Thermally-induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material and preparation method thereof
Through the copolymerization and heat-induced crosslinking technology of phenolphthaleinyl diamine and benzyl diamine, a heat-induced crosslinking phenolphthaleinyl polybenzoxazole film was formed, which solved the problem of plasticization of polyimide film under high pressure and significantly improved the Gas separation performance and structural stability are achieved.
Patent Information
- Application Number
- CN202310594564.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-24
AI Technical Summary
Polyimide gas separation membrane materials are prone to plasticization under high pressure, resulting in poor gas separation performance, and traditional crosslinking methods may damage the membrane structure.
Phenolphthaleinyl diamine is used as diamine monomer to form a heat-induced crosslinking phenolphthaleinyl polybenzoxazole gas separation film material through heat-induced crosslinking and heat rearrangement reaction. Combined with benzyl diamine copolymerization, it improves the anti-plasticization ability and crosslinking degree.
It significantly improves gas permeability and selectivity, avoids membrane structure damage, enhances the anti-plasticization performance and structural stability of the polymer, and increases CO2 flux by more than 120 times.
Smart Images

Figure CN119019684A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of membrane separation, and in particular relates to a thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material and a preparation method thereof. Background Art
[0002] As a green separation technology, gas separation membranes have the advantages of low cost, low energy consumption, simple operation, high selectivity, high efficiency and easy scale-up compared with traditional separation methods. Among them, polyimide gas separation membranes have high gas selectivity, excellent thermal stability, good mechanical properties and good film-forming properties, and are considered to be a promising gas separation material. However, traditional polyimide membranes have low gas permeability and are prone to plasticization when separating gases with high concentrations of soluble gases (such as CO2 and CH4). Plasticization refers to a phenomenon in which the mobility and free volume of polymer segments increase with the increase of feed side pressure, thereby increasing the permeability of gas separation membranes and sharply reducing selectivity. In order to improve the gas separation performance of polyimide, rigid large side groups cardo groups can be introduced into the polymer main chain to reduce the bulk density of the polymer, increase the free volume, and increase the gas permeability.
[0003] A new type of phenolphthalein diamine reacts with 6FDA to generate polyimide Ac-6FDA-DAP. This cardo group polymer can be thermally decarboxylated and self-crosslinked at 300-350°C, and can also undergo thermal rearrangement at 375-450°C to form a polybenzoxazole structure. Thermally induced crosslinking can prevent it from plasticizing at 30atm, and TR can significantly increase gas permeability by 3.5-20 times. (DuP, Wang Z, Zhang T, et al. Journal of Membrane Science. 2022, 662: 120934.)
[0004] The methods for synthesizing polyimide include one-step method, two-step method and three-step method. The two-step method is divided into chemical imidization and thermal imidization. Chemical imidization is to add a dehydrating agent and a catalyst to close the ring after the polyamic acid is formed; thermal imidization is to heat the polyamic acid solution to 180-200°C and add an azeotropic drying agent, such as toluene, to help remove the water formed in the polyamic acid ring closure reaction. (Omole IC, Miller SJ, Koros W J. Macromolecules. 2008, 41 (17): 6367-6375.)
[0005] Copolymerized polyimide provides the possibility of preparing membranes with gas permeability and selectivity that cannot be obtained with homopolyimide. In addition, copolymerized polyimide can be directly prepared from currently known monomers, and the physical or chemical properties of polyimide can be changed by changing the comonomer ratio. Even more, by copolymerizing a polyimide with high selectivity but low permeability with a polyimide with high permeability, it is possible to combine a polyimide gas separation membrane material with both high permeability and high selectivity. (Wang L, Cao Y, Zhou M, et al. Journal of Membrane Science. 2007, 305 (1-2): 338-346.)
[0006] Benzyl-induced cross-linking is a general method for cross-linking polymer membranes, which aims to improve the gas separation performance of polymers and enhance the stability of membranes. This method is based on the aromatic methyl substituents in benzyl polyimide as cross-linking reaction sites. The cross-linking reaction occurs at 250°C in air, which is much lower than the decomposition temperature of most polyimides (usually above 430°C), ensuring the integrity of the polymer backbone structure. The phenylization thermal oxidative cross-linking reaction gives the prepared membrane a high CO2 / CH4 separation selectivity and high permeability. (Zhu S, Wang Z, Shi Y, et al. Macromolecules. 2022, 55(15): 6890-6900.)
[0007] The presence of a large number of benzene rings in the phenolphthalein group gives this type of polymer excellent thermal stability, and the presence of the lactone ring structure gives this type of polymer good solubility. The aromatic heterocyclic structure of the side group reduces the density of the polymer and increases the free volume, which is beneficial to improving the gas separation performance of the polyimide membrane material. Benzyl polyimide generally has high permeability, and the benzyl group can achieve thermal oxidation cross-linking. Summary of the invention
[0008] The purpose of the present invention is to address some deficiencies in the preparation process of polyimide gas separation membrane materials and the problem of unsatisfactory gas separation performance, and select phenolphthalein diamine, which contains a large cardo side group, is low in price and easy to obtain. After obtaining the polyimide membrane, a heat-induced self-crosslinking treatment is performed below the glass transition temperature, which not only obtains an excellent three-dimensional network structure, but also avoids the destruction of the polymer membrane structure. The present invention uses 3,3'-diaminophenolphthalein as the phenolphthalein diamine, and uses the azeotropic distillation method to retain the hydroxyl groups on the phenolphthalein diamine, so that a large number of hydrogen bonds exist on the polyimide polymer chain, thereby improving its anti-plasticization ability, and can further improve the problem of low gas permeability of homopolymerized phenolphthalein polyimide by adding benzyl diamine for copolymerization.
