Ag-based organic coordination nanoparticles, preparation method thereof, photoresist composition and application thereof
Through the combination of Ag-based organic coordination nanoparticles, photoinitiator and organic dispersing solvent, the pattern formation and substrate protection of extreme ultraviolet photoresist under EUV radiation is solved, and high resolution and high sensitivity photolithography is achieved Performance to meet semiconductor manufacturing needs with smaller feature sizes.
Patent Information
- Application Number
- CN202310566757.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-18
AI Technical Summary
The existing extreme ultraviolet photoresist is difficult to achieve efficient pattern formation and protect substrate materials under EUV radiation, and the size distribution of nanoparticles has a great impact on the photoresist performance, making it difficult to meet the semiconductor manufacturing needs of smaller characteristic sizes.
Ag-based organic coordination nanoparticles are used to synthesize silver salt and organic ligand at specific temperatures and solvent conditions to form nanoparticles of 1nm-4nm, and combined with photoinitiator and organic dispersion solvent to form a photoresist Composition, high resolution and high sensitivity pattern formation is achieved by electron beam or extreme ultraviolet exposure development technology.
Ag-based organic coordination nanoparticles are realized in the photoresist, and the non-exposed areas can be effectively removed after development, obtaining photolithography performance with high resolution, high sensitivity and low line roughness, which can meet the needs of more Small feature size semiconductor manufacturing requirements.
Smart Images

Figure CN119019448A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photoresists, and in particular to Ag-based organic coordination nanoparticles and a preparation method thereof, a photoresist composition and an application thereof. Background Art
[0002] Photoresist refers to a corrosion-resistant thin film material whose solubility changes when exposed to ultraviolet light, electron beam, ion beam, extreme ultraviolet (EUV) or soft x-rays. It is widely used in pattern transfer in the manufacturing process of high-end micro-nano structures, including semiconductor integrated circuits, liquid crystal panel processing, and high-end optical device manufacturing. With the continuous advancement of semiconductor technology and the development of Moore's Law, semiconductor processes have continued to decrease, and higher requirements have been put forward for the reduction of processing feature sizes. In order to meet more advanced semiconductor processes and achieve smaller feature sizes, photolithography technology is also constantly developing, from I-line, G-line, Deep Ultraviolet (DUV) (including 248nm KrF lithography and 193nm ArF lithography) to extreme ultraviolet lithography, electron beam lithography and other fine processing methods. After the photoresist film is exposed and developed to form a photolithographic pattern, it will be dry or wet etched. The part of the substrate material not covered by the film is directly etched, while the substrate surface covered by the film is protected by the photoresist film and is not etched. Etching resistance is a very important evaluation index of photoresist. Excellent etching resistance can ensure that the photoresist can protect the substrate surface from damage during the etching process, effectively simplify the etching process, and greatly improve the yield of the finished etching product.
[0003] Extreme ultraviolet lithography has attracted attention as a basic technology for manufacturing next-generation semiconductor devices. EUV lithography is a pattern forming technology that uses EUV rays with a wavelength of about 13.5 nanometers as an exposure light source. According to EUV lithography, it is known that extremely fine patterns (for example, less than or equal to about 20 nanometers) can be formed in the exposure process during the manufacture of semiconductor devices. For exposure in the extreme ultraviolet band, the absorptivity of the photoresist itself, the reaction mechanism of solubility changes after exposure, and the size distribution of the photoresist components have a great influence on the comprehensive performance of the photoresist. Since metal elements have a higher absorptivity to EUV radiation, metal-containing photoresist materials have aroused people's interest, and metal oxide nanoparticle photoresist is one of the hot research directions. The Ober research group at Cornell University in the United States first introduced the concept of metal oxide nanoparticles as the next-generation extreme ultraviolet photoresist material. The synthesis of these nanoparticles is generally by controlling the hydrolysis of Zr or Hf alcohol salts in excess carboxylic acid, followed by precipitation treatment, thereby obtaining a nanoparticle photoresist of ZrO2 or HfO2 with organic ligands, and the size of the corresponding nanoparticles is controlled at 2-5nm, making it conducive to lithography below 20nm. In order to further find a more efficient metal organic nanophotoresist, the present invention focuses on Ag-based organic ligand nanoparticle photoresist and prepares a photoresist with excellent lithographic performance. Summary of the invention
[0004] The invention provides a novel Ag-based organic coordination nanoparticle and a preparation method thereof, a photoresist composition containing the same and application thereof.
