Hydrophilic porous silicon dioxide in-situ polymerization modified polyester and preparation method thereof

By combining a water-soluble copolyester dispersant with a dynamic mixer, highly uniform dispersion of hydrophilic porous silica in polyester was achieved, solving the problem of dispersion difficulties and meeting the processing requirements of high-quality fibers and films.

CN119019658APending Publication Date: 2024-11-26CHINESE TEXTILE ACAD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310610108.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve highly uniform dispersion of hydrophilic porous silica in polyester matrices, leading to operational difficulties and safety hazards, and making it difficult to meet the processing requirements of high-quality fibers and films.

Method used

A water-soluble copolyester dispersant was used to pre-disperse hydrophilic porous silica. Combined with the design of a dynamic mixer and an esterification reactor, in-situ uniform dispersion of porous silica in polyester was achieved through jet injection and high shear force.

Benefits of technology

This method achieves highly uniform dispersion of hydrophilic porous silica in polyester, meeting the processing requirements of high-quality fibers and films, and reducing operational difficulty and safety hazards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019658A_ABST
    Figure CN119019658A_ABST
Patent Text Reader

Abstract

The invention provides hydrophilic porous silicon dioxide in-situ polymerization modified polyester and a preparation method thereof, and belongs to the technical field of high polymer material synthesis. The method comprises the following steps: dissolving a water-soluble copolyester dispersing agent consisting of terephthalic acid, ethylene glycol, m-phthalic acid-5-sulfonate and polyethylene glycol structural units in water; adding hydrophilic porous silicon dioxide into the solution of the dispersing agent, and grinding to obtain an aqueous dispersion liquid of the hydrophilic porous silicon dioxide; blending the aqueous dispersion liquid of the hydrophilic porous silicon dioxide, terephthalic acid and ethylene glycol; breaking a hydrogen bond cross-linked three-dimensional network structure agglomerate between the hydrophilic porous silicon dioxide in the pre-dispersed slurry; and carrying out esterification reaction, pre-polycondensation reaction and final polycondensation reaction to obtain the hydrophilic porous silicon dioxide in-situ polymerization modified polyester. The polyester is continuously prepared by the method. By applying the preparation method, the in-situ polymerization modified polyester in which hydrophilic porous silicon dioxide is highly uniformly dispersed can be continuously prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer material synthesis, in particular to a hydrophilic porous silica in-situ polymerization modified polyester and a preparation method thereof. Background Art

[0002] Hydrophilic porous silica is a three-dimensional honeycomb porous nano-silica with the characteristics of low density, high porosity, high specific surface area, low thermal conductivity, etc. At the same time, it also shows unique properties in light absorption, thermal resistance, magnetism, negative ions, antistatic and catalysis, and is an important inorganic nano-material for regulating the function of fiber materials. Due to the large specific surface area, low density and light powder of hydrophilic porous silica, during the melt mixing process with polyester, on the one hand, it is very easy to cause a lot of dust during the feeding process of hydrophilic porous silica, causing operational difficulties and safety hazards; on the other hand, the density difference between hydrophilic porous silica and polyester is huge, and it is difficult to achieve a highly uniform dispersion of hydrophilic porous silica in the polyester matrix by relying solely on the mechanical shear force provided by the mixing equipment. Summary of the invention

[0003] In view of this, the present invention provides a hydrophilic porous silica in-situ polymerization modified polyester and a preparation method thereof. By using the preparation method, the hydrophilic porous silica in-situ polymerization modified polyester with highly uniform dispersion can be continuously prepared, thereby being more suitable for practical use.

[0004] In order to achieve the above first object, the technical scheme of the preparation method of hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention is as follows:

[0005] The method for preparing hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention comprises the following steps:

[0006] A water-soluble copolyester dispersant composed of terephthalic acid, ethylene glycol, isophthalic acid-5-sulfonate, and polyethylene glycol structural units in a molar ratio of (60-92):(91-100):(8-40):(0-9) is dissolved in water to obtain a solution of the water-soluble copolyester dispersant, wherein the molecular weight of the polyethylene glycol structural unit in the water-soluble copolyester dispersant is 600-3000;

[0007] Adding hydrophilic porous silica to the solution of the dispersant and grinding to obtain an aqueous dispersion of hydrophilic porous silica, wherein in the aqueous dispersion of hydrophilic porous silica, the specific surface area of ​​the hydrophilic porous silica is greater than or equal to 100 m 2 / g, the mass percentage of hydrophilic porous silica is 3 to 30wt%, and the content of water-soluble copolyester dispersant is 5 to 50wt% of the total mass of hydrophilic porous silica;

[0008] The aqueous dispersion of the hydrophilic porous silica, terephthalic acid, and ethylene glycol are mixed to obtain a pre-dispersed slurry, wherein the mass percentage of water in the pre-dispersed slurry is less than or equal to 6wt%, and the molar ratio of terephthalic acid to ethylene glycol is 1.08 to 2.0;

[0009] breaking hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica in the pre-dispersed slurry to obtain a reaction stock solution;

[0010] The reaction stock solution is subjected to an esterification reaction to obtain a hydrophilic porous silica in-situ polymerization-modified polyester oligomer;

[0011] The hydrophilic porous silica in-situ polymerization-modified polyester oligomer undergoes a pre-polycondensation reaction and a final polycondensation reaction in sequence to obtain the hydrophilic porous silica in-situ polymerization-modified polyester.

[0012] The method for preparing the hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention can also be further implemented by adopting the following technical measures.

[0013] Preferably, before the step of breaking up the hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica in the pre-dispersed slurry to obtain the reaction stock solution, the step also includes preheating the pre-dispersed slurry, wherein the preheating of the pre-dispersed slurry is completed in a preheater, and the temperature of the preheater is 60-100°C.

[0014] Preferably, the step of breaking up the hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica in the pre-dispersed slurry to obtain the reaction stock solution is completed in a dynamic mixer.

[0015] Preferably, during the step of subjecting the reaction stock solution to an esterification reaction to obtain a hydrophilic porous silica in-situ polymerization-modified polyester oligomer, the reaction stock solution is injected into the esterification reactor in the form of a jet, wherein the flow rate of the jet is greater than or equal to 3 m / s.

[0016] Preferably, the esterification reactor comprises a reactor container shell, a reaction stock solution inlet pipeline (1), an esterification steam pipeline (10), a hydrophilic porous silica in-situ polymerization modified oligomer discharge pipeline (3), and a gas baffle (9).

[0017] The reaction stock solution inlet pipeline (1) is arranged at the bottom of the reactor container shell;

[0018] The esterification steam pipeline (10) is arranged on the top of the shell of the reactor container;

[0019] The hydrophilic porous silica in-situ polymerization modified oligomer discharge pipeline (3) is arranged at the bottom of the reactor container shell;

[0020] The gas baffle (9) is arranged in the inner cavity of the reactor container, and the arrangement position of the gas baffle (9) is lower than the outlet of the esterification steam pipeline (10), so that the esterification steam pipeline (10) must pass through the maze passage formed by the gas baffle (9) before reaching the outlet of the esterification steam pipeline (10).

[0021] Preferably, the bottom of the esterification reactor including the reactor container shell is low in the middle and high at the edges, and the hydrophilic porous silica in-situ polymerization modified oligomer discharge pipeline (3) is arranged at the lowest point of the esterification reactor including the reactor container shell.

[0022] Preferably, the method for preparing hydrophilic porous silica in-situ polymerization-modified polyester further comprises a jet flow rate regulator (2).