[0009] In order to achieve the above-mentioned object, the first aspect of the present invention provides a thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material, the structural formula of which is shown in Formula I:
[0010]
[0011] Wherein, R1, R2, and R3 are each independently H or C1-C4 alkyl;
[0012] m1, m2, m and n represent the number of repeating units, m1, m2, m are between 20 and 500, n is 0, or n is between 20 and 500;
[0013] Ar is a linking unit of a dianhydride anhydride group, the dianhydride anhydride group is derived from a dianhydride monomer, and the dianhydride monomer is at least one of pyromellitic anhydride, pyrophthalic anhydride, biphenyltetracarboxylic anhydride, hexafluoroisopropylphthalic anhydride, benzophenonetetracarboxylic anhydride and oxydiphthalic anhydride.
[0014] The structures of the dianhydride monomers are as follows:
[0015]
[0016]
[0017] According to the present invention, preferably, the heat-induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, heat-induced cross-linking, and thermal rearrangement reactions of diamine monomers and dianhydride monomers.
[0018] According to the present invention, preferably, the diamine monomer is 3,3'-diaminophenolphthalein, or the diamine monomer is 3,3'-diaminophenolphthalein and benzyldiamine.
[0019] According to the present invention, preferably, n is between 20 and 500, and the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is selected from any one of the following:
[0020] (i) Formula I wherein R1 = CH3, R2 = H, R3 = H;
[0021] (ii) Formula I wherein R1=CH3, R2=CH3, R3=H or R1=H, R2=CH3, R3=CH3;
[0022] (iii) Formula I wherein R1=CH3, R2=CH3, R3=CH3;
[0023] (iv) Formula I wherein R1 = CH3, R2 = CH2CH3, R3 = H or R1 = CH2CH3, R2 = CH3, R3 = H;
[0024] (v) In formula I, R1=CH3, R2=CH2CH3, R3=CH2CH3 or R1=CH2CH3, R2=CH2CH3, R3=CH3.
[0025] According to the present invention, preferably, when R1=CH3, R2=H, and R3=H in formula I, the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, thermally induced cross-linking, and thermal rearrangement reaction of monomer (a), 3,3'-diaminophenolphthalein, and dianhydride monomer;
[0026] 2-Methyl-1,3-phenylenediamine.
[0027] When R1=CH3, R2=CH3, R3=H or R1=H, R2=CH3, R3=CH3 in formula I, the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, thermally induced cross-linking, and thermal rearrangement reaction of monomer (b), 3,3'-diaminophenolphthalein and dianhydride monomer;
[0028] 2,4-dimethyl-1,3-phenylenediamine or 2,4-dimethyl-1,5-phenylenediamine.
[0029] When R1=CH3, R2=CH3, R3=CH3 in formula I, the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, thermally induced cross-linking, and thermal rearrangement reaction of monomer (c), 3,3'-diaminophenolphthalein and dianhydride monomer;
[0030] 2,4,6-Trimethyl-1,3-phenylenediamine.
[0031] When R1=CH3, R2=CH2CH3, R3=H or R1=CH2CH3, R2=CH3, R3=H in formula I, the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, thermally induced cross-linking, and thermal rearrangement reaction of monomer (d), 3,3'-diaminophenolphthalein and dianhydride monomer;
[0032] 2-methyl-4-ethyl-1,3-phenylenediamine or 4-methyl-2-ethyl-1,5-phenylenediamine.
[0033] When R1=CH3, R2=CH2CH3, R3=CH2CH3 or R1=CH2CH3, R2=CH2CH3, R3=CH3 in formula I, the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, thermally induced cross-linking, and thermal rearrangement reaction of monomer (e), 3,3'-diaminophenolphthalein and dianhydride monomer;
[0034] Diethyltoluenediamine.
[0035] The second aspect of the present invention provides a method for preparing a heat-induced cross-linked phenolphthalein polybenzoxazole gas separation membrane material, the method comprising the following steps:
[0036] (1) under the protection of an inert gas, contacting a diamine monomer, a first solvent and a dianhydride monomer to carry out an imidization reaction to obtain a polyimide; the dianhydride monomer is at least one selected from pyromellitic anhydride, pyromellitic anhydride, biphenyltetracarboxylic anhydride, hexafluoroisopropylphthalic anhydride, benzophenone tetracarboxylic anhydride and oxydiphthalic anhydride; the diamine monomer is 3,3'-diaminophenolphthalein, or the diamine monomer is 3,3'-diaminophenolphthalein and benzyldiamine; the benzyldiamine is at least one selected from 2-methyl-1,3-phenylenediamine, 2,4-dimethyl-1,3-phenylenediamine, 2,4-dimethyl-1,5-phenylenediamine, 2,4,6-trimethyl-1,3-phenylenediamine, 2-methyl-4-ethyl-1,3-phenylenediamine, 4-methyl-2-ethyl-1,5-phenylenediamine and diethyltoluenediamine;
[0037] (2) Preparation of dense polyimide film
[0038] The polyimide obtained in step (1) is dissolved in a first solvent, and filtered to prepare a dense polyimide membrane;
[0039] (3) Heat-induced cross-linking treatment of dense membrane
[0040] In an air atmosphere, the polyimide dense film dried in step (2) is heated to 300-400° C. and kept warm to obtain the heat-induced cross-linked dense film;
[0041] (4) Thermal rearrangement
[0042] Under a nitrogen atmosphere, the heat-induced cross-linked dense membrane prepared in step (3) is heated to 400-450° C. and kept warm to obtain the heat-induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material.
