density, which is beneficial to the electrochemical properties of lithium cobalt oxide.
[0037] In some embodiments of the present invention, the cobalt oxide has at least one of the following characteristics:
[0038] Feature 4: The value of ΔDv5 is 0.26μm≤ΔDv5≤0.37μm; the value of ΔDv10 is 0.4μm≤ΔDv10≤0.5μm; the value of ΔDv50 is 1.85μm≤ΔDv50≤1.95μm;
[0039] Feature 5: The specific surface area of the cobalt oxide is greater than or equal to 10m 2 / g; preferably, the specific surface area is 10 to 12.6 m 2 / g;
[0040] Feature 6: The tap density of the cobalt oxide is greater than or equal to 2.25 g / cm 3 Preferably, the tap density is 2.25 to 2.4 g / cm 3 .
[0041] The present invention provides a method for preparing cobalt trioxide, comprising the following steps:
[0042] Step 1: sending the cobalt carbonate into a flash dryer for drying to obtain a pre-oxidized material;
[0043] Step 2: Send the pre-oxidized material into a suspension furnace for sintering, and after cooling, screen and demagnetize to obtain cobalt tetroxide.
[0044] The cobalt carbonate of the present invention is partially oxidized while being dried and dehydrated in a flash dryer to obtain a pre-oxidized material, which can effectively prevent the cobalt carbonate from sticking to the wall during subsequent sintering in a suspension furnace. The sticking to the wall is not conducive to the full contact between the particles and oxygen, thus causing problems such as uneven oxidation.
[0045] The present invention adopts a suspension furnace to sinter the pre-oxidized material. In the suspension furnace, the material is in a suspended state, and the heat and mass transfer rate is much greater than that of the material in a fixed bed and a fluidized bed; the gas in the furnace is in a fierce turbulent state, the material is heated evenly, and the reaction rate is high. This firing method has a small particle size and high firing activity, so the obtained cobalt tetroxide has good homogeneity, high tap density, high specific surface area, and high processing strength.
[0046] Both flash drying and suspension furnace sintering processes reduce the processing time of materials, allowing the materials to shrink rapidly at high temperatures, improving the bonding strength within the material particles, and thereby increasing the material's tap density, specific surface area, and processing strength.
[0047] In some embodiments of the present invention, the drying temperature in step 1 is 250-400°C, which can be 250°C, 300°C, 350°C, 400°C, etc.; the drying time is 10-30s, which can be 10s, 20s, 30s, etc.; the temperature and time of flash drying have an impact on the pre-oxidation degree of cobalt carbonate. The higher the temperature and the longer the time, the higher the oxidation degree of cobalt carbonate; if the temperature is too low, the pre-oxidation degree of cobalt carbonate is low, which is not conducive to improving the tap density of the material; if the temperature is too high, the equipment requirements are high, which will cause design waste and reduce the sintering activity of cobalt tetroxide.
[0048] In some embodiments of the present invention, the water content of the pre-oxidation material in step one is ≤1.5%, and can be 1.5%, 1.2%, 0.8%, 0.5%, 0.2%, etc.; the cobalt content is 60%-72.2%, and can be 60%, 62%, 64%, 66%, 68%, 70%, 72.2%, etc.
[0049] In some embodiments of the present invention, the feeding rate of the cobalt carbonate into the flash dryer in step 1 is 5 to 15 kg / min.
[0050] In some embodiments of the present invention, the sintering temperature in step 2 is 710-750°C, which can be 710°C, 720°C, 730°C, 740°C, 750°C, etc.; the time is 2-3 min, which can be 2 min, 2.5 min, 3 min, etc.; the sintering temperature and time have an impact on the properties of cobalt oxide. Too high a temperature will result in over-sintering of the material; too low a temperature will result in insufficient oxidation and impure products.
[0051] In some embodiments of the present invention, the feeding rate of the pre-oxidized material into the suspension furnace is 4kg-11kg / min, which can be 4kg / min, 7kg / min, 9kg / min, 11kg / min, etc.