[0023] The jet flow rate regulator (2) is arranged on the reaction stock solution inlet pipeline (1) and is used to adjust the flow rate and / or injection angle of the reaction stock solution injected into the esterification reaction kettle in the form of a jet.

[0024] Preferably, the method for preparing hydrophilic porous silica in-situ polymerization-modified polyester further comprises a rotating motor, a stirring shaft (5) and a tangential flow stirring paddle (4).

[0025] One end of the stirring shaft (5) is fixedly connected to the output shaft of the rotating motor;

[0026] The tangential flow stirring blade (4) is fixedly connected to the other end of the stirring shaft (5).

[0027] Preferably, the method for preparing hydrophilic porous silica in-situ polymerization-modified polyester further comprises an axial stirring blade (6), a guide tube (7),

[0028] The guide tube (7) is arranged on the periphery of the stirring shaft (5).

[0029] The axial stirring paddle (6) is fixedly connected to the stirring shaft (5), and the rotation radius of the axial stirring paddle (6) is less than or equal to the radius of the guide tube (7).

[0030] Preferably, an angle θ is formed between the line connecting the incident point of the jet flow rate regulator (2) on the reactor vessel shell, the corresponding point on the bottom edge of the guide tube (7), and the stirring shaft (5), and the angle is 15°≤θ≤75°.

[0031] Preferably, the method for preparing the hydrophilic porous silica in-situ polymerization modified polyester further comprises a heating coil (8),

[0032] The heating coil (8) is arranged in the middle and lower part of the inner cavity of the esterification reaction kettle.

[0033] Preferably, the shape of the gas baffle (9) is "W"-shaped or "V"-shaped, and the number of installed layers of the gas baffle (9) is single-layer or multi-layer.

[0034] Preferably, in the step of adding hydrophilic porous silica to the dispersant solution and grinding to obtain an aqueous dispersion of hydrophilic porous silica, an average dispersed particle size of the hydrophilic porous silica in the aqueous dispersion is less than or equal to 1000 nm.

[0035] Preferably, the preheater is selected from at least one of a tube bundle heat exchanger and a shell and tube heat exchanger.

[0036] Preferably, the shear unit of the dynamic mixer comprises a shear stator and a shear rotor, the shear unit has 2 to 5 stages, the interval width between the shear stator and the rotor is less than or equal to 2 mm, and the rotation speed of the shear rotor is 1400 to 3000 rpm.

[0037] Preferably, in the step of subjecting the reaction stock solution to an esterification reaction to obtain a hydrophilic porous silica in-situ polymerized modified polyester oligomer, the esterification rate of the hydrophilic porous silica in-situ polymerized modified polyester oligomer is 89-97%.

[0038] In order to achieve the above second purpose, the technical scheme of hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention is as follows:

[0039] The hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention is continuously prepared by the preparation method of the hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention.

[0040] The intrinsic viscosity of the hydrophilic porous silica in-situ polymerized modified polyester is 0.5 to 0.8 dL / g.

[0041] The hydrophilic porous silica in-situ polymerization modified polyester has a hydrophilic porous silica content of 0.3-4.0 wt %.

[0042] The filter pressure value FPV of the filter with a filtration accuracy of 2μm is less than or equal to 1.5MPa.cm 2 / g.

[0043] The invention provides a method for preparing hydrophilic porous silica in-situ polymerization modified polyester, which can realize the continuous production of the hydrophilic porous silica in-situ polymerization modified polyester with highly uniform dispersion.

[0044] The hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention has a filtration pressure value FPV less than or equal to 1.5 MPa.cm through a filter screen with a filtration accuracy of 2 μm. 2 / g, which can meet the processing requirements of high-quality fibers, films and other products. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0046] Figure 1 A process flow chart of the preparation method of the hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention;

[0047] Figure 2 The present invention provides a schematic structural diagram of an esterification reaction kettle with a gas baffle for preparing a hydrophilic porous silica in-situ polymerization-modified polyester used in the process provided by the present invention. DETAILED DESCRIPTION

[0048] In view of this, the present invention provides a hydrophilic porous silica in-situ polymerization modified polyester and a preparation method thereof. By using the preparation method, the hydrophilic porous silica in-situ polymerization modified polyester with highly uniform dispersion can be continuously prepared, thereby being more suitable for practical use.

[0049] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the following is a detailed description of a hydrophilic porous silica in-situ polymerization modified polyester and its preparation method according to the present invention, its specific implementation method, structure, characteristics and effects, in conjunction with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures, or characteristics in one or more embodiments can be combined in any suitable form.

[0050] The term "and / or" in this article is merely a description of the association relationship of associated objects, indicating that three relationships may exist, for example, A and / or B. Specifically, it is understood that: A and B may be included at the same time, A may exist alone, or B may exist alone, and any of the above three situations may be met.

[0051] Preparation method of hydrophilic porous silica in-situ polymerization modified polyester

[0052] See attached Figure 1 The method for preparing hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention comprises the following steps:

[0053] A water-soluble copolyester dispersant composed of terephthalic acid, ethylene glycol, isophthalic acid-5-sulfonate, and polyethylene glycol structural units in a molar ratio of (60-92):(91-100):(8-40):(0-9) is dissolved in water to obtain a solution of the water-soluble copolyester dispersant, wherein the molecular weight of the polyethylene glycol structural unit in the water-soluble copolyester dispersant is 600-3000. The molar ratio of terephthalic acid, ethylene glycol, isophthalic acid-5-sulfonate, and polyethylene glycol structural units is controlled within the above range, and the prepared water-soluble copolyester dispersant has good compatibility with hydrophilic porous silica and polyester. The molecular weight of the polyethylene glycol structural unit is controlled within the above range, which can give the prepared water-soluble copolyester dispersant good solubility and good affinity with hydrophilic porous silica.

[0054] Adding hydrophilic porous silica to the solution of the dispersant and grinding the mixture to obtain an aqueous dispersion of the hydrophilic porous silica, wherein the specific surface area of ​​the hydrophilic porous silica in the aqueous dispersion of the hydrophilic porous silica is greater than or equal to 100 m 2 / g, the mass percentage of hydrophilic porous silica is 3-30wt%, and the content of water-soluble copolyester dispersant is 5-50wt% of the total mass of hydrophilic porous silica. By controlling the content of porous silica in the aqueous dispersion of hydrophilic porous silica and the mass fraction of the water-soluble copolyester dispersant relative to the hydrophilic porous silica within the above ranges, highly stable ultrafine dispersion of the hydrophilic porous silica in the aqueous solution can be achieved.

[0055] The aqueous dispersion of hydrophilic porous silica, terephthalic acid and ethylene glycol are prepared to obtain a pre-dispersed slurry, wherein the mass percentage of water in the pre-dispersed slurry is less than or equal to 6wt%, and the molar ratio of terephthalic acid to ethylene glycol is 1.08 to 2.0. Controlling the water content in the pre-dispersed slurry within the above range is conducive to avoiding the agglomeration of the hydrophilic porous silica due to the rapid evaporation of water when the slurry is injected into the high-temperature material of the esterification reactor. Controlling the molar ratio of terephthalic acid to ethylene glycol within the above range, terephthalic acid has good slurrying properties, and the slurry is conducive to the full esterification reaction of terephthalic acid after entering the esterification reactor.