[0043] According to the present invention, preferably, step (1) comprises: dissolving the diamine monomer in the first solvent under low-temperature ice bath and nitrogen protection, stirring evenly, adding the dianhydride monomer in batches so that the concentration of the diamine monomer and dianhydride monomer solution is 25-35w%, continuously stirring and reacting for 20-30h until a high-viscosity polyamic acid solution is formed, removing the ice bath, then adding an azeotropic desiccant and stirring until the mixture is evenly mixed, heating to 180-200°C for thermal imidization reaction, the reaction time is 4-8h, forming a high-viscosity polyimide solution, stopping heating and adding the first solvent for dilution, and finally pouring the obtained polyimide solution into methanol for precipitation, crushing the precipitate, filtering and washing, removing the residual solvent, and then subjecting the obtained polyimide to programmed temperature drying.
[0044] In the present invention, the diamine monomer is dissolved in the first solvent, the stirring time is 20 to 40 minutes in a low-temperature ice bath and under nitrogen protection, the stirring time after adding the azeotropic desiccant is 20 to 40 minutes, and the amount of the first solvent added is such that the concentration of the diamine monomer and dianhydride monomer solution in the system is 25 to 35w%.
[0045] According to the present invention, preferably, the first solvent is selected from at least one of N-methyl-2-pyrrolidone, N,N-dimethylformamide and N,N-dimethylacetamide.
[0046] According to the present invention, preferably, the molar ratio of the diamine monomer to the dianhydride monomer is 1:1, and the molar ratio of 3,3'-diaminophenolphthalein to benzyldiamine is 2:1-1:2.
[0047] According to the present invention, preferably, the azeotropic desiccant is at least one of toluene, xylene and o-dichlorobenzene; preferably toluene.
[0048] According to the present invention, preferably, the programmed temperature is 50-70°C for 20-28h, 80-100°C for 10-16h, 110-130°C for 10-16h, 140-160°C for 20-28h.
[0049] According to the present invention, the gradient temperature rising program is 60°C for 24h, 90°C for 12h, 120°C for 12h, and 150°C for 24h.
[0050] According to the present invention, preferably, step (2) comprises: dissolving the polyimide obtained in step (1) in a first solvent, stirring until completely dissolved, filtering with a 0.45-1 μm polytetrafluoroethylene filter membrane, injecting the filtered solution into a flat glass culture dish, and then placing it in a vacuum oven, setting a gradient temperature rise program for drying, wherein the gradient temperature rise program is the same as step (1), to obtain a dense polyimide film with uniform thickness and smooth surface.
[0051] According to the present invention, preferably, the film thickness of the polyimide dense film is 50 to 100 μm, preferably 70 to 80 μm.
[0052] According to the present invention, preferably, in step (3), the heating rate of the programmed temperature is 4 to 6° C. / min, and the holding time is 1 to 3 h.
[0053] According to the present invention, preferably, in step (4), the heating rate of the programmed temperature is 4 to 6° C. / min, and the insulation time is 1 to 3 h.
[0054] The third aspect of the present invention provides a heat-induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material obtained by the preparation method.
[0055] The present invention selects low-priced, easily obtainable phthalein-containing structure monomers, and the lactone ring below Tg is decomposed into free radicals for heat-induced crosslinking, which not only improves the plasticization resistance of the polymer film, but also avoids the hole collapse problem caused by high-temperature crosslinking. At the same time, since this type of monomer contains phenolic hydroxyl groups, that is, the polyimide is an ortho-hydroxy polyimide, a thermal rearrangement reaction can be further performed after the polyimide film is thermally induced crosslinked to form a polybenzoxazole film with a more distorted and more rigid structure. In addition, copolymerization of a benzyl diamine-containing copolymer on the basis of phenolphthalein polyimide can improve the gas separation performance of the homopolymer polyimide, and can also perform thermal oxidation crosslinking on the benzyl group, further increase the degree of crosslinking and improve structural stability. This type of PBO membrane is used for gas separation, and gas permeability is greatly improved, wherein only copolymerization makes the flux of CO2 increase by 20 times, and the flux of CO2 of the copolymer polyimide after thermal rearrangement treatment is increased by more than 120 times compared with the homopolymer polyimide.
[0056] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Exemplary embodiments of the present invention will be described in more detail with reference to the accompanying drawings.
[0058] Figure 1 The following is the equation for synthesizing polyimide by condensation polymerization of diamine monomer and dianhydride monomer in the embodiment of the present invention.
[0059] Figure 2 is the three polyimides in the embodiment of the present invention. 1 H-NMR spectrum (DMSO-d6), where a is the 1 H-NMR spectrum (DMSO-d6), b is PI-B 1 H-NMR spectrum (DMSO-d6), c is PI-C 1 H-NMR spectrum (DMSO-d6).
[0060] FIG. 3 is a flow chart showing a thermally induced crosslinking reaction of polyimide in an air atmosphere and a thermal rearrangement reaction in a nitrogen atmosphere according to an embodiment of the present invention.
[0061] Figure 4 The polyimide films prepared in the examples of the present invention are as follows: a is the flexibility display of the PI film; b is the PI film.