[0005] The present invention provides a Ag-based organic coordination nanoparticle, the general formula of which is: [Ag m (R) n (Q) x ] y ,
[0006] Among them, R can be selected from bis(diphenylphosphino)methane (dppm), bis(dicyclohexylphosphino)methane (abbreviated as dcpm), bis(diphenylamino)methane, N,N-bis(diphenylphosphino)amine (abbreviated as dppa), N,N,N',N'-tetramethyldiaminomethane, N,N,N',N'-tetraethyldiaminomethane, and the like.
[0007] Q can be selected from CH3COO, C2H5COO, C3H7COO, i-C3H7COO, C4H9COO, C6H 13 COO, C9H 19 COO, C6H5COO, CF3COO, C2F5COO, C3F7COO, i-C3F7COO, C4F9COO, C6F 13 COO, C9F 19COO, C6H5COO, etc.
[0008] Among them, the ranges of m, n, x, and y are all 1-4.
[0009] Furthermore, the Ag-based organic coordination nanoparticles may have the following structure:
[0010] Ag2(dppm)2(CH3COO)2;
[0011] Ag4(dppm)2(CH3COO)4;
[0012] Ag4(dppm)2(CF3COO)4;
[0013] Ag2(dppm)2(C2H5COO)2;
[0014] Ag4(dppm)2(C2F5COO)4;
[0015] Ag4(dppm)2(C4F9COO)4;
[0016] Ag2(dcpm)2(CH3COO)2;
[0017] Ag4(dppa)2(CH3COO)4
[0018] The size of the Ag-based organic coordination nanoparticle crystals is 1 nm-4 nm, preferably 1 nm-2 nm.
[0019] The above-mentioned Ag-based organic coordination nanoparticles are prepared by the following method:
[0020] The silver salt and the first organic ligand are added to a sample bottle respectively, and an organic solvent is added to dissolve them, stirred for a certain time under a certain temperature condition, filtered, concentrated, cooled and crystallized or evaporated and crystallized, and finally recrystallized in an organic solvent to obtain Ag-based organic coordination nanoparticles.
[0021] Further, the ratio of the silver salt to the first organic ligand is 1:(0.5-1);
[0022] The organic solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-ethoxy-2-propanol, tetrahydrofuran, methanol, ethanol, propanol, dichloromethane and chloroform.
[0023] The stirring temperature is controlled at 0-120°C, preferably 15-80°C, more preferably 20-40°C.
[0024] The invention also provides a photoresist composition comprising the nanoparticles.
[0025] Furthermore, the above-mentioned photoresist composition further includes a photoinitiator and an organic dispersing solvent, wherein the photoinitiator preferably occupies 0.1wt%-10wt% of the composition, and the nanoparticles preferably occupy 1wt%-20wt% of the composition.
[0026] Further, the photoinitiator is selected from any one or more of N-hydroxynaphthaleneimide trifluoromethanesulfonic acid, 1,4-aminonaphthalenesulfonic acid, 2-amino-5,7-naphthalene disulfonic acid, tert-butylphenyl iodonium salt perfluorooctanesulfonic acid, triphenylsulfonium perfluorobutanesulfonic acid, triphenylsulfonium perfluorobutyl and triphenylsulfonium trifluorosulfonic acid.
[0027] Further, the organic dispersing solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-methoxy-2-propanol, propylene glycol mono-n-propyl ether, propylene glycol butyl ether, 1-ethoxy-2-propanol, methanol, ethanol, and propanol. The solvent is preferably 1-ethoxy-2-propanol.
[0028]
Method for patterning metal-organic coordination nanoparticles in photoresist
[0029] The present invention also provides a method for forming a photolithographic pattern, using the above-mentioned photoresist composition, dripping the photoresist composition onto a substrate, spin coating it into a film, heating it on a hot stage, then exposing it with an electron beam or mid-ultraviolet, deep ultraviolet, or extreme ultraviolet, and developing it with a developer.