[0056] breaking hydrogen-bonded cross-linked three-dimensional network structure agglomerates between hydrophilic porous silica in the pre-dispersed slurry to obtain a reaction stock solution;

[0057] The reaction stock solution is subjected to an esterification reaction to obtain a hydrophilic porous silica in-situ polymerization-modified polyester oligomer;

[0058] The hydrophilic porous silica in-situ polymerization-modified polyester oligomer undergoes a pre-polycondensation reaction and a final polycondensation reaction in sequence to obtain the hydrophilic porous silica in-situ polymerization-modified polyester.

[0059] Before the step of breaking the hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica in the pre-dispersed slurry to obtain the reaction stock solution, the step of preheating the pre-dispersed slurry is also included, wherein the preheating of the pre-dispersed slurry is completed in a preheater, and the temperature of the preheater is 60-100° C. Heating the slurry prepared by the aqueous dispersion of hydrophilic porous silica, terephthalic acid, and ethylene glycol to the above temperature range is conducive to the swelling of small molecules of ethylene glycol into the three-dimensional network structure agglomerates of porous silica.

[0060] The step of breaking up the hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica in the pre-dispersed slurry to obtain the reaction stock solution is completed in a dynamic mixer.

[0061] In the step of obtaining the hydrophilic porous silica in-situ polymerized modified polyester oligomer by esterification of the reaction stock solution, the reaction stock solution is injected into the esterification reactor in the form of a jet, wherein the jet flow rate is greater than or equal to 3 m / s. The flow rate of the high-speed jet of the preheated slurry injected into the esterification reactor with a gas baffle is controlled within the above range, which will produce an entrainment effect, so that the hydrophilic porous silica in the preheated slurry is quickly dispersed in the entrained polyester oligomer.

[0062] Among them, see Appendix Figure 2 The esterification reactor comprises a reactor container shell, a reaction stock solution inlet pipeline 1, an esterification steam pipeline 10, a hydrophilic porous silica in-situ polymerization modified oligomer discharge pipeline 3, and a gas baffle 9. The reaction stock solution inlet pipeline 1 is arranged at the bottom of the reactor container shell; the esterification steam pipeline 10 is arranged at the top of the reactor container shell; the hydrophilic porous silica in-situ polymerization modified oligomer discharge pipeline 3 is arranged at the bottom of the reactor container shell; the gas baffle 9 is arranged in the inner cavity of the reactor container, and the gas baffle 9 is arranged at a position lower than the outlet of the esterification steam pipeline 10, so that the esterification steam pipeline 10 must pass through the labyrinth passage formed by the gas baffle 9 before reaching the outlet of the esterification steam pipeline 10. A gas baffle is installed in the gas phase space above the esterification reactor so that the esterification steam enters the gas phase pipeline after being baffled by the gas baffle, which can effectively prevent the esterification steam from entraining high specific surface area and ultra-low density hydrophilic porous silica powder into the gas phase pipeline.

[0063] The bottom of the esterification reactor including the reactor container shell is low in the middle and high at the edges, and the hydrophilic porous silica in-situ polymerization modified oligomer discharge pipeline 3 is arranged at the lowest point of the esterification reactor including the reactor container shell.

[0064] The method for preparing hydrophilic porous silica in-situ polymerization modified polyester further comprises a jet flow rate regulator 2. The jet flow rate regulator 2 is arranged on the reaction stock solution inlet pipeline 1, and is used to adjust the flow rate and / or injection angle of the reaction stock solution injected into the esterification reactor in the form of a jet.

[0065] The method for preparing hydrophilic porous silica in-situ polymerization modified polyester further comprises a rotating motor, a stirring shaft 5 and a tangential flow stirring paddle 4. One end of the stirring shaft 5 is fixedly connected to the output shaft of the rotating motor; the tangential flow stirring paddle 4 is fixedly connected to the other end of the stirring shaft 5.

[0066] Among them, the preparation method of hydrophilic porous silica in-situ polymerization modified polyester also includes an axial stirring paddle 6 and a guide tube 7. The guide tube 7 is arranged on the periphery of the stirring shaft 5, the axial stirring paddle 6 is fixedly connected to the stirring shaft 5, and the rotation radius of the axial stirring paddle 6 is less than or equal to the radius of the guide tube 7. The stirring system of the esterification reactor includes a combined agitator and a guide tube composed of a lower tangential flow stirring paddle and an upper axial flow stirring paddle. The lower tangential flow stirring paddle of the agitator is arranged below the guide tube and in the lower head of the esterification reactor, and its diameter is greater than the inner diameter of the guide tube. The tangential flow stirring paddle arranged in the lower head of the esterification reactor and rotating at a high speed has a strong shear force, which can realize the rapid shear dispersion of high specific surface area and ultra-low density hydrophilic silica particles in the preheated slurry injected from the lower head of the esterification reactor in the form of a high-speed jet. The diameter of the tangential flow stirring paddle is greater than the inner diameter of the guide tube, which is conducive to reducing the velocity retention area of ​​the stirring fluid in the lower head of the esterification reactor. The tangential flow impeller can be selected from a straight blade open turbine impeller, a slanted blade open turbine impeller or a curved blade open turbine impeller. The upper axial flow impeller of the agitator is arranged in the middle of the guide tube. Through the combination of the axial flow impeller and the guide tube, the fluid in the esterification reactor can have a high circulation flow rate, so that the high specific surface area and ultra-low density hydrophilic silica particles in the preheated slurry injected in the form of a high-speed jet can be quickly diffused in the esterification reactor. The axial flow impeller is selected from a variable-section spiral arc impeller, a propeller propeller or a slanted blade impeller.

[0067] Among them, the line between the incident point of the jet flow rate regulator 2 on the reactor container shell and the corresponding point of the bottom edge of the guide tube 7 and the stirring shaft 5 has an angle θ, 15°≤θ≤75°. A slurry injection flow rate regulator is set on the lower head of the esterification reactor. The slurry injection flow rate can be controlled by adjusting the flow area of ​​the slurry annular injection port, so that the preheated slurry is injected into the polyester oligomer in the form of a high-speed jet, and the hydrophilic porous silica in the preheated slurry is quickly dispersed in the entrained polyester oligomer through the entrained suction effect. By setting the injection direction of the slurry injection flow rate regulator to be inclined with the stirring shaft of the esterification reactor agitator, the angle θ between the two is controlled within the range of 15°≤θ≤75°; injecting the preheated slurry from the lower head of the esterification reactor within this inclination angle range is conducive to the rapid dispersion of the preheated slurry in the polyester oligomer in the esterification reactor, and avoiding the agglomeration of high specific surface area and ultra-low density hydrophilic porous silica particles.

[0068] The method for preparing hydrophilic porous silica in-situ polymerization modified polyester further comprises a heating coil 8. The heating coil 8 is arranged in the middle and lower part of the inner cavity of the esterification reaction kettle.

[0069] The shape of the gas baffle plate 9 is "W"-shaped or "V"-shaped, and the number of gas baffle plates 9 installed is single-layer or multi-layer.

[0070] In the step of adding hydrophilic porous silica to a dispersant solution and grinding to obtain an aqueous dispersion of hydrophilic porous silica, the average dispersed particle size of the hydrophilic porous silica in the aqueous dispersion is less than or equal to 1000 nm. By controlling the average dispersed particle size of the hydrophilic porous silica in the aqueous dispersion of the hydrophilic porous silica within the above range, an in-situ polymerization-modified polyester in which the hydrophilic porous silica is highly uniformly dispersed can be prepared.