[0062] Figure 5 Schematic diagram of the reaction mechanism of heat-induced cross-linking of a polyimide film in an embodiment of the present invention in a high-purity air atmosphere.
[0063] Figure 6 The polyimide films in the embodiments of the present invention are obtained by heat-induced crosslinking treatment at 300°C, 325°C, 350°C, and 400°C in a high-purity air atmosphere, and the polybenzoxazole films synthesized by thermal rearrangement of the films after heat-induced crosslinking treatment at 300°C or 325°C at 400°C, 425°C, and 450°C. a is PI-A-300-air film, PI-A-325-air film, PI-A-350-air film, PI-A-400-air film, PI-A-300-air-400-N2, PI-A-325-air-425-N2 film, and PI-A-325-air-450-N2; b is PI-B-300-air film, PI-B-325-air film, PI-B-350-air film, PI-B-400-air film, I-B-300-air-400-N2, PI-B-325-air-425-N2 membrane and PI-B-325-air-450-N2; c is PI-C-300-air membrane, PI-C-325-air membrane, PI-C-350-air membrane, PI-C-400-air membrane, PI-C-300-air-400-N2, PI-C-325-air-425-N2 membrane and PI-C-325-air-450-N2.
[0064] Figure 7 This is a comparison chart of the anti-plasticization properties of three untreated polyimide original films in the embodiments of the present invention.
[0065] FIG8 is a comparison of infrared spectra of polymer films before and after heat treatment at different temperatures in an embodiment of the present invention. DETAILED DESCRIPTION
[0066] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention. The present invention is further described below in conjunction with the examples, but the scope of the present invention is not limited to these examples.
[0067] Example 1
[0068] Take 4.18g (348.32g / mol, 12mmol) of 3,3'-diaminophenolphthalein and add it to a 100ml four-necked flask, add 22ml NMP and stir for 30min under low temperature ice bath and nitrogen protection, add 5.33g (444.24g / mol, 12mmol) of 6FDA twice, the solid content is 30wt%, continue to stir and react for 12h, form a high viscosity polyamic acid solution, add 15mL toluene, remove the ice bath. Heat to 180℃ and react for 6h to obtain a high viscosity polyimide solution, dilute it and pour it into methanol solution for precipitation, wash it with methanol when filtering, remove the residual solvent, and increase the temperature gradually: 60℃24h, 90℃12h, 120℃12h, 150℃24h, and obtain 7.81g of dried polyimide. The H-NMR spectrum (DMSO-d6) of the polyimide synthesized by the reaction of 3,3'-diaminophenolphthalein and 6FDA is as follows Figure 2 As shown in a. It should be noted that the ortho-hydroxyl group of phenolphthalein diamine is retained during the thermal imidization process, which can be clearly observed from the H-NMR spectrum of polyimide.
[0069] Take 1.00g of dried polyimide powder and dissolve it in DMF, stir until it is completely dissolved, the solid content of the casting solution is 8.0wt%, filter it with a 0.45 or 1μm polytetrafluoroethylene filter membrane, inject the filtered solution into a flat glass culture dish, and then put it into a vacuum oven, repeat the vacuum drying procedure of polyimide in step (1), and obtain a dense polyimide film with uniform thickness and smooth surface, with a film thickness of 70 to 80μm. The flow chart of the thermal induced cross-linking thermal rearrangement reaction of polyimide in air atmosphere is shown in Figure 3.
[0070] Will be like Figure 4 The dried polyimide film shown is placed in a carbonization furnace, and the temperature is increased to 300°C, 325°C, 350°C, and 400°C at a heating rate of 5°C / min in an air atmosphere, and the holding time is 2 hours. The obtained heat-induced cross-linked films are named PI-A-300, PI-A-325, PI-A-350, and PI-A-400, respectively. The reaction mechanism diagram of heat-induced cross-linking of polyimide film in air atmosphere is shown in Figure 5.
[0071] The dense membrane after thermal cross-linking treatment at 300°C or 325°C for 2 hours was placed in a carbonization furnace and heated to 400°C, 425°C, and 450°C at a heating rate of 5°C / min under a nitrogen atmosphere. The insulation time was 2 hours. The polybenzoxazole membranes obtained after thermal cross-linking were named PI-A-300-400, PI-A-325-425, and PI-A-325-450, respectively.
[0072] Comparison of polymer film images before and after treatment Figure 6 As shown in Table 1, the gas permeability and gas selectivity of the polyimide membrane synthesized with DAP and 6FDA, the membranes treated with thermal induced cross-linking at 300°C, 325°C, 350°C and 400°C in air atmosphere for 2 h, and the PI-A-300-400 membrane, PI-A-325-425 membrane and PI-A-325-450 membrane.
[0073] Table 1
[0074]
[0075] As can be seen from Table 1, the permeability increases after thermal induced crosslinking, which is mainly because the lactone ring on the phenolphthalein group begins to decompose into free radicals to form a crosslinked structure, and the chain spacing increases. The increase in selectivity is due to the formation of a more rigid polymer skeleton after thermal crosslinking, which makes the polymer membrane have better size screening performance. The CO2 permeability of PI-A-300-400 did not increase significantly, and was even lower than that of PI-A-400. This is because the thermal crosslinking at 300°C formed a stable crosslinked structure. At a relatively low thermal rearrangement temperature (400°C), its thermal rearrangement conversion rate is low, and the less polybenzoxazole structure has little effect on its gas separation performance. The gas permeability of the polybenzoxazole gas separation membrane obtained by thermal rearrangement after the temperature is increased has been greatly improved, and the CO2 flux after treatment at 450°C is as high as 963.91 barrer.
