Method for reducing haze of high-density polyethylene film
By optimizing the amount of crosslinking agent added and combining the use of diisophenyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole, high haze of high density polyethylene films is solved Problem, achieving a significant effect of reducing haze and improving transparency.
Patent Information
- Application Number
- CN202411167238.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
The haze of high-density polyethylene films is high, affecting its transparency and imaging degree. The prior art is limited in reducing haze.
By optimizing the amount of the crosslinking agent, diisophenyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole are used as a composite crosslinking agent, mixed uniformly in the extruder and blown The high-density polyethylene film was prepared by processing in a membrane machine.
It significantly reduces the haze of high-density polyethylene films, improves its transparency and imaging, and is suitable for internal display packaging applications.
Smart Images

Figure CN119019720A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-density polyethylene films, in particular to a method for reducing the haze of high-density polyethylene films. Background Art
[0002] High-density polyethylene (HDPE) is a highly crystalline non-polar synthetic resin formed by copolymerization of ethylene and a small amount of α-olefin monomers. It is synthesized under relatively low pressure. Its molecular structure is mainly linear, with few branches in the molecule, high crystallinity, high density, high operating temperature, hardness and mechanical strength, and good chemical resistance. HDPE's good tensile strength makes it suitable for making various packaging films, including shopping bags, garbage bag linings, packaging bags, etc. In addition, HDPE has also developed rapidly in the application of high-strength films for preparing packaging materials such as food, agricultural and sideline products, and textiles. Haze is used to characterize the cloudy appearance caused by light scattering inside or on the surface of a transparent or translucent film. Its quantitative definition is the percentage of the transmitted light intensity that deviates from the incident light by more than 2.5° to the total transmitted light intensity. That is, the greater the haze, the lower the gloss and transparency of the film, especially the imaging degree. Haze is one of the important optical properties of HDPE film. For packaging applications that need to show the internal objects, such as food packaging, shopping bags, etc., reducing haze is one of the main requirements for HDPE film materials. However, due to the high crystallinity of HDPE, its film haze is often much higher than other types of polyethylene films of the same thickness.
[0003] At present, there are two main methods for reducing the haze of HDPE film in industry. The first is based on materials and additives, mainly optimizing the film formula to improve its transmittance, thereby reducing the haze. For example, patents with publication numbers CN105778232A and CN110982152A disclose methods for reducing the haze of films by adding low-density polyethylene or crystallization nucleating additives to HDPE film materials; the second is based on film blowing process, mainly adjusting process parameters or improving the design of key components in the equipment. However, the above methods have limited effect on reducing the haze of high-density polyethylene films. Based on this, a method for reducing the haze of high-density polyethylene films is provided. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the present invention provides a method for reducing the haze of high-density polyethylene film. By optimizing the amount of cross-linking agent added and using diisopropyl peroxide / di-tert-butyl peroxide / 2-phenylimidazole in combination, the haze of the high-density polyethylene film can be greatly reduced.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for reducing the haze of a high-density polyethylene film, comprising the following steps:
[0006] (1) Select high-density polyethylene pellets or powder;
[0007] (2) selecting diisopropyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole as composite cross-linking agents;
[0008] (3) uniformly mixing the high-density polyethylene and the composite cross-linking agent to obtain a mixture;
[0009] (4) feeding the mixed material into an extruder for melt extrusion and granulation to obtain high-density polyethylene particles;
[0010] (5) The high-density polyethylene particles are blown into shape by a film blowing machine to produce a high-density polyethylene film.
[0011] Preferably, in step (1), the high-density polyethylene is an ethylene copolymer or an ethylene homopolymer.
[0012] Preferably, the density of the high-density polyethylene is 0.935-0.975 g / cm 3 The melt index at 190°C under a load of 5kg is 0.05-50g / 10min, the ratio of weight-average molecular weight to number-average molecular weight is 20-35, there is no obvious double peak or multi-peak in the molecular weight distribution, the residual magnesium element is less than 50ppm, and the loss factor is reduced from more than 1.51 to less than 1.35 in the dynamic viscosity test at 190°C and 0.1rad / s.
[0013] Preferably, in step (2), the mass ratio of diisophenyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole is (0-2):(0-4):(0-3).
[0014] Preferably, in step (3), the added amount of the composite cross-linking agent is 1-5000 ppm.
[0015] Preferably, the added amount of the composite cross-linking agent is 25-200 ppm.
[0016] Preferably, in step (4), the temperature of the extruder is 130-350° C., and the extrusion flow rate is 95 kg / h; the parameters of the extruder are as follows: the screw diameter is 51.4 mm, and the aspect ratio is 40:1.
[0017] Preferably, in step (5), the blow molding process is as follows: controlling the die temperature to 200° C., the film output to 26 kg / h, the pulling speed to 360 mm / s, and the film thickness to 5-50 μm.
[0018] Preferably, the film thickness is 22 μm.
[0019] The present invention provides a method for reducing the haze of a high-density polyethylene film, which has the following beneficial effects compared with the prior art:
[0020] The invention can significantly reduce the haze of the high-density polyethylene film by reasonably optimizing the addition amount of the cross-linking agent and using diisopropyl peroxide / di-tert-butyl peroxide / 2-phenylimidazole in combination, which is beneficial to the application of the high-density polyethylene film in internal display packaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0022] Figure 1 This is a graph showing the relationship between the amount of the composite cross-linking agent added and the haze of the film of the present invention. DETAILED DESCRIPTION
[0023] The following examples are used to explain the implementation methods of the present application in detail, so that the implementation process of how the present application uses technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.