[0071] The preheater is selected from at least one of a tube bundle heat exchanger and a shell-and-tube heat exchanger. Both the tube bundle heat exchanger and the shell-and-tube heat exchanger are plug flow heat exchangers and have the advantage of a large heat exchange area. As a slurry preheater, the slurry temperature can be adjusted within a large temperature range without back-mixing problems. Of the tube bundle heat exchangers and the shell-and-tube heat exchangers, the tube bundle heat exchanger is more preferred because the tube bundle heat exchanger has a heat exchange tube winding structure that can further homogenize the pre-dispersed slurry.

[0072] The shear unit of the dynamic mixer includes a shear stator and a shear rotor, the number of stages of the shear unit is 2 to 5, the gap width between the shear stator and the rotor is less than or equal to 2 mm, and the speed of the shear rotor is 1400 to 3000 rpm. The number of stages of the shear unit composed of the shear stator and the rotor, the gap width between the shear stator and the rotor, and the speed of the shear rotor of the dynamic mixer are controlled within the above range. Under the high tangential speed generated by the high-speed rotation of the shear rotor of the dynamic mixer, the hydrophilic porous silica three-dimensional network structure agglomerates in the preheated slurry are subjected to strong hydraulic shear, centrifugal extrusion, impact tearing and turbulence in the narrow gap between the shear stator and the rotor in the shear unit. The three-dimensional network structure agglomerates formed by hydrogen bond crosslinking of the hydrophilic porous silica are decomposed into monodisperse aggregates, which can significantly reduce the viscosity of the preheated slurry while achieving ultrafine dispersion of the hydrophilic porous silica in the preheated slurry.

[0073] In the step of obtaining the hydrophilic porous silica in-situ polymerization-modified polyester oligomer by esterification of the reaction stock solution, the esterification rate of the hydrophilic porous silica in-situ polymerization-modified polyester oligomer is 89-97%. The esterification rate of the hydrophilic porous silica in-situ polymerization-modified polyester oligomer is controlled within the above range to meet the requirements of the subsequent pre-polycondensation reaction on the esterification rate of the oligomer.

[0074] In-situ polymerization of hydrophilic porous silica to modify polyester

[0075] The hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention is continuously prepared by the preparation method of the hydrophilic porous silica in-situ polymerization modified polyester provided by the present invention.

[0076] The intrinsic viscosity of the hydrophilic porous silica in-situ polymerized modified polyester is 0.5 to 0.8 dL / g.

[0077] The content of hydrophilic porous silica in the hydrophilic porous silica in-situ polymerization modified polyester is 0.3-4.0 wt %.

[0078] The filter pressure value FPV of the filter with a filtration accuracy of 2μm is less than or equal to 1.5MPa.cm 2 / g.

[0079] By controlling the intrinsic viscosity within the above range, the molecular weight of the hydrophilic porous silica in-situ polymerization modified polyester can meet the requirements of melt spinning and film drawing and other molding processes. The filtration pressure value FPV of the hydrophilic porous silica in-situ polymerization modified polyester is not higher than 1.5MPa.cm through a filter with a filtration accuracy of 2μm. 2 / g, which can meet the processing requirements of high-quality fibers, films and other products.

[0080] Example 1

[0081] S1, dissolving a water-soluble copolyester dispersant having a molar ratio of terephthalic acid, ethylene glycol, isophthalic acid-5-sulfonate and a polyethylene glycol structural unit having a molecular weight of 2000 in water in a stirring tank, then adding hydrophilic porous silica and uniformly mixing with a high shear stirrer to obtain a pre-dispersed liquid, continuously conveying the pre-dispersed liquid to a sand mill unit composed of three sand mills in series, grinding and dispersing the pre-dispersed liquid to obtain an aqueous dispersion of hydrophilic porous silica, wherein the specific surface area of ​​the hydrophilic porous silica is 200m 2 / g, the content of hydrophilic porous silica in the aqueous dispersion is 20wt%, the dispersed particle size is 90nm, and the content of water-soluble copolyester dispersant is 10wt% of the total mass of hydrophilic porous silica

[0082] S2, preparing a pre-dispersed slurry with an aqueous dispersion of hydrophilic porous silica, terephthalic acid and ethylene glycol in a slurry mixing tank, wherein the molar ratio of ethylene glycol to terephthalic acid is 1.1, the amount of the aqueous dispersion of hydrophilic porous silica added is 11.8wt% of the total mass of terephthalic acid, and the water content in the pre-dispersed slurry is 6.0wt%.

[0083] S3, transporting the pre-dispersed slurry to a slurry preheating tank, and preparing a preheated slurry with a temperature of 80° C. by heating and swelling.

[0084] S4, after the preheated slurry is broken by a dynamic mixer into the hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica, it is injected into the esterification reactor in the form of a high-speed jet, and the hydrophilic porous silica in-situ polymerization modified polyester oligomer is obtained through esterification reaction. The dynamic mixer shear unit stage number is 3, the gap width between the shear stator and the rotor is 2mm, the speed of the shear rotor is 1500 rpm, and the flow rate of the high-speed jet of the preheated slurry injected into the esterification reactor is 5m / s; the esterification reaction is carried out in two esterification reactors connected in series in sequence, the temperatures of the two esterification reactors are 255°C and 260°C respectively, and the esterification rate of the prepared hydrophilic porous silica in-situ polymerization modified polyester oligomer is 97%.

[0085] S5, continuously conveying the hydrophilic porous silica in situ polymerization modified polyester oligomer to the pre-polycondensation system for pre-polycondensation reaction to obtain the hydrophilic porous silica in situ polymerization modified polyester prepolymer; the pre-polycondensation reaction system consists of a pre-polycondensation reactor, and the reaction temperature is 275°C. When the intrinsic viscosity of the hydrophilic porous silica in situ polymerization modified polyester prepolymer reaches 0.20dL / g, it is continuously conveyed to the final polycondensation system for final polycondensation reaction to obtain the hydrophilic porous silica in situ polymerization modified polyester. The final polycondensation system consists of a final polycondensation reactor, and the reaction temperature is 280°C.

[0086] When the characteristic viscosity of the hydrophilic porous silica in-situ polymerization modified polyester melt reaches 0.67dL / g, it is continuously transported from the final polycondensation reactor to the casting head and sequentially undergoes casting, cooling, pelletizing and drying processes to obtain in-situ polymerization modified polyester chips with a hydrophilic porous silica content of 2wt%.

[0087] Example 2

[0088] S1, dissolving a water-soluble copolyester dispersant having a molar ratio of terephthalic acid, ethylene glycol, isophthalic acid-5-sulfonate and a polyethylene glycol structural unit having a molecular weight of 3000 in water in a stirring tank, then adding hydrophilic porous silica and uniformly mixing with a high shear stirrer to obtain a pre-dispersed liquid, continuously conveying the pre-dispersed liquid to a sand mill unit composed of two sand mills in series, grinding and dispersing the pre-dispersed liquid to obtain an aqueous dispersion of hydrophilic porous silica, wherein the specific surface area of ​​the hydrophilic porous silica is 100m 2 / g, the content of hydrophilic porous silica in the aqueous dispersion is 40wt%, the dispersed particle size is 80nm, and the content of water-soluble copolyester dispersant is 5wt% of the total mass of hydrophilic porous silica

[0089] S2, preparing a pre-dispersed slurry by mixing an aqueous dispersion of hydrophilic porous silica with terephthalic acid and ethylene glycol in a slurry mixing tank, wherein the molar ratio of ethylene glycol to terephthalic acid is 1.08, the amount of the aqueous dispersion of hydrophilic porous silica added is 12 wt% of the total mass of terephthalic acid, and the water content in the pre-dispersed slurry is 4.6 wt%.

[0090] S3, transporting the pre-dispersed slurry to a slurry preheating tank, and preparing a preheated slurry with a temperature of 80° C. by heating and swelling.