[0076] For the condensable gas CO2, the permeation isotherm of the glassy polymer may show an upward trend due to the plasticization caused by the swelling of the polymer film under high pressure. Figure 7 It can be seen that when the CO2 pressure is 30atm, the untreated polyimide film (PI-A) still does not show plasticization phenomenon. This is because the use of azeotropic distillation method retains a large number of hydroxyl groups on phenolphthalein diamine, which increases its intermolecular force and improves its anti-plasticization ability.
[0077] Example 2
[0078] Take 2.09g (348.32g / mol, 6mmol) of 3,3'-diaminophenolphthalein and 0.90g (150.22g / mol, 6mmol) of 2,4,6-trimethylm-phenylenediamine into a 100ml four-necked flask, add 19ml NMP and stir for 30min under low temperature ice bath and nitrogen protection, add 5.33g (444.24g / mol, 12mmol) of 6FDA twice, solid content is 30wt%, continue stirring and react for 12h, form a high viscosity polyamic acid solution, add 15mL toluene, remove the ice bath. Heat to 180℃ for 6h, dilute the high viscosity polyimide solution and pour it into methanol solution for precipitation, wash with methanol when filtering, remove residual solvent, and increase the temperature gradually: 60℃24h, 90℃12h, 120℃12h, 150℃24h, and obtain 7.23g of dried polyimide. The H-NMR spectrum (DMSO-d6) of the copolymerized polyimide synthesized by the reaction of 3,3'-diaminophenolphthalein and 2,4,6-trimethylm-phenylenediamine with 6FDA, such as Figure 2 As shown in b.
[0079] Take 1.00g of dried polyimide powder and dissolve it in DMF, stir until it is completely dissolved, the solid content of the casting solution is 8.0wt%, filter it with a 0.45 or 1μm polytetrafluoroethylene filter membrane, inject the filtered solution into a flat glass culture dish, and then put it into a vacuum oven, repeat the vacuum drying procedure of polyimide in step (1), and obtain a dense polyimide film with uniform thickness and smooth surface, with a film thickness of 70 to 80μm. The flow chart of the thermal induced cross-linking thermal rearrangement reaction of polyimide in air atmosphere is shown in Figure 3.
[0080] Will be like Figure 4 The dried polyimide film shown is placed in a carbonization furnace, and heated to 300°C, 325°C, 350°C and 400°C at a heating rate of 5°C / min in an air atmosphere, and the heat preservation time is 2h. The obtained heat-induced cross-linked films are named PI-B-300, PI-B-325, PI-B-350 and PI-B-400 respectively. The reaction mechanism diagram of heat-induced cross-linking of polyimide film in air atmosphere is shown in Figure 5.
[0081] The dense membrane after thermal cross-linking treatment at 300°C or 325°C for 2 hours was placed in a carbonization furnace and heated to 400°C, 425°C, and 450°C at a heating rate of 5°C / min under a nitrogen atmosphere. The insulation time was 2 hours. The polybenzoxazole membranes obtained after thermal cross-linking were named PI-B-300-400, PI-B-325-425, and PI-B-325-450, respectively.
[0082] Comparison of polymer film images before and after treatment Figure 6As shown in Table 2, the gas permeability and gas selectivity of the polyimide membrane synthesized by DAP and DAM with 6FDA, the membranes treated with thermal induced cross-linking at 300℃, 325℃, 350℃ and 400℃ in air atmosphere for 2h, and the PI-B-300-400 membrane, PI-B-325-425 membrane and PI-B-325-450 membrane.
[0083] Table 2
[0084]
[0085] As can be seen from Table 2, the permeability increases after thermal induced crosslinking, which is mainly because the lactone ring on the phenolphthalein group begins to decompose into free radicals to form a crosslinked structure, and the benzyl group also undergoes thermal oxidation crosslinking, and the chain spacing increases. The increase in selectivity is due to the formation of a rigid polymer skeleton after thermal crosslinking, which makes the polymer membrane have better size screening performance. The gas permeability of the polybenzoxazole gas separation membrane obtained after thermal rearrangement has been greatly improved. After treatment at 450℃, the CO2 flux is as high as 749.54 barrer, but lower than the CO2 flux of PI-A-325-450. Because 2,4,6-trimethylm-phenylenediamine (DAM) occupies a certain proportion in the polymer and cannot undergo thermal rearrangement reaction, the polybenzoxazole structure in PI-B is less than that in PI-A, and the effect of the polybenzoxazole structure on the permeability of the former is less than that of the latter.
[0086] Although the number of hydroxyl groups on phenolphthalein diamine in Example 2 is less than that in Example 1, DAM is also a rigid structure. Figure 7 It can be seen that when the CO2 pressure is 30atm, the untreated polyimide film (PI-B) still does not show plasticization phenomenon, indicating that the phenolphthalein-based polyimide after copolymerization with DAM still has excellent anti-plasticization properties.