[0052] The embodiment of the present invention further provides a lithium cobalt oxide, which is obtained by mixing a lithium source with the cobalt oxide of any of the above embodiments and sintering the mixture.
[0053] In an optional embodiment, the lithium source includes at least one of lithium carbonate and lithium hydroxide.
[0054] An embodiment of the present invention further provides a positive electrode plate, comprising the above-mentioned lithium cobalt oxide.
[0055] An embodiment of the present invention also provides a lithium battery, including the above-mentioned positive electrode plate, the lithium battery also includes a negative electrode plate, an electrolyte, a separator, etc., forming a complete battery structure with good cycle performance.
[0056] Specifically, the specific types of the negative electrode sheet, electrolyte, and separator are not limited. During the charge and discharge process of the secondary battery, active ions are intercalated and removed back and forth between the positive electrode sheet and the negative electrode sheet, and the electrolyte plays a role in conducting ions between the positive electrode sheet and the negative electrode sheet.
[0057] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0058] Example 1
[0059] A method for preparing cobalt tetroxide comprises the following steps:
[0060] Step 1: Take cobalt carbonate with a moisture content of 10%, put it into a flash dryer for flash drying to obtain a pre-oxidized material; the flash dryer is set at a temperature of 300°C, a feed rate of 10kg / min, and a drying time of 20s. The obtained pre-oxidized material has a moisture content of 1.2% and a cobalt content of 63%.
[0061] Step 2: The pre-oxidized material is directly sent into a suspension furnace for sintering. After cooling, it is sieved and demagnetized to obtain cobalt tetroxide. The sintering temperature is 730°C, the sintering time is 2 minutes, and the feed rate is 7kg / min.
[0062] Example 2
[0063] A method for preparing cobalt tetroxide comprises the following steps:
[0064] Step 1: Take cobalt carbonate with a moisture content of 10%, put it into a flash dryer for flash drying to obtain a pre-oxidized material; the flash dryer is set at a temperature of 250°C, a feed rate of 15kg / min, and a drying time of 30s. The obtained pre-oxidized material has a moisture content of 1.4% and a cobalt content of 60%.
[0065] Step 2: The pre-oxidized material is directly sent into a suspension furnace for sintering. After cooling, it is sieved and demagnetized to obtain cobalt tetroxide. The sintering temperature is 710°C, the sintering time is 3 minutes, and the feed rate is 11 kg / min.
[0066] Example 3
[0067] A method for preparing cobalt tetroxide comprises the following steps:
[0068] Step 1: Take cobalt carbonate with a moisture content of 10%, put it into a flash dryer for flash drying to obtain a pre-oxidized material; the flash dryer is set at a temperature of 400°C, a feed rate of 5kg / min, and a drying time of 10s. The moisture content of the obtained pre-oxidized material is 0.6%, and the cobalt content is 69%.
[0069] Step 2: The pre-oxidized material is directly sent into a suspension furnace for sintering. After cooling, it is sieved and demagnetized to obtain cobalt tetroxide. The sintering temperature is 750°C, the sintering time is 2 minutes, and the feed rate is 4 kg / min.
[0070] Example 4
[0071] The difference from Example 1 is that the flash dryer in step 1 is set at 250°C.
[0072] The obtained pre-oxidized material has a water content of 1.3% and a cobalt content of 62%.
[0073] Example 5
[0074] The difference from Example 1 is that the flash dryer in step 1 is set at 350°C.
[0075] The obtained pre-oxidized material has a water content of 1.1% and a cobalt content of 64%.
[0076] Example 6
[0077] The difference from Example 1 is that the drying time in step 1 is 30 seconds.
[0078] The obtained pre-oxidized material has a water content of 0.8% and a cobalt content of 64%.
[0079] Example 7
[0080] The difference from Example 1 is that the sintering temperature in step 2 is 710°C.
[0081] Example 8
[0082] The difference from Example 1 is that the sintering temperature in step 2 is 750°C.