[0091] S4, after the preheated slurry is broken by a dynamic mixer into the hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica, it is injected into the esterification reactor in the form of a high-speed jet, and the hydrophilic porous silica in-situ polymerization modified polyester oligomer is obtained through esterification reaction. The dynamic mixer shear unit stage number is 3, the gap width between the shear stator and the rotor is 2mm, the speed of the shear rotor is 2000 rpm, and the flow rate of the high-speed jet of the preheated slurry injected into the esterification reactor is 3m / s; the esterification reaction is carried out in two esterification reactors connected in series, the temperatures of the two esterification reactors are 260℃ and 265℃ respectively, and the esterification rate of the prepared hydrophilic porous silica in-situ polymerization modified polyester oligomer is 97%.

[0092] S5, continuously conveying the hydrophilic porous silica in situ polymerization modified polyester oligomer to the pre-condensation system for pre-condensation reaction to obtain the hydrophilic porous silica in situ polymerization modified polyester prepolymer; the pre-condensation reaction system consists of two pre-condensation reaction kettles connected in series, and the temperatures of the two pre-condensation reaction kettles are 270°C and 275°C, respectively. When the characteristic viscosity of the hydrophilic porous silica in situ polymerization modified polyester prepolymer reaches 0.30dL / g, it is continuously conveyed to the final polycondensation system for final polycondensation reaction to obtain the hydrophilic porous silica in situ polymerization modified polyester. The final polycondensation system consists of one final polycondensation reaction kettle, and the reaction temperature is 285°C.

[0093] When the characteristic viscosity of the hydrophilic porous silica in-situ polymerization modified polyester melt reaches 0.50dL / g, it is continuously transported from the final polycondensation reactor to the casting head and sequentially undergoes casting, cooling, pelletizing and drying processes to obtain in-situ polymerization modified polyester chips with a hydrophilic porous silica content of 4wt%.

[0094] Example 3

[0095] S1, dissolving a water-soluble copolyester dispersant having a molar ratio of 60:92:40:8 of terephthalic acid, ethylene glycol, isophthalic acid-5-sulfonate and a polyethylene glycol structural unit with a molecular weight of 600 in water in a stirring tank, then adding hydrophilic porous silica and uniformly mixing with a high shear stirrer to obtain a pre-dispersed liquid, continuously conveying the pre-dispersed liquid to a sand mill unit composed of 5 sand mills in series, grinding and dispersing to obtain an aqueous dispersion of hydrophilic porous silica, wherein the specific surface area of ​​the hydrophilic porous silica is 1000m 2 / g, the content of hydrophilic porous silica in the aqueous dispersion is 3wt%, the dispersed particle size is 1000nm, and the content of water-soluble copolyester dispersant is 50wt% of the total mass of hydrophilic porous silica

[0096] S2, preparing a pre-dispersed slurry with an aqueous dispersion of hydrophilic porous silica, terephthalic acid and ethylene glycol in a slurry mixing tank, wherein the molar ratio of ethylene glycol to terephthalic acid is 2, the amount of the aqueous dispersion of hydrophilic porous silica added is 11.6wt% of the total mass of terephthalic acid, and the water content in the pre-dispersed slurry is 5.9wt%.

[0097] S3, transporting the pre-dispersed slurry to a slurry preheating tank, and preparing a preheated slurry with a temperature of 100° C. by heating and swelling.

[0098] S4, after the preheated slurry is broken by a dynamic mixer into the hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica, it is injected into the esterification reactor in the form of a high-speed jet, and the hydrophilic porous silica in-situ polymerization modified polyester oligomer is obtained through esterification reaction. The dynamic mixer shear unit stage is 2, the gap width between the shear stator and the rotor is 1mm, the speed of the shear rotor is 3000 rpm, and the flow rate of the high-speed jet of the preheated slurry injected into the esterification reactor is 5m / s; the esterification reaction is carried out in two esterification reactors connected in series, the temperatures of the two esterification reactors are 255°C and 260°C respectively, and the esterification rate of the prepared hydrophilic porous silica in-situ polymerization modified polyester oligomer is 97%.

[0099] S5, continuously conveying the hydrophilic porous silica in situ polymerization modified polyester oligomer to the pre-condensation system for pre-condensation reaction to obtain the hydrophilic porous silica in situ polymerization modified polyester prepolymer; the pre-condensation reaction system consists of two pre-condensation reaction kettles connected in series, and the temperatures of the two pre-condensation reaction kettles are 280°C and 285°C, respectively. When the characteristic viscosity of the hydrophilic porous silica in situ polymerization modified polyester prepolymer reaches 0.40dL / g, it is continuously conveyed to the final polycondensation system for final polycondensation reaction to obtain the hydrophilic porous silica in situ polymerization modified polyester. The final polycondensation system consists of one final polycondensation reaction kettle, and the reaction temperature is 290°C.

[0100] When the characteristic viscosity of the hydrophilic porous silica in-situ polymerization modified polyester melt reaches 0.80dL / g, it is continuously transported from the final polycondensation reactor to the casting head and sequentially undergoes casting, cooling, pelletizing and drying processes to obtain in-situ polymerization modified polyester chips with a hydrophilic porous silica content of 0.3wt%.

[0101] Example 4

[0102] S1, dissolving a water-soluble copolyester dispersant having a molar ratio of terephthalic acid, ethylene glycol, isophthalic acid-5-sulfonate and a polyethylene glycol structural unit having a molecular weight of 1000 in water in a stirring tank, then adding hydrophilic porous silica and uniformly mixing with a high shear stirrer to obtain a pre-dispersed liquid, continuously conveying the pre-dispersed liquid to a sand mill unit composed of five sand mills in series, grinding and dispersing the pre-dispersed liquid to obtain an aqueous dispersion of hydrophilic porous silica, wherein the specific surface area of ​​the hydrophilic porous silica is 800 m 2 / g, the content of hydrophilic porous silica in the aqueous dispersion is 10wt%, the dispersed particle size is 800nm, and the content of water-soluble copolyester dispersant is 40wt% of the total mass of hydrophilic porous silica

[0103] S2, preparing a pre-dispersed slurry by mixing an aqueous dispersion of hydrophilic porous silica with terephthalic acid and ethylene glycol in a slurry mixing tank, wherein the molar ratio of ethylene glycol to terephthalic acid is 1.15, the amount of the aqueous dispersion of hydrophilic porous silica added is 9.3wt% of the total mass of terephthalic acid, and the water content in the pre-dispersed slurry is 5.3wt%.

[0104] S3, transporting the pre-dispersed slurry to a slurry preheating tank, and preparing a preheated slurry with a temperature of 100° C. by heating and swelling.

[0105] S4, after the preheated slurry is broken by a dynamic mixer into the hydrogen bond cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica, it is injected into the esterification reactor in the form of a high-speed jet, and the hydrophilic porous silica in-situ polymerization modified polyester oligomer is obtained through esterification reaction. The number of shear units of the dynamic mixer is 3, the gap width between the shear stator and the rotor is 1mm, the speed of the shear rotor is 2000 rpm, and the flow rate of the high-speed jet of the preheated slurry injected into the esterification reactor is 5m / s; the esterification reaction is carried out in two esterification reactors connected in series, the temperatures of the two esterification reactors are 260°C and 265°C respectively, and the esterification rate of the prepared hydrophilic porous silica in-situ polymerization modified polyester oligomer is 97%.