[0087] Example 3
[0088] Take 2.09g (348.32g / mol, 6mmol) of 3,3'-diaminophenolphthalein and 1.07g (178.28g / mol, 6mmol) of diethyltoluenediamine into a 100ml four-necked flask, add 20ml of NMP and stir for 30min under low temperature ice bath and nitrogen protection, add 5.33g (444.24g / mol, 12mmol) of 6FDA twice, solid content is 30wt%, continue stirring and react for 12h, form a high viscosity polyamic acid solution, add 10mL of toluene, remove the ice bath. Heat to 180℃ and react for 6h, dilute the highly viscous polyimide solution and pour it into methanol solution for precipitation, wash with methanol when filtering, remove residual solvent, and increase the temperature gradually: 60℃24h, 90℃12h, 120℃12h, 150℃24h, and obtain 7.23g of dried polyimide. The H-NMR spectrum (DMSO-d6) of the copolymerized polyimide synthesized by the reaction of 3,3'-diaminophenolphthalein and diethyltoluenediamine with 6FDA is shown in Figure 2 As shown in c.
[0089] Take 1.00g of dried polyimide powder and dissolve it in DMF, stir until it is completely dissolved, the solid content of the casting solution is 8.0wt%, filter it with a 0.45 or 1μm polytetrafluoroethylene filter membrane, inject the filtered solution into a flat glass culture dish, and then put it into a vacuum oven, repeat the vacuum drying procedure of polyimide in step (1), and obtain a dense polyimide film with uniform thickness and smooth surface, with a film thickness of 70 to 80μm. The flow chart of the thermal induced cross-linking thermal rearrangement reaction of polyimide in air atmosphere is shown in Figure 3.
[0090] Will be like Figure 4 The dried polyimide film shown is placed in a carbonization furnace, and heated to 300°C, 325°C, 350°C and 400°C at a heating rate of 5°C / min in an air atmosphere, and the heat preservation time is 2h. The obtained heat-induced cross-linked films are named PI-C-300, PI-C-325, PI-C-350 and PI-C-400 respectively. The reaction mechanism diagram of heat-induced cross-linking of polyimide film in air atmosphere is shown in Figure 5.
[0091] The dense membrane after thermal cross-linking treatment at 300°C or 325°C for 2 hours was placed in a carbonization furnace and heated to 400°C, 425°C, and 450°C at a heating rate of 5°C / min under a nitrogen atmosphere. The insulation time was 2 hours. The polybenzothiophene films obtained after thermal cross-linking were named PI-C-300-400, PI-C-325-425, and PI-C-325-450, respectively.
[0092] Comparison of polymer film images before and after treatment Figure 6As shown in Table 2, the gas permeability and gas selectivity of the polyimide membrane synthesized with DAP and DETDA and 6FDA, the membranes treated with thermal induced cross-linking at 300°C, 325°C, 350°C and 400°C in air atmosphere for 2 h, and the PI-C-300-400 membrane, PI-C-325-425 membrane and PI-C-325-450 membrane.
[0093] Table 3
[0094]
[0095]
[0096] As can be seen from Table 3, the permeability decreases after thermal induced crosslinking, which is opposite to the results in Examples 1 and 2. This is mainly because the benzyl group in diethyltoluenediamine (DETDA) reduces its free volume when it is thermally oxidatively crosslinked, and this effect also affects the crosslinked structure formed by the decomposition of the lactone ring on the phenolphthalein group. At 400°C, due to the degradation of small molecules, its CO2 permeability is higher than that of the original membrane; at the same time, due to the size screening effect of the crosslinked structure, its selectivity is also better than that of the original membrane. The gas permeability of the polybenzoxazole gas separation membrane obtained after thermal rearrangement has been greatly improved, and the CO2 flux after treatment at 450°C is as high as 642.41barrer. However, this result is lower than the CO2 flux of PI-B-325-450 and the CO2 flux of PI-A-325-450. The reason is the same as that in Specific Example 2, and the volume proportion of DETDA in the polymer is greater than that of DAM, which has a greater restriction on the polybenzoxazole structure to increase its flux.
[0097] from Figure 7 It can be seen that when the CO2 pressure is 30 atm, the untreated polyimide film (PI-C) does not show plasticization, but its anti-plasticization performance is obviously inferior to that of PI-A and PI-B. This is because the ethyl group on DETDA is worse than the methyl group on DAM, which makes the polymer more flexible, but it is undeniable that PI-C still has excellent anti-plasticization performance.
[0098] Example 4
[0099] Take 1.39g (348.32g / mol, 4mmol) of 3,3'-diaminophenolphthalein and 1.20g (150.22g / mol, 8mmol) of 2,4,6-trimethylm-phenylenediamine into a 100ml four-necked flask, add 18ml NMP and stir for 30min under low temperature ice bath and nitrogen protection, add 5.33g (444.24g / mol, 12mmol) of 6FDA twice, solid content is 30wt%, continue stirring and react for 12h, form a high viscosity polyamic acid solution, add 10mL toluene, remove the ice bath. Heat to 180℃ for 6h, dilute the high viscosity polyimide solution and pour it into methanol solution for precipitation, wash with methanol when filtering, remove residual solvent, and increase the temperature gradually: 60℃24h, 90℃12h, 120℃12h, 150℃24h, and obtain 7.23g of dried polyimide. The H-NMR spectrum (DMSO-d6) of the copolymerized polyimide synthesized by the reaction of 3,3'-diaminophenolphthalein and 2,4,6-trimethylm-phenylenediamine with 6FDA is shown in Figure 2 As shown in b.