[0024] Example 1
[0025] A method for reducing the haze of a high-density polyethylene film comprises the following steps:
[0026] (1) Select high-density polyethylene pellets or powder; wherein the density of high-density polyethylene is 0.935 g / cm 3 The melt index at 190°C under a load of 5kg is 0.05g / 10min, the ratio of the weight-average molecular weight to the number-average molecular weight is 20, there is no obvious double peak or multi-peak in the molecular weight distribution, the residual magnesium element is less than 50ppm, and the loss factor is reduced from more than 1.51 to less than 1.35 in the dynamic viscosity test at 190°C and 0.1rad / s.
[0027] (2) Diisopropyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole are selected as composite cross-linking agents, and the addition amount thereof is 25 ppm; wherein the mass ratio of diisopropyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole is 1:3:3.
[0028] (3) The high-density polyethylene and the composite cross-linking agent are uniformly mixed to obtain a mixture.
[0029] (4) The mixed material is fed into an extruder for melt extrusion and granulation to obtain high-density polyethylene particles; during this period, the temperature of the extruder is controlled at 150° C. and the extrusion flow rate is 95 kg / h; the parameters of the extruder are as follows: the screw diameter is 51.4 mm and the aspect ratio is 40:1.
[0030] (5) The high-density polyethylene particles are blown into a high-density polyethylene film by a film blowing machine. During the blow molding process, the die temperature is controlled at 200°C, the film output is 26kg / h, the pulling speed is 360mm / s, and the film thickness is 22μm.
[0031] Example 2
[0032] A method for reducing the haze of a high-density polyethylene film comprises the following steps:
[0033] (1) Select high-density polyethylene pellets or powder; wherein the density of high-density polyethylene is 0.945 g / cm 3 The melt index at 190°C under a load of 5kg is 15g / 10min, the ratio of the weight-average molecular weight to the number-average molecular weight is 25, there are no obvious double peaks or multiple peaks in the molecular weight distribution, the residual magnesium element is less than 50ppm, and the loss factor is reduced from more than 1.51 to less than 1.35 in the dynamic viscosity test at 190°C and 0.1rad / s.
[0034] (2) Diisopropyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole are selected as composite cross-linking agents, and the addition amount thereof is 50 ppm; wherein the mass ratio of diisopropyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole is 2:1:1.
[0035] (3) The high-density polyethylene and the composite cross-linking agent are uniformly mixed to obtain a mixture.
[0036] (4) The mixed material is fed into an extruder for melt extrusion and granulation to obtain high-density polyethylene particles; during this period, the temperature of the extruder is controlled at 250° C. and the extrusion flow rate is 95 kg / h; the parameters of the extruder are as follows: the screw diameter is 51.4 mm and the aspect ratio is 40:1.
[0037] (5) The high-density polyethylene particles are blown into a high-density polyethylene film by a film blowing machine. During the blow molding process, the die temperature is controlled at 200°C, the film output is 26kg / h, the pulling speed is 360mm / s, and the film thickness is 25μm.
[0038] Example 3
[0039] A method for reducing the haze of a high-density polyethylene film comprises the following steps:
[0040] (1) Select high-density polyethylene pellets or powder; wherein the density of high-density polyethylene is 0.960 g / cm 3 The melt index at 190°C under a load of 5kg is 25g / 10min, the ratio of the weight-average molecular weight to the number-average molecular weight is 30, there is no obvious double peak or multi-peak in the molecular weight distribution, the residual magnesium element is less than 50ppm, and the loss factor is reduced from more than 1.51 to less than 1.35 in the dynamic viscosity test at 190°C and 0.1rad / s.
[0041] (2) Diisopropyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole are selected as composite cross-linking agents, and the addition amount thereof is 100 ppm; wherein the mass ratio of diisopropyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole is 3:1:1.
[0042] (3) The high-density polyethylene and the composite cross-linking agent are uniformly mixed to obtain a mixture.
[0043] (4) The mixed material is fed into an extruder for melt extrusion and granulation to obtain high-density polyethylene particles; during this period, the temperature of the extruder is controlled at 280° C. and the extrusion flow rate is 95 kg / h; the parameters of the extruder are as follows: the screw diameter is 51.4 mm and the aspect ratio is 40:1.
[0044] (5) The high-density polyethylene particles are blown into a high-density polyethylene film by a film blowing machine. During the blow molding process, the die temperature is controlled at 200°C, the film output is 26kg / h, the pulling speed is 360mm / s, and the film thickness is 25μm.
[0045] Example 4
[0046] A method for reducing the haze of a high-density polyethylene film comprises the following steps:
[0047] (1) Select high-density polyethylene pellets or powder; wherein the density of high-density polyethylene is 0.975 g / cm 3 The melt index at 190°C under a load of 5kg is 50g / 10min, the ratio of weight-average molecular weight to number-average molecular weight is 35, there is no obvious double peak or multi-peak in the molecular weight distribution, the residual magnesium element is less than 50ppm, and the loss factor is reduced from greater than 1.51 to less than 1.35 in the dynamic viscosity test at 190°C and 0.1rad / s.
[0048] (2) Diisopropyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole are selected as composite cross-linking agents, and the addition amount thereof is 200 ppm; wherein the mass ratio of diisopropyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole is 1:2:5.
[0049] (3) The high-density polyethylene and the composite cross-linking agent are uniformly mixed to obtain a mixture.
[0050] (4) The mixed material is fed into an extruder for melt extrusion and granulation to obtain high-density polyethylene particles; during this period, the temperature of the extruder is controlled at 210° C. and the extrusion flow rate is 95 kg / h; the parameters of the extruder are as follows: the screw diameter is 51.4 mm and the aspect ratio is 40:1.
[0051] (5) The high-density polyethylene particles are blown into a high-density polyethylene film