[0106] S5, continuously conveying the hydrophilic porous silica in situ polymerization modified polyester oligomer to the pre-polycondensation system for pre-polycondensation reaction to obtain the hydrophilic porous silica in situ polymerization modified polyester prepolymer; the pre-polycondensation reaction system consists of a pre-polycondensation reactor, and the reaction temperature is 280°C. When the intrinsic viscosity of the hydrophilic porous silica in situ polymerization modified polyester prepolymer reaches 0.22dL / g, it is continuously conveyed to the final polycondensation system for final polycondensation reaction to obtain the hydrophilic porous silica in situ polymerization modified polyester. The final polycondensation system consists of a final polycondensation reactor, and the reaction temperature is 285°C.

[0107] When the characteristic viscosity of the hydrophilic porous silica in-situ polymerization modified polyester melt reaches 0.62dL / g, it is continuously transported from the final polycondensation reactor to the casting head and sequentially undergoes casting, cooling, pelletizing and drying processes to obtain in-situ polymerization modified polyester chips with a hydrophilic porous silica content of 0.8wt%.

[0108] Example 5

[0109] S1, dissolving a water-soluble copolyester dispersant having a molar ratio of 85:91:25:9 of terephthalic acid, ethylene glycol, isophthalic acid-5-sulfonate and a polyethylene glycol structural unit having a molecular weight of 1000 in water in a stirring tank, then adding hydrophilic porous silica and uniformly mixing with a high shear stirrer to obtain a pre-dispersed liquid, continuously conveying the pre-dispersed liquid to a sand mill unit composed of five sand mills in series, grinding and dispersing the pre-dispersed liquid to obtain an aqueous dispersion of hydrophilic porous silica, wherein the specific surface area of ​​the hydrophilic porous silica is 600 m 2 / g, the content of hydrophilic porous silica in the aqueous dispersion is 15wt%, the dispersed particle size is 500nm, and the content of water-soluble copolyester dispersant is 40wt% of the total mass of hydrophilic porous silica

[0110] S2, preparing a pre-dispersed slurry by mixing an aqueous dispersion of hydrophilic porous silica with terephthalic acid and ethylene glycol in a slurry mixing tank, wherein the molar ratio of ethylene glycol to terephthalic acid is 1.20, the amount of the aqueous dispersion of hydrophilic porous silica added is 11.7wt% of the total mass of terephthalic acid, and the water content in the pre-dispersed slurry is 5.9wt%.

[0111] S3, transporting the pre-dispersed slurry to a slurry preheating tank, and preparing a preheated slurry with a temperature of 60° C. by heating and swelling.

[0112] S4, after the preheated slurry is broken into the hydrogen bond cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica by a dynamic mixer, it is injected into the esterification reactor in the form of a high-speed jet, and the hydrophilic porous silica in-situ polymerization modified polyester oligomer is obtained through esterification reaction. The number of shear units of the dynamic mixer is 3, the gap width between the shear stator and the rotor is 1mm, the speed of the shear rotor is 2000 rpm, and the flow rate of the high-speed jet of the preheated slurry injected into the esterification reactor is 5m / s; the esterification reaction is carried out in two esterification reactors connected in series, the temperatures of the two esterification reactors are 255°C and 260°C respectively, and the esterification rate of the prepared hydrophilic porous silica in-situ polymerization modified polyester oligomer is 97%.

[0113] S5, continuously conveying the hydrophilic porous silica in situ polymerization modified polyester oligomer to the pre-polycondensation system for pre-polycondensation reaction to obtain the hydrophilic porous silica in situ polymerization modified polyester prepolymer; the pre-polycondensation reaction system consists of a pre-polycondensation reactor, and the reaction temperature is 275°C. When the intrinsic viscosity of the hydrophilic porous silica in situ polymerization modified polyester prepolymer reaches 0.20dL / g, it is continuously conveyed to the final polycondensation system for final polycondensation reaction to obtain the hydrophilic porous silica in situ polymerization modified polyester. The final polycondensation system consists of a final polycondensation reactor, and the reaction temperature is 280°C.

[0114] When the characteristic viscosity of the hydrophilic porous silica in-situ polymerization modified polyester melt reaches 0.55dL / g, it is continuously transported from the final polycondensation reactor to the casting head and sequentially undergoes casting, cooling, pelletizing and drying processes to obtain in-situ polymerization modified polyester chips with a hydrophilic porous silica content of 1.5wt%.

[0115] Example 6

[0116] S1, dissolving a water-soluble copolyester dispersant having a molar ratio of terephthalic acid, ethylene glycol, and isophthalic acid-5-sulfonate structural units of 80:100:20 in water in a stirring tank, then adding hydrophilic porous silica and uniformly mixing with a high shear stirrer to obtain a pre-dispersed liquid, which is continuously conveyed to a sand mill unit composed of three sand mills in series for grinding and dispersion to obtain an aqueous dispersion of hydrophilic porous silica, wherein the specific surface area of ​​the hydrophilic porous silica is 300 m 2 / g, the content of hydrophilic porous silica in the aqueous dispersion is 20wt%, the dispersed particle size is 169nm, and the content of water-soluble copolyester dispersant is 20wt% of the total mass of hydrophilic porous silica

[0117] S2, preparing a pre-dispersed slurry with an aqueous dispersion of hydrophilic porous silica, terephthalic acid and ethylene glycol in a slurry mixing tank, wherein the molar ratio of ethylene glycol to terephthalic acid is 2, the amount of the aqueous dispersion of hydrophilic porous silica added is 11.8wt% of the total mass of terephthalic acid, and the water content in the pre-dispersed slurry is 4.8wt%.

[0118] S3, transporting the pre-dispersed slurry to a slurry preheating tank, and preparing a preheated slurry with a temperature of 80° C. by heating and swelling.

[0119] S4, after the preheated slurry is broken into hydrogen bond cross-linked three-dimensional network structure agglomerates between hydrophilic porous silica by a dynamic mixer, it is injected into an esterification reactor in the form of a high-speed jet, and a hydrophilic porous silica in-situ polymerization modified polyester oligomer is obtained through an esterification reaction. The number of shear units of the dynamic mixer is 3, the gap width between the shear stator and the rotor is 1 mm, the speed of the shear rotor is 1400 rpm, and the flow rate of the high-speed jet of the preheated slurry injected into the esterification reactor is 4 m / s; the esterification reaction is carried out in an esterification reactor at a reaction temperature of 260°C, and the esterification rate of the prepared hydrophilic porous silica in-situ polymerization modified polyester oligomer is 89%.

[0120] S5, continuously conveying the hydrophilic porous silica in-situ polymerization modified polyester oligomer to the pre-condensation system for pre-condensation reaction to obtain the hydrophilic porous silica in-situ polymerization modified polyester prepolymer; the pre-condensation reaction system consists of a pre-condensation reactor, and the reaction temperature is 285°C. When the characteristic viscosity of the hydrophilic porous silica in-situ polymerization modified polyester prepolymer reaches 0.30dL / g, it is continuously conveyed to the final polycondensation system for final polycondensation reaction to obtain the hydrophilic porous silica in-situ polymerization modified polyester. The final polycondensation system consists of a final polycondensation reactor, and the reaction temperature is 280°C.

[0121] When the characteristic viscosity of the hydrophilic porous silica in-situ polymerization modified polyester melt reaches 0.60dL / g, it is continuously transported from the final polycondensation reactor to the casting head and sequentially undergoes casting, cooling, pelletizing and drying processes to obtain in-situ polymerization modified polyester chips with a hydrophilic porous silica content of 2wt%.