[0100] Take 1.00g of dried polyimide powder and dissolve it in DMF, stir until it is completely dissolved, the solid content of the casting solution is 8.0wt%, filter it with a 0.45 or 1μm polytetrafluoroethylene filter membrane, inject the filtered solution into a flat glass culture dish, and then put it into a vacuum oven, repeat the vacuum drying procedure of polyimide in step (1), and obtain a dense polyimide membrane with uniform thickness and smooth surface, with a membrane thickness of 70 to 80μm. Table 4 is its gas separation performance:
[0101] Table 4
[0102]
[0103] Example 5
[0104] Take 1.39g (348.32g / mol, 4mmol) of 3,3'-diaminophenolphthalein and 1.43g (178.28g / mol, 8mmol) of diethyltoluenediamine into a 100ml four-necked flask, add 19ml of NMP and stir for 30min under low temperature ice bath and nitrogen protection, add 5.33g (444.24g / mol, 12mmol) of 6FDA twice, with a solid content of 30wt%, continue stirring and react for 12h to form a high viscosity polyamic acid solution, add 10mL of toluene, remove the ice bath. Heat to 180℃ for 6h, dilute the highly viscous polyimide solution and pour it into methanol solution for precipitation, wash with methanol when filtering, remove residual solvent, and increase the temperature gradually: 60℃ for 12h, 90℃ for 12h, 120℃ for 24h, 150℃ for 24h, and obtain 6.80g of dried polyimide. The H-NMR spectrum (DMSO-d6) of the copolymerized polyimide synthesized by the reaction of 3,3'-diaminophenolphthalein and diethyltoluenediamine with 6FDA is shown in Figure 2 As shown in c.
[0105] Take 1.00g of dried polyimide powder and dissolve it in DMF, stir until it is completely dissolved, the solid content of the casting solution is 8.0wt%, filter it with a 0.45 or 1μm polytetrafluoroethylene filter membrane, inject the filtered solution into a flat glass culture dish, and then put it into a vacuum oven, repeat the vacuum drying procedure of polyimide in step (1), and obtain a dense polyimide membrane with uniform thickness and smooth surface, with a membrane thickness of 70 to 80μm. Table 5 is its gas separation performance:
[0106] Table 5
[0107]
[0108] Example 6
[0109] The difference between this comparative example and Example 2 is that after forming a high-viscosity polyamic acid solution, 5 mL of acetic anhydride and 5 mL of anhydrous pyridine are added, and the ice bath is removed. The reaction is continued at room temperature for 24 hours, and the highly viscous polyimide solution is poured into a methanol solution for precipitation, washed with methanol during filtration, and the residual solvent is removed. The dried product is vacuum-dried in an oven at 80°C for 24 hours to obtain 8.25 g of dried polyimide. The remaining steps are the same. PI-D-300, PI-D-325, PI-D-350, PI-D-400, PI-D-300-400, PI-D-325-425 and PI-D-325-450 are obtained respectively. Table 6 shows its gas separation performance:
[0110] Table 6
[0111]
[0112] As can be seen from Table 6, in Example 6, chemical imidization is used, and compared with Example 2, CO2 flux is improved, but CO2 / CH4 selectivity is lower. For the heat-induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material, the improvement of flux is relatively easy, and the low selectivity is difficult to improve. In addition, the heat-induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material obtained by chemical imidization is not good in the later application, and defects such as spinning hollow fibers will occur.
[0113] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
[0114] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material, characterized in that: Its structural formula is shown in Formula I: Wherein, R1, R2, and R3 are each independently H or C1-C4 alkyl; m1, m2, m and n represent the number of repeating units, m1, m2, m are between 20 and 500, n is 0, or n is between 20 and 500; Ar is a linking unit of a dianhydride anhydride group, the dianhydride anhydride group is derived from a dianhydride monomer, and the dianhydride monomer is at least one of pyromellitic anhydride, pyrophthalic anhydride, biphenyltetracarboxylic anhydride, hexafluoroisopropylphthalic anhydride, benzophenonetetracarboxylic anhydride and oxydiphthalic anhydride.
2. The thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material according to claim 1, wherein: The heat-induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, heat-induced cross-linking and thermal rearrangement reactions of diamine monomers and dianhydride monomers.
3. The thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material according to claim 2, wherein: The diamine monomer is 3,3'-diaminophenolphthalein, or the diamine monomer is 3,3'-diaminophenolphthalein and benzyldiamine.
4. The thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material according to any one of claims 1 to 3, wherein: n is between 20 and 500, and the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is selected from any one of the following: (i) Formula I wherein R1 = CH3, R2 = H, R3 = H; (ii) Formula I wherein R1=CH3, R2=CH3, R3=H or R1=H, R2=CH3, R3=CH3; (iii) Formula I wherein R1=CH3, R2=CH3, R3=CH3; (iv) Formula I wherein R1 = CH3, R2 = CH2CH3, R3 = H or R1 = CH2CH3, R2 = CH3, R3 = H; (v) In formula I, R1=CH3, R2=CH2CH3, R3=CH2CH3 or R1=CH2CH3, R2=CH2CH3, R3=CH3.