[0083] Comparative Example 1
[0084] The difference from Example 1 is that step 1 adopts oven drying, and the specific steps are as follows: take cobalt carbonate with a water content of 10%, put it into a blast oven for drying, set the temperature to 110°C, and the drying time is 8 hours.
[0085] The water content of the obtained pre-oxidized material is 5%, and the cobalt content is 53%.
[0086] Comparative Example 2
[0087] The difference from Example 1 is that step 2 uses a rotary kiln for sintering, and the specific steps are as follows: the pre-oxidized material is placed in a rotary kiln for sintering, and after cooling, it is sieved and demagnetized to obtain cobalt tetroxide. The sintering temperature is 730°C, the sintering time is 4h, and the feed rate is 200kg / h.
[0088] The obtained pre-oxidized material has a water content of 1.2% and a cobalt content of 63%.
[0089] Comparative Example 3
[0090] Step 1: Take cobalt carbonate with a water content of 10%, put it into a blast oven for drying, set the temperature to 110° C., and dry it for 8 hours to obtain dried cobalt tetroxide.
[0091] Step 2: Place the dried cobalt oxide in a rotary kiln for sintering, and after cooling, sieve and demagnetize to obtain cobalt oxide. The sintering temperature is 750° C., the sintering time is 4 hours, and the feed rate is 200 kg / h.
[0092] The water content of the obtained pre-oxidized material is 5%, and the cobalt content is 53%.
[0093] Comparative Example 4
[0094] The difference from Example 1 is that the flash dryer in step 1 is set at 150°C.
[0095] The obtained pre-oxidized material has a water content of 3% and a cobalt content of 48%.
[0096] Comparative Example 5
[0097] The difference from Example 1 is that the flash dryer in step 1 is set at 500°C.
[0098] The obtained pre-oxidized material has a water content of 0.9% and a cobalt content of 70%.
[0099] Figure 1 The scanning electron microscope (SEM) images of the cobalt oxide prepared in Example 1 (a) and Comparative Example 3 (b) show that the primary particles of the Example material are fine and the primary particles are tightly combined, while the primary particles of the Comparative Example material are coarse and have large gaps.
[0100] Test Example 1
[0101] The processing strength of the cobalt tetroxide prepared in the embodiment and the comparative example was evaluated, and the processing strength of the powder was evaluated by the change in the particle size of the cobalt tetroxide powder after pressing. The specific method is as follows: the initial particle size Dv5, Dv10, and Dv50 of the powder to be tested are tested, and then the powder sample to be tested is placed on a pressure particle size analyzer, and the pressure parameter is set to 7500N. After the powder sample is pressed, the particle size Dv5', Dv10', and Dv50' of the powder sample are measured again, and then the particle size difference ΔDv5, ΔDv10, and ΔDv50 are calculated. Taking ΔDv5 as an example, ΔDv5=Dv5-Dv5'; the particle size difference data of the embodiment and the comparative example are shown in Table 1.
[0102] Test Example 2
[0103] The cobalt tetroxide prepared in Example 1 and Comparative Example 3 was subjected to a ball milling test, and the morphology of the particles after ball milling was observed by scanning electron microscopy. The ball milling conditions were as follows: the rotation speed was 500 rpm, and the ball milling time was 10 min.
[0104] Figure 2 The SEM images of the cobalt tetroxide prepared in Example 1 (a) and Comparative Example 3 (b) after ball milling experiments show that the degree of particle crushing in Example 1 is lower than that in Comparative Example 3, indicating that Example 1 has better processing strength.
[0105] Test Example 3
[0106] According to the method for determining the tap density of powder products in GB / T 21354-2008, the tap density (TD) of cobalt tetroxide was determined by vibrating 500 times. The results are shown in Table 1.
[0107] Test Example 4
[0108] The cobalt tetroxide prepared in the examples and comparative examples was subjected to specific surface area analysis. The specific method is as follows: using a TriStar 3020 (Micromeritics) analyzer for testing, liquid nitrogen adsorption, weighing the weight before and after adsorption, and calculating the specific surface area (BET). The results are shown in Table 1.