[0030] The spin coating speed is further controlled at 1000-6000 rpm; the heating temperature of the hot stage is controlled at 50-110° C., and the heating time is controlled at 30-900 s.
[0031] Furthermore, the exposure dose is 50 to 8000 mJ / cm 2 .
[0032] Further, the developer is selected from a mixture of any one or more of decahydronaphthalene, tetrahydronaphthalene, indene, indane, quinoline, 1-methylnaphthalene, toluene, o-xylene, m-xylene, p-xylene, ethyl acetate, butyl acetate, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, propylene glycol mono-n-propyl ether, propylene glycol butyl ether, n-hexane and cyclohexane, and the developing temperature is room temperature or 20°C to 50°C.
[0033] The thickness of the pre-film layer after removing the organic dispersion solvent may be 10 nm to 100 nm. Specifically, the thickness of the pre-film layer may be 10 nm to 20 nm, 20 nm to 30 nm, 30 nm to 40 nm, 40 nm to 50 nm, 50 nm to 60 nm, 60 nm to 70 nm, 70 nm to 80 nm, 80 nm to 90 nm, 90 nm to 100 nm.
[0034] The substrate is selected from a silicon plate. Other substrates that are insoluble in the developer can also be selected according to actual needs.
[0035] Furthermore, the above nanoparticles are used in the field of photoresists, especially electron beam, mid-ultraviolet, deep ultraviolet, and EUV photoresists. Regarding masks, deep ultraviolet and longer wavelength light sources are transmissive masks, extreme ultraviolet is a reflective mask, and electron beams are exposed according to the pattern set by the software.
[0036] The Ag-based organic coordination nanoparticles provided by the embodiment of the present invention have a special structure. The photoacid generator generates photoacid after being irradiated by ultraviolet light. The photoacid can interact with the Ag-based organic coordination nanoparticles, thereby changing the polarity of the Ag-based organic coordination nanoparticles, causing the nanoparticles to agglomerate. Therefore, the solubility of the Ag-based organic coordination nanoparticles before and after exposure changes. Due to these characteristics, the Ag-based organic coordination nanoparticles are used as photoresist components, and the solubility of the photosensitive part and the light-shielding part of the photoresist in the developer can be different. The photosensitive part agglomerates in the developer, and the solubility is reduced, while the light-shielding part does not agglomerate and dissolves in the developer, so that the non-exposed area can be removed after development, and a pattern of a desired shape is obtained. Using the Ag-based organic coordination nanoparticles of the present invention as photoresist components can achieve more excellent lithography performances such as high resolution, high sensitivity, and low line roughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The structural formula of the crystalline compound prepared in Example 1 of the present invention;
[0038] Figure 2 This is the H NMR spectrum of the crystalline compound prepared in Example 1 of the present invention;
[0039] Figure 3 The dynamic light scattering particle size test result of Example 1 of the present invention;
[0040] Figure 4 is the exposure pattern of Example 1 of the present invention;
[0041] Figure 5 is the structural formula of Example 2 of the present invention;
[0042] Figure 6 This is the H NMR spectrum of Example 2 of the present invention;
[0043] Figure 7 The dynamic light scattering particle size test result of Example 2 of the present invention;
[0044] Figure 8 is the exposure pattern of Example 2 of the present invention;
[0045] Fig. 9The structure of Embodiment 3 of the present invention;
[0046] Fig.10 This is the H NMR spectrum of Example 3 of the present invention;
[0047] Fig.11 The dynamic light scattering particle size test result of Example 3 of the present invention;
[0048] Fig.12 This is the exposure pattern of Example 3 of the present invention. DETAILED DESCRIPTION
[0049] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0051] The present invention provides a Ag-based organic coordination nanoparticle, the general formula of which is: [Ag m (R) n (Q) x ] y
[0052] Among them, R can be selected from bis(diphenylphosphino)methane (dppm), bis(dicyclohexylphosphino)methane (abbreviated as dcpm), bis(diphenylamino)methane, N,N-bis(diphenylphosphino)amine (abbreviated as dppa), N,N,N',N'-tetramethyldiaminomethane, N,N,N',N'-tetraethyldiaminomethane, and the like.