[0122] Comparative Example 1

[0123] Compared with Example 1, in this comparative example, only the flow rate of the preheated slurry injected into the esterification reaction kettle in step S4 is reduced to 0.9 m / s, and the other implementation methods are the same as those in Example 1.

[0124] Comparative Example 2

[0125] Compared with Example 1, the high shear dispersion of the preheated slurry by the dynamic mixer in step S4 is eliminated in this comparative example, and the other implementation methods are the same as those in Example 1.

[0126] Comparative Example 3

[0127] Compared with Example 1, the temperature of the slurry preheating tank in step S3 is lowered to 50° C., and the other implementation methods are the same as those in Example 1.

[0128] Comparative Example 4

[0129] Compared with Example 1, the water-soluble copolyester in step S1 is replaced with polypropylene glycol with a molecular weight of 600, and the other implementation methods are the same as those in Example 1.

[0130] Experimental Example 1

[0131] The hydrophilic porous silica in-situ polymerization modified polyester prepared in Examples 1 to 6 and Comparative Examples 1 to 4 was subjected to a filter pressure value FPV test through a filter screen with a filtration accuracy of 2 μm. The test method is as follows:

[0132] Filter Pressure Value (FPV) of Hydrophilic Porous Silica In-situ Polymerization Modified Polyester (MPa.cm 2 / g), defined as the pressure increase value generated by each gram of hydrophilic porous silica on the filter per unit area. The test method is: a single screw extruder with an aspect ratio of Φ25mm×25D, a melt metering pump with a volume of 1.2cc, a melt pressure sensor and an effective filtration area S of 6.15cm 2 The filter screens with a filtration accuracy of 2 μm are connected in sequence to form a filter press performance tester; the process conditions for the filter press performance test are: the melt temperature is 295°C, the pre-pump pressure setting value of the melt metering pump is 6.5 MPa, and the metering flow rate of the melt metering pump is 38 g / min; first, 500 g of polyester polyethylene terephthalate is extruded from the filter press performance tester, and the equilibrium pressure is recorded as the initial pressure Ps, then 4000 g of functional polyester is extruded from the filter press performance tester, and then 500 g of polyester polyethylene terephthalate is extruded from the filter press performance tester, and the equilibrium pressure is recorded as the termination pressure Pt, and finally according to the formula: FPV = (P t -P s )×6.15 / m c The filter pressure value FPV is calculated, where: FPV is the filter pressure value, the unit is MPa.cm 2 / g; Ps is the initial pressure, in MPa; Pt is the final pressure, in MPa; mc is the mass of the hydrophilic porous silica powder in the test sample, in g. The test results are shown in Table 1.

[0133] Table 1

[0134] <![CDATA[Filter pressure value FPV (MPa·cm 2 / g)]]> Example 1 0.37 Example 2 0.30 Example 3 1.50 Example 4 1.19 Example 5 0.93 Example 6 0.62 Comparative Example 1 0.73 Comparative Example 2 0.52 Comparative Example 3 0.49 Comparative Example 4 1.83

[0135] It can be seen from the data in Table 1 that the FPV of the hydrophilic porous silica in-situ polymerization modified polyester produced by the continuous production method of the present invention is not higher than 1.5 MPa.cm through a filter with a filtration accuracy of 2 μm. 2 / g, indicating that the hydrophilic porous silica in the polyester matrix modified by in-situ polymerization of the hydrophilic porous silica produced by the continuous production method of the present invention has a smaller dispersed particle size.

[0136] Compared with Example 1, in Comparative Example 1, only the flow rate of the preheated slurry injected into the esterification reactor in step S4 is reduced to 0.9 m / s, and the other implementation methods are the same as those in Example 1, but the filter pressure value of the prepared hydrophilic porous silica in-situ polymerization modified polyester is increased to 0.73 MPa.cm 2 The filter pressure value of the hydrophilic porous silica in-situ polymerization modified polyester prepared in Example 1 is increased by 0.36 MPa.cm 2 / g. This shows that compared with Comparative Example 2, the dispersed particle size of the hydrophilic porous silica in the polyester modified by in-situ polymerization of the hydrophilic porous silica prepared in Example 1 is smaller. Since the flow rate of the high-speed jet of the preheated slurry injected into the esterification reactor in Example 1 is controlled at 5m / s, this will produce an entrainment effect, so that the hydrophilic porous silica in the preheated slurry is quickly dispersed in the entrained polyester oligomer.

[0137] Compared with Example 1, Comparative Example 2 cancels the high shear dispersion of the preheated slurry by the dynamic mixer in step S4. The other implementation methods are the same as those in Example 1, but the filter pressure value of the prepared hydrophilic porous silica in-situ polymerization modified polyester is increased to 0.52 MPa.cm 2 The filter pressure value of the hydrophilic porous silica in-situ polymerization modified polyester prepared in Example 1 is increased by 0.15 MPa.cm 2 / g. This shows that compared with Comparative Example 2, the dispersed particle size of the hydrophilic porous silica in the in-situ polymerization-modified polyester prepared by Example 1 is smaller. Due to the high tangential speed generated by the high-speed rotation of the shear rotor of the dynamic mixer in Example 1, the three-dimensional network structure agglomerates of the hydrophilic porous silica in the preheated slurry are subjected to the combined effects of strong hydraulic shear, centrifugal extrusion, impact tearing and turbulence in the narrow gap between the shear stator and the rotor in the shear unit, so that the three-dimensional network structure agglomerates of the hydrophilic porous silica formed by hydrogen bond cross-linking are decomposed into monodisperse aggregates, which can significantly reduce the viscosity of the preheated slurry while achieving ultrafine dispersion of the hydrophilic porous silica in the preheated slurry.

[0138] Compared with Example 1, in Comparative Example 3, the temperature of the slurry preheating tank in step S3 is reduced to 50°C. The other implementation methods are the same as those in Example 1, but the filter pressure value of the prepared hydrophilic porous silica in-situ polymerization modified polyester is increased to 0.49 MPa.cm 2 The filter pressure value of the hydrophilic porous silica in-situ polymerization modified polyester prepared in Example 1 is increased by 0.12 MPa.cm 2 / g. This shows that compared with Comparative Example 3, the hydrophilic porous silica in the in-situ polymerization-modified polyester prepared in Example 1 has a smaller dispersed particle size. Since the pre-dispersed slurry in Example 1 is heated and swelled at 80°C in the slurry preheating tank, it is beneficial for the small molecules of ethylene glycol to swell and enter the porous silica three-dimensional network structure agglomerates.

[0139] Compared with Example 1, in Comparative Example 4, the water-soluble copolyester in step S1 is replaced by polypropylene glycol with a molecular weight of 600. The other implementation methods are the same as those in Example 1, but the filter pressure value of the prepared hydrophilic porous silica in-situ polymerization modified polyester is increased to 1.83 MPa.cm 2The filter pressure value of the hydrophilic porous silica in-situ polymerization modified polyester prepared in Example 1 is increased by 1.46 MPa.cm 2 / g. This shows that compared with Comparative Example 4, the dispersed particle size of the hydrophilic porous silica in the polyester modified by in-situ polymerization of the hydrophilic porous silica prepared in Example 1 is smaller. Since in Example 1, the water-soluble copolyester with a molar ratio of terephthalic acid, ethylene glycol, isophthalic acid-5-sulfonate and polyethylene glycol structural units with a molecular weight of 2000 of 80:97.4:20:2.6 is used as the dispersant of the hydrophilic porous silica, the hydrophilic porous silica will be endowed with good affinity with both polyester and water, which is conducive to the efficient dispersion of the hydrophilic porous silica in the high-temperature polyester material.