[0109] Table 1
[0110]
[0111]
[0112] It can be seen from the data in Table 1 that the cobalt oxide prepared in the embodiment of the present invention has a higher processing strength than that in the comparative example, and the change in Dv50 particle size under 7500N pressing is less than 2μm. This is because the two processes of flash drying and suspension furnace sintering synergistically reduce the processing time of the material, so that the material can shrink rapidly at high temperature, improve the bonding strength inside the material particles, and thus improve the processing strength of the material. Specifically, comparative example 1 uses a blower to dry cobalt carbonate. The powder obtained in step 1 not only has a high water content, but also has a low dispersion of cobalt carbonate, and the particles are prone to sintering and agglomeration, resulting in the obtained cobalt oxide having a smaller specific surface area. Comparative example 2 uses a rotary kiln to oxidize and sinter the pre-oxidized material. At the same sintering temperature, the rotary kiln sintering time is 4h, while the suspension furnace sintering time of Example 1 is 2min, and the product tap density and specific surface area obtained in Example 1 are both high, indicating that suspension sintering can enable the particles to shrink rapidly.
[0113] Comparing Examples 1, 4, and 5, it can be seen from Examples 4 and 5 that the flash drying temperature affects the processing strength, specific surface area, and tap density of cobalt tetroxide. The material obtained at a flash drying temperature of 300°C has the best comprehensive performance. The reason is that too high a temperature leads to a decrease in the sintering activity of the pre-oxidized material, and too low a temperature leads to the wall adhesion of cobalt carbonate, both of which are not conducive to improving the performance of cobalt tetroxide.
[0114] By comparing Examples 1 and 6, it can be seen that the flash drying time affects the processing strength, specific surface area and tap density of cobalt oxide. Specifically, the longer the flash drying time, the greater the mechanical collision of the particles, and the more likely it is to lose powder, which affects the product quality. Therefore, the cobalt oxide obtained in Example 6 is slightly worse than that in Example 1.
[0115] By comparing Examples 1, 7, and 8, it can be seen that the sintering temperature has a greater influence on the specific surface area and tap density of cobalt oxide, but a lower influence on its processing strength. Specifically, as the sintering temperature increases, the smaller the specific surface area of the material, the greater the tap density. The appropriate temperature can be selected according to requirements.
[0116] Test Example 5
[0117] The cobalt trioxide prepared in the embodiment and the comparative example was mixed with a lithium source and sintered to obtain a lithium cobalt oxide positive electrode material, and then a battery was assembled and charged and discharged. The specific method is as follows:
[0118] (1) Cobalt tetroxide and lithium carbonate are mixed in a molar ratio of Li:Co=1.05:1, ground and mixed, and then sintered to obtain lithium cobalt oxide; the sintering temperature is 1100° C. and the time is 24 hours.
[0119] (2) Lithium cobalt oxide, acetylene black, and PVDF are ground and mixed in a weight ratio of 8:1:1, and then N-methylpyrrolidone (NMP) is added to obtain a positive electrode slurry; graphite, acetylene black, hydroxymethyl cellulose, and styrene butadiene rubber are ground and mixed in a weight ratio of 94.5:2:1.5:2, and then added to deionized water to obtain a negative electrode slurry; the positive electrode slurry and the negative electrode slurry are uniformly coated on aluminum foil and copper foil, respectively, and dried and rolled to obtain positive electrode sheets and negative electrode sheets.
[0120] (3) Button cell assembly: The positive electrode sheet and the negative electrode sheet were further punched into circular electrode sheets with a diameter of 12 mm, and then a CR2032 button cell was assembled using a glass fiber separator as a separator and a 1M LiPF6 solution (the solvent was a mixed solution of EMC, DC, and DMC in a volume ratio of 1:1:1) as an electrolyte.
[0121] (4) Charge and discharge test: The button battery is charged and discharged at a rate of 0.1C.