[0053] Q can be selected from CH3COO, C2H5COO, C3H7COO, i-C3H7COO, C4H9COO, C6H 13 COO, C9H 19 COO, C6H5COO, CF3COO, C2F5COO, C3F7COO, i-C3F7COO, C4F9COO, C6F 13 COO, C9F 19 COO, C6H5COO, etc.
[0054] Among them, the ranges of m, n, x, and y are all 1-4;
[0055] Furthermore, the Ag-based organic coordination nanoparticles may have the following structure:
[0056] Ag2(dppm)2(CH3COO)2;
[0057] Ag4(dppm)2(CH3COO)4;
[0058] Ag4(dppm)2(CF3COO)4;
[0059] Ag2(dppm)2(C2H5COO)2;
[0060] Ag4(dppm)2(C2F5COO)4;
[0061] Ag4(dppm)2(C4F9COO)4;
[0062] Ag2(dcpm)2(CH3COO)2;
[0063] Ag4(dppa)2(CH3COO)4.
[0064] The size of the Ag-based organic coordination nanoparticle crystals is 1 nm-4 nm, preferably 1 nm-2 nm.
[0065] The Ag-based organic coordination nanoparticles provided by the embodiment of the present invention have a special structure. The photoacid generator generates photoacid after being irradiated by ultraviolet light. The photoacid can interact with the Ag-based organic coordination nanoparticles, thereby changing the polarity of the Ag-based organic coordination nanoparticles, causing the nanoparticles to agglomerate. Therefore, the solubility of the Ag-based organic coordination nanoparticles before and after exposure changes. Due to these characteristics, the Ag-based organic coordination nanoparticles are used as photoresist components, and the solubility of the photosensitive part and the light-shielding part of the photoresist in the developer can be different. The photosensitive part agglomerates, and the solubility is reduced in the developer, while the light-shielding part does not agglomerate and dissolves in the developer, so that the non-exposed area can be removed after development, and a pattern of a desired shape is obtained. Using the Ag-based organic coordination nanoparticles of the present invention as photoresist components can achieve more excellent lithography performances such as high resolution, high sensitivity, and low line roughness.
[0066] The above-mentioned Ag-based organic coordination nanoparticles are prepared by the following method:
[0067] The silver salt and the first organic ligand are added to a sample bottle respectively, and an organic solvent is added to dissolve them, stirred for a certain time under a certain temperature condition, filtered, concentrated, cooled and crystallized or evaporated and crystallized, and finally recrystallized in an organic solvent to obtain Ag-based organic coordination nanoparticles.
[0068] Further, the ratio of the silver salt to the first organic ligand is 1:(0.5-1);
[0069] The organic solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-ethoxy-2-propanol, tetrahydrofuran, methanol, ethanol, propanol, dichloromethane and chloroform.
[0070] The stirring temperature is controlled at 0-120°C, preferably 15-80°C, more preferably 20-40°C.
[0071] Some embodiments of the present invention provide Ag organic coordination nanoparticle photoresist compositions, including the above-mentioned nanoparticles, and also include a photoinitiator and an organic dispersing solvent. The photoinitiator preferably occupies 0.1wt%-10wt% of the composition, and the nanoparticles preferably occupy 1wt%-20% of the composition.
[0072] Further, the photoinitiator is selected from any one or more of N-hydroxynaphthaleneimide trifluoromethanesulfonic acid, 1,4-aminonaphthalenesulfonic acid, 2-amino-5,7-naphthalene disulfonic acid, tert-butylphenyl iodonium salt perfluorooctanesulfonic acid, triphenylsulfonium perfluorobutanesulfonic acid, triphenylsulfonium perfluorobutyl and triphenylsulfonium trifluorosulfonic acid.
[0073] Further, the organic dispersing solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-methoxy-2-propanol, propylene glycol mono-n-propyl ether, propylene glycol butyl ether, 1-ethoxy-2-propanol, methanol, ethanol, and propanol. The solvent is preferably 1-ethoxy-2-propanol.