[0140] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0141] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing hydrophilic porous silica in-situ polymerization modified polyester, It is characterized in that The following steps are involved: A water-soluble copolyester dispersant composed of terephthalic acid, ethylene glycol, isophthalic acid-5-sulfonate, and polyethylene glycol structural units in a molar ratio of (60-92):(91-100):(8-40):(0-9) is dissolved in water to obtain a solution of the water-soluble copolyester dispersant, wherein the molecular weight of the polyethylene glycol structural unit in the water-soluble copolyester dispersant is 600-3000; Adding hydrophilic porous silica to the solution of the dispersant and grinding to obtain an aqueous dispersion of hydrophilic porous silica, wherein in the aqueous dispersion of hydrophilic porous silica, the specific surface area of ​​the hydrophilic porous silica is greater than or equal to 100 m 2 / g, the mass percentage of hydrophilic porous silica is 3 to 30wt%, and the content of water-soluble copolyester dispersant is 5 to 50wt% of the total mass of hydrophilic porous silica; The aqueous dispersion of the hydrophilic porous silica, terephthalic acid, and ethylene glycol are mixed to obtain a pre-dispersed slurry, wherein the mass percentage of water in the pre-dispersed slurry is less than or equal to 6wt%, and the molar ratio of terephthalic acid to ethylene glycol is 1.08 to 2.0; breaking hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica in the pre-dispersed slurry to obtain a reaction stock solution; The reaction stock solution is subjected to an esterification reaction to obtain a hydrophilic porous silica in-situ polymerization-modified polyester oligomer; The hydrophilic porous silica in-situ polymerization-modified polyester oligomer undergoes a pre-polycondensation reaction and a final polycondensation reaction in sequence to obtain the hydrophilic porous silica in-situ polymerization-modified polyester.

2. The method for preparing the hydrophilic porous silica in-situ polymerization modified polyester according to claim 1, It is characterized in that Before the step of breaking up the hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica in the pre-dispersed slurry to obtain the reaction stock solution, the step also includes preheating the pre-dispersed slurry, wherein the preheating of the pre-dispersed slurry is completed in a preheater, and the temperature of the preheater is 60-100°C.

3. The method for preparing the hydrophilic porous silica in-situ polymerization modified polyester according to claim 1, It is characterized in that The step of breaking the hydrogen-bonded cross-linked three-dimensional network structure agglomerates between the hydrophilic porous silica in the pre-dispersed slurry to obtain the reaction stock solution is completed in a dynamic mixer.

4. The method for preparing the hydrophilic porous silica in-situ polymerization modified polyester according to claim 1, It is characterized in that During the step of obtaining the hydrophilic porous silica in-situ polymerization-modified polyester oligomer by esterification of the reaction stock solution, the reaction stock solution is injected into the esterification reaction kettle in the form of a jet, wherein the flow rate of the jet is greater than or equal to 3 m / s.

5. The method for preparing the hydrophilic porous silica in-situ polymerization modified polyester according to claim 4, It is characterized in that The esterification reactor comprises a reactor container shell, a reaction stock solution inlet pipeline (1), an esterification steam pipeline (10), a hydrophilic porous silica in-situ polymerization modified oligomer discharge pipeline (3), and a gas baffle (9). The reaction stock solution inlet pipeline (1) is arranged at the bottom of the reactor container shell; The esterification steam pipeline (10) is arranged on the top of the shell of the reactor container; The hydrophilic porous silica in-situ polymerization modified oligomer discharge pipeline (3) is arranged at the bottom of the reactor container shell; The gas baffle (9) is arranged in the inner cavity of the reactor container, and the arrangement position of the gas baffle (9) is lower than the outlet of the esterification steam pipeline (10), so that the esterification steam pipeline (10) must pass through the maze passage formed by the gas baffle (9) before reaching the outlet of the esterification steam pipeline (10).

6. The method for preparing the hydrophilic porous silica in-situ polymerization modified polyester according to claim 5, It is characterized in that The bottom of the esterification reactor including the reactor container shell is in a shape of low in the middle and high at the edges, and the hydrophilic porous silica in-situ polymerization modified oligomer discharge pipeline (3) is arranged at the lowest point of the esterification reactor including the reactor container shell.

7. The method for preparing the hydrophilic porous silica in-situ polymerization modified polyester according to claim 5, It is characterized in that It also includes a jet flow rate regulator (2), The jet flow rate regulator (2) is arranged on the reaction stock solution inlet pipeline (1) and is used to adjust the flow rate and / or injection angle of the reaction stock solution injected into the esterification reaction kettle in the form of a jet.

8. The method for preparing the hydrophilic porous silica in-situ polymerization modified polyester according to claim 7, It is characterized in that It also includes a rotating motor, a stirring shaft (5) and a tangential flow stirring blade (4), One end of the stirring shaft (5) is fixedly connected to the output shaft of the rotating motor; The tangential flow stirring blade (4) is fixedly connected to the other end of the stirring shaft (5).

9. The method for preparing the hydrophilic porous silica in-situ polymerization modified polyester according to claim 8, It is characterized in that It also includes an axial stirring blade (6) and a guide tube (7). The guide tube (7) is arranged on the periphery of the stirring shaft (5). The axial stirring paddle (6) is fixedly connected to the stirring shaft (5), and the rotation radius of the axial stirring paddle (6) is less than or equal to the radius of the guide tube (7); Preferably, an angle θ is formed between the line connecting the incident point of the jet flow rate regulator (2) on the shell of the reactor container and the corresponding point of the bottom edge of the guide tube (7) and the stirring shaft (5), and the angle is 15°≤θ≤75°; Preferably, the method for preparing the hydrophilic porous silica in-situ polymerization modified polyester further comprises a heating coil (8), The heating coil (8) is arranged in the middle and lower part of the inner cavity of the esterification reaction kettle; Preferably, the shape of the gas baffle (9) is "W"-shaped or "V"-shaped, and the number of installed layers of the gas baffle (9) is single-layer or multi-layer; Preferably, in the step of adding hydrophilic porous silica to the dispersant solution and grinding to obtain an aqueous dispersion of hydrophilic porous silica, an average dispersed particle size of the hydrophilic porous silica in the aqueous dispersion is less than or equal to 1000 nm; Preferably, the preheater is selected from at least one of a tube bundle heat exchanger and a shell and tube heat exchanger; Preferably, the shear unit of the dynamic mixer comprises a shear stator and a shear rotor, the number of stages of the shear unit is 2 to 5, the interval width between the shear stator and the rotor is less than or equal to 2 mm, and the rotation speed of the shear rotor is 1400 to 3000 rpm; Preferably, in the step of subjecting the reaction stock solution to an esterification reaction to obtain a hydrophilic porous silica in-situ polymerized modified polyester oligomer, the esterification rate of the hydrophilic porous silica in-situ polymerized modified polyester oligomer is 89-97%.

10. A hydrophilic porous silica in-situ polymerization modified polyester, It is characterized in that The hydrophilic porous silica in-situ polymerization-modified polyester is continuously prepared by the preparation method of the hydrophilic porous silica in-situ polymerization-modified polyester according to any one of claims 1 to 9. The intrinsic viscosity of the hydrophilic porous silica in-situ polymerized modified polyester is 0.5 to 0.8 dL / g. The hydrophilic porous silica in-situ polymerization modified polyester has a hydrophilic porous silica content of 0.3-4.0 wt %. The filter pressure value FPV of the filter with a filtration accuracy of 2μm is less than or equal to 1.5MPa.cm 2 / g.