5. The thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material according to claim 4, wherein: When R1=CH3, R2=H, R3=H in formula I, the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, thermally induced cross-linking, and thermal rearrangement reaction of monomer (a), 3,3'-diaminophenolphthalein and dianhydride monomer; When R1=CH3, R2=CH3, R3=H or R1=H, R2=CH3, R3=CH3 in formula I, the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, thermally induced cross-linking, and thermal rearrangement reaction of monomer (b), 3,3'-diaminophenolphthalein and dianhydride monomer; When R1=CH3, R2=CH3, R3=CH3 in formula I, the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, thermally induced cross-linking, and thermal rearrangement reaction of monomer (c), 3,3'-diaminophenolphthalein and dianhydride monomer; When R1=CH3, R2=CH2CH3, R3=H or R1=CH2CH3, R2=CH3, R3=H in formula I, the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, thermally induced cross-linking, and thermal rearrangement reaction of monomer (d), 3,3'-diaminophenolphthalein and dianhydride monomer; When R1=CH3, R2=CH2CH3, R3=CH2CH3 or R1=CH2CH3, R2=CH2CH3, R3=CH3 in formula I, the thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material is a PBO polymer synthesized by thermal imidization, thermally induced cross-linking, and thermal rearrangement reaction of monomer (e), 3,3'-diaminophenolphthalein and dianhydride monomer; 6. A method for preparing a heat-induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material, characterized in that: The method comprises the following steps: (1) under the protection of an inert gas, contacting a diamine monomer, a first solvent and a dianhydride monomer to carry out an imidization reaction to obtain a polyimide; the dianhydride monomer is at least one selected from pyromellitic anhydride, pyromellitic anhydride, biphenyltetracarboxylic anhydride, hexafluoroisopropylphthalic anhydride, benzophenone tetracarboxylic anhydride and oxydiphthalic anhydride; the diamine monomer is 3,3'-diaminophenolphthalein, or the diamine monomer is 3,3'-diaminophenolphthalein and benzyldiamine; the benzyldiamine is at least one selected from 2-methyl-1,3-phenylenediamine, 2,4-dimethyl-1,3-phenylenediamine, 2,4-dimethyl-1,5-phenylenediamine, 2,4,6-trimethyl-1,3-phenylenediamine, 2-methyl-4-ethyl-1,3-phenylenediamine, 4-methyl-2-ethyl-1,5-phenylenediamine and diethyltoluenediamine; (2) Preparation of dense polyimide film The polyimide obtained in step (1) is dissolved in a first solvent, and filtered to prepare a dense polyimide membrane; (3) Heat-induced cross-linking treatment of dense membrane In an air atmosphere, the polyimide dense film dried in step (2) is heated to 300-400° C. and kept warm to obtain the heat-induced cross-linked dense film; (4) Thermal rearrangement Under a nitrogen atmosphere, the heat-induced cross-linked dense membrane prepared in step (3) is heated to 400-450° C. and kept warm to obtain the heat-induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material.
7. The preparation method according to claim 6, wherein: Step (1) comprises: Under low-temperature ice bath and nitrogen protection, the diamine monomer is dissolved in the first solvent, stirred evenly, and the dianhydride monomer is added in batches to make the concentration of the diamine monomer and dianhydride monomer solution 25-35w%, and the stirring reaction is continued for 20-30h until a high-viscosity polyamic acid solution is formed, the ice bath is removed, and then an azeotropic desiccant is added and stirred until the mixture is evenly mixed, and the mixture is heated to 180-200°C for thermal imidization reaction, and the reaction time is 4-8h to form a high-viscosity polyimide solution, and the heating is stopped and the first solvent is added for dilution, and finally the obtained polyimide solution is poured into methanol for precipitation, and the precipitate is crushed, filtered, washed, and the obtained polyimide is subjected to programmed temperature drying after the residual solvent is removed.
8. The preparation method according to claim 6 or 7, wherein: The first solvent is selected from at least one of N-methyl-2-pyrrolidone, N,N-dimethylformamide and N,N-dimethylacetamide; The molar ratio of the diamine monomer to the dianhydride monomer is 1:1, and the molar ratio of 3,3'-diaminophenolphthalein to benzyl diamine is 2:1-1:
2.
9. The preparation method according to claim 8, wherein: In step (1), the azeotropic desiccant is at least one of toluene, xylene and o-dichlorobenzene; preferably toluene; The programmed temperature rise is 50-70°C for 20-28h, 80-100°C for 10-16h, 110-130°C for 10-16h, and 140-160°C for 20-28h.
10. The preparation method according to claim 7, wherein: Step (2) comprises: The polyimide obtained in step (1) is dissolved in the first solvent, stirred until completely dissolved, filtered with a 0.45-1 μm polytetrafluoroethylene filter membrane, injected into a flat glass culture dish, and then placed in a vacuum oven, set a gradient temperature program for drying, and obtain a dense polyimide film with uniform thickness and smooth surface.
11. The preparation method according to claim 6 or 10, wherein: The film thickness of the polyimide dense film is 50 to 100 μm, preferably 70 to 80 μm.
12. The preparation method according to claim 6, wherein: In step (3), the heating rate of the programmed temperature is 4 to 6°C / min, and the holding time is 1 to 3 hours; In step (4), the heating rate of the programmed temperature is 4 to 6°C / min, and the insulation time is 1 to 3 hours.
13. A thermally induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material prepared by the preparation method described in any one of claims 6 to 12.
Citation Information
Patent Citations
Polyimide containing phenolic hydroxy
CN102516541A
Thermally rearranged poly(benzoxazole-imide) copolymer having cross-linked structure, gas separation membrane comprising same and preparation method therefor
CN105899580A
Method for preparing porous gas separation membrane material with thermally-induced rigid structure
CN105921037A
Thermally-induced cross-linked phenolphthalein-based polybenzoxazole gas separation membrane material and preparation method thereof
CN112915818A
Aromatic diamine monomer simultaneously containing phenolphthalein Cardo and alkyl structures and preparation method and application of polyimide of aromatic diamine monomer