[0074] Some embodiments of the present invention provide a method for patterning Ag organic coordinated nanoparticle photoresist, using the above-mentioned photoresist composition, dropping the photoresist composition onto a substrate by spin coating, heating it on a hot stage, then exposing it with an electron beam or mid-ultraviolet, deep ultraviolet, or extreme ultraviolet, and developing it with a developer.
[0075] The spin coating speed is further controlled at 1000-6000 rpm; the heating temperature of the hot stage is controlled at 50-110° C., and the heating time is controlled at 30-900 s.
[0076] Furthermore, the exposure dose is 50 to 8000 mJ / cm 2 .
[0077] Furthermore, the developer is selected from a mixture of any one or more of decahydronaphthalene, tetrahydronaphthalene, indene, indane, quinoline, 1-methylnaphthalene, toluene, o-xylene, m-xylene, ethyl acetate, butyl acetate, ethanol, n-propanol, isopropanol, n-butanol, n-hexane and cyclohexane, and the developing temperature is room temperature or 20°C to 50°C.
[0078] The thickness of the pre-film layer after removing the organic dispersion solvent may be 10 nm to 100 nm. Specifically, the thickness of the pre-film layer may be 10 nm to 20 nm, 20 nm to 30 nm, 30 nm to 40 nm, 40 nm to 50 nm, 50 nm to 60 nm, 60 nm to 70 nm, 70 nm to 80 nm, 80 nm to 90 nm, 90 nm to 100 nm.
[0079] The substrate is selected from a silicon plate. Other substrates that are insoluble in the developer can also be selected according to actual needs.
[0080] Furthermore, the above nanoparticles are used in the field of photoresists, especially electron beam, mid-ultraviolet, deep ultraviolet, extreme ultraviolet and / or EUV photoresists. Regarding the mask, deep ultraviolet and longer wavelength light sources are transmissive masks, extreme ultraviolet is a reflective mask, and the electron beam is exposed according to the pattern set by the software.
[0081] Example 1
[0082] Dissolve 0.769 g of bis(diphenylphosphino)methane in 20 mL of dichloromethane, add 0.884 g of silver trifluoroacetate, stir for 12 h, filter, and evaporate to remove the solvent to obtain a white solid product. Recrystallize in dichloromethane, dry in vacuum at room temperature, and take a sample for H NMR spectrum test (see Appendix Figure 2 , where δ3.26(CH2), δ7.26,7.40(C6H5)), the crystal structure is as attached Figure 1 As shown, the molecular formula is Ag4(dppm)2(CF3COO)4.
[0083] 0.5 g of Ag4(dppm)2(CF3COO)4 and 0.05 g of N-hydroxynaphthalimide trifluoromethanesulfonate were weighed and dissolved in 0.945 g of propylene glycol monomethyl ether acetate. The solution was filtered three times with a 0.22 μm filter to obtain a photoresist composition. The dynamic light scattering particle size test showed that the average particle size was 1.7 nm (see Appendix Figure 3 ). Set the coating machine speed to 2000rpm, the time is 1min, and a uniform photoresist film is spin-coated on the silicon wafer. Then, the wafer is placed on a hot plate at 80℃ and heated for 1min. The above wafer is exposed to a 254nm wavelength mercury lamp light source with a dose of 1260mJ / cm 2 , using m-xylene as the developer, developing for 10 seconds, and obtaining a line pattern with a half-pitch of 10 μm (see Appendix Figure 4 ).
[0084] Example 2
[0085] Dissolve 0.157 g of bis(diphenylphosphino)methane in 16 mL of dichloromethane, add 0.136 g of silver acetate, and stir until a clear solution is obtained. Filter, concentrate the solution, and cool it to produce a white precipitate. Separate the precipitate, recrystallize it from dichloromethane / n-hexane, and sample the crystals for H NMR testing (see Appendix). Figure 6 , H NMR spectrum δ2.02 (CH3), δ3.31 (CH2), δ7.0-7.5 (C6H5)). The crystal structure is as attached. Figure 5 As shown, the molecular formula is Ag4(dppm)2(CH3COO)4 and it was dried in vacuum at room temperature.