[0122] The first discharge specific capacity of the battery finally prepared by using the cobalt tetroxide of the embodiment and the comparative example as the raw material is shown in Table 2, and the charge and discharge curves of the battery finally prepared by using the cobalt tetroxide of the embodiment 1 and the comparative example 3 as the raw material are shown in Table 2. Figure 3 .
[0123] Table 2
[0124]
[0125] The electrochemical properties of cobalt oxide are comprehensively affected by its specific surface area and tap density. Specifically, the tap density has a greater influence on the specific capacity of the material. From the analysis of Table 2, it can be seen that when comparing Examples 1, 4, and 5, as the tap density of the material increases, the specific surface area increases, and the specific capacity increases; when comparing Examples 1 and 6, as the tap density of the material increases, the specific surface area increases, and the specific capacity increases; when comparing Examples 1, 7, and 8, as the tap density of the material increases, the specific capacity increases.
[0126] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A cobalt trioxide, characterized in that: It has the following characteristics: Feature 1: The particle size difference between the Dv5 of the cobalt tetroxide at 7500N pressure and the Dv5 at zero pressure ΔDv5≤0.37μm; Feature 2: The particle size difference ΔDv10 of the cobalt tetroxide under a pressure of 7500N relative to the particle size difference ΔDv10 under zero pressure is ≤0.5 μm; Feature 3: The particle size difference ΔDv50 of the cobalt tetroxide at a pressure of 7500N relative to the Dv50 at zero pressure is ≤1.95μm.
2. The cobalt tetraoxide according to claim 1, characterized in that Having at least one of the following characteristics: Feature 4: The value of ΔDv5 is 0.26μm≤ΔDv5≤0.37μm; the value of ΔDv10 is 0.4μm≤ΔDv10≤0.5μm; the value of ΔDv50 is 1.85μm≤ΔDv50≤1.95μm; Feature 5: The specific surface area of the cobalt oxide is greater than or equal to 10m 2 / g; Feature 6: The tap density of the cobalt oxide is greater than or equal to 2.25 g / cm 3 .
3. The method for preparing cobalt tetraoxide according to any one of claims 1 to 2, characterized in that: The following steps are involved: Step 1: sending the cobalt carbonate into a flash dryer for drying to obtain a pre-oxidized material; Step 2: sending the pre-oxidized material into a suspension furnace for sintering, and screening and demagnetizing after cooling to obtain cobalt tetroxide.
4. The method for preparing cobalt trioxide according to claim 3, characterized in that: The drying temperature in step 1 is 250-400° C. and the drying time is 10-30 seconds.
5. The method for preparing cobalt trioxide according to claim 3 or 4, characterized in that: The water content of the pre-oxidation material is ≤1.5%, and the cobalt content is 60%-72.2%.
6. The method for preparing cobalt trioxide according to claim 3, characterized in that: The sintering temperature in step 2 is 710-750° C. and the sintering time is 2-3 minutes.
7. The method for preparing cobalt trioxide according to claim 3, characterized in that: The feeding rate of the cobalt carbonate into the flash dryer in step 1 is 5 to 15 kg / min.
8. The method for preparing cobalt tetroxide according to claim 3, characterized in that: In step 2, the feed rate of the pre-oxidized material into the suspension furnace is 4-11 kg / min.
9. A lithium cobalt oxide, characterized in that: The lithium cobalt oxide is obtained by mixing a lithium source with the cobalt tetroxide according to any one of claims 1 to 2 and sintering the mixture.
10. A positive electrode sheet, characterized in that: Including the lithium cobalt oxide as described in claim 9.
Citation Information
Patent Citations
Preparation method of battery grade spherical cobaltosic oxide
CN108328665A
Method for preparing large-granularity cobaltosic oxide
CN108946824A
Device and process method for preparing light calcined magnesia by suspension calcination
CN111747663A
Method for manufacturing high-density cobaltosic oxide
CN1583576A
Cited By
Method for detecting compressive strength of lithium ion battery positive electrode material and application of method
CN121185758A