[0086] Weigh 0.5g Ag4(dppm)2(CH3COO)4 and 0.05g N-hydroxynaphthalimide trifluoromethanesulfonate, dissolve in 0.945g propylene glycol monomethyl ether acetate, and filter the solution three times with a 0.22μm filter. The dynamic light scattering particle size test showed that the average particle size was 1.7nm (see Appendix Figure 7 ). Set the coating machine speed to 2000rpm, the time is 1min, and a uniform photoresist film is spin-coated on the silicon wafer. Then, the wafer is placed on a hot plate at 80℃ and heated for 1min. The above wafer is exposed to a 254nm wavelength mercury lamp light source with a dose of 2000mJ / cm 2 , using o-xylene as the developer, developing for 15 seconds, and obtaining a line pattern with a half-pitch of 10 μm (see Appendix Figure 8 ).
[0087] Example 3
[0088] Dissolve 0.104 g of Ag4(dppm)2(CH3COO)4 crystals in 30 mL of methanol, add 0.056 g of bis(diphenylphosphine)methane, and stir until a clear solution is obtained. Filter, concentrate the solution, and cool it to form a precipitate. Separate the precipitate, recrystallize it in dichloromethane / n-hexane, separate the precipitate, and sample the crystals for H NMR testing (see Appendix). Fig.10 , among which, the H NMR spectrum is δ2.12 (CH3), δ3.36 (CH2), δ6.95-7.45 (C6H5)), and the crystal structure is as attached Fig. 9 As shown, the molecular formula is Ag2(dppm)2(CH3COO)2 and it was dried in vacuum at room temperature.
[0089] Weigh 0.5 g Ag2(dppm)2(OAc)2 and 0.05 g N-hydroxynaphthaleneimide trifluoromethanesulfonate, dissolve in 0.945 g propylene glycol monomethyl ether acetate, and filter the solution three times with a 0.22 μm filter. The dynamic light scattering particle size test showed that the average particle size was 1.3 nm (see Appendix). Fig.11). Set the coating machine speed to 2000rpm, the time is 1min, and a uniform photoresist film is spin-coated on the silicon wafer. Then, the wafer is placed on a hot plate at 80℃ and heated for 1min. The above wafer is exposed to a 254nm wavelength mercury lamp light source with a dose of 270mJ / cm 2 , using m-xylene as the developer, developing for 30 seconds to obtain a line pattern with a half-pitch of 10 μm (see Appendix Fig.12 ).
[0090] In summary, the present invention obtains a variety of effective nanoparticles and corresponding compositions, verifies the structure and has good lithography performance under mid-ultraviolet and electron beam conditions, which can achieve better lithography performance such as high resolution, high sensitivity, and low line roughness.
Claims
1. An Ag-based organic coordination nanoparticle, characterized in that: The general formula is: [Ag m (R) n (Q) x ] y , the ranges of m, n, x, and y are all 1-4; Wherein, R is selected from bis(diphenylphosphino)methane (dppm), bis(dicyclohexylphosphino)methane (abbreviated dcpm), bis(diphenylamino)methane, N,N-bis(diphenylphosphino)amine (abbreviated dppa), N,N,N',N'-tetramethyldiaminomethane, N,N,N',N'-tetraethyldiaminomethane; Q is selected from CH3COO, C2H5COO, C3H7COO, i-C3H7COO, C4H9COO, C6H 13 COO, C9H 19 COO, C6H5COO, CF3COO, C2F5COO, C3F7COO, i-C3F7COO, C4F9COO, C6F 13 COO, C9F 19 COO, C6H5COO.
2. The Ag-based organic coordination nanoparticles according to claim 1, characterized in that: Its specific structure is: Ag2(dppm)2(CH3COO)2; Ag4(dppm)2(CH3COO)4; Ag4(dppm)2(CF3COO)4; Ag2(dppm)2(C2H5COO)2; Ag4(dppm)2(C2F5COO)4; Ag4(dppm)2(C4F9COO)4; Ag2(dcpm)2(CH3COO)2; Ag4(dppa)2(CH3COO)4.
3. The Ag-based organic coordination nanoparticles according to claim 1, characterized in that: The size of the Ag-based organic coordination nanoparticle crystal is 1nm-4nm.
4. The method for preparing Ag-based organic coordination nanoparticles according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: adding silver salt and a first organic ligand into a sample bottle respectively, adding an organic solvent to dissolve them, stirring for a certain time under certain temperature conditions, filtering, concentrating, cooling crystallization or evaporation crystallization, and finally recrystallizing in an organic solvent to obtain Ag-based organic coordination nanoparticles, wherein the ratio of the silver salt to the first organic ligand is 1:(0.5-1).
5. The method for preparing Ag-based organic coordination nanoparticles according to claim 4, characterized in that: The organic solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-ethoxy-2-propanol, tetrahydrofuran, methanol, ethanol, propanol, dichloromethane and chloroform.
6. The method for preparing Ag-based organic coordination nanoparticles according to claim 4, characterized in that: The stirring temperature is controlled at 0-120°C.
7. A photoresist composition comprising the Ag-based organic coordination nanoparticles according to any one of claims 1 to 3, and further comprising a photoinitiator and an organic dispersing solvent, wherein: The photoinitiator occupies 0.1 wt%-10 wt% of the composition, and the Ag-based organic coordination nanoparticles occupies 1 wt%-20 wt% of the composition.
8. The photoresist composition according to claim 7, characterized in that The photoinitiator is selected from any one or more of N-hydroxynaphthaleneimide trifluoromethanesulfonic acid, 1,4-aminonaphthalenesulfonic acid, 2-amino-5,7-naphthalene disulfonic acid, tert-butylphenyl iodonium salt perfluorooctanesulfonic acid, triphenylsulfonium perfluorobutanesulfonic acid, triphenylsulfonium perfluorobutyl and triphenylsulfonium trifluorosulfonic acid.
9. The photoresist composition according to claim 7, characterized in that: The organic dispersing solvent is selected from any one or more of ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, propylene glycol methyl ether acetate, 1-methoxy-2-propanol, propylene glycol mono-n-propyl ether, propylene glycol butyl ether, 1-ethoxy-2-propanol, methanol, ethanol, and propanol.
10. A method for patterning Ag organic coordinated nanoparticle photoresist, comprising: using the photoresist composition as claimed in any one of claims 7 to 9, dripping the photoresist composition onto a substrate by spin coating, heating it on a hot stage, exposing it to electron beam or mid-ultraviolet, deep ultraviolet or extreme ultraviolet light, and developing it with a developer, wherein the spin coating speed is 1000 to 6000 rpm; the heating temperature of the hot stage is controlled at 50 to 110° C., the heating time is controlled at 30 to 900 s, and the exposure dose is 50 to 8000 mJ / cm 2The developer is selected from a mixture of any one or more of decahydronaphthalene, tetrahydronaphthalene, indene, indane, quinoline, 1-methylnaphthalene, toluene, o-xylene, m-xylene, ethyl acetate, butyl acetate, ethanol, n-propanol, isopropanol, n-butanol, n-hexane and cyclohexane, and the developing temperature is room temperature or 20°C to 50°C; the thickness of the pre-film layer after removing the organic dispersing solvent can be 10nm to 100nm.
11. Use of the Ag-based organic coordination nanoparticles according to any one of claims 1 to 3 for electron beam, mid-ultraviolet, deep ultraviolet and / or extreme ultraviolet photoresists.
Citation Information
Patent Citations
Metal peroxo compounds with organic co-ligands for electron beam, deep uv and extreme uv photoresist applications
CN104145217A
Photoactive, inorganic ligand-capped inorganic nanocrystals
CN110832618A
Photoresist composition and method of forming thin film pattern and array substrate using same
CN111766762A
Photoresist and patterning method of imine material
CN111880371A
Photoresist composition based on metal nanoparticles and application thereof
CN114089599A
Cited By
Method for improving smoothness of micro-nano structure through photoresist pretreatment process
CN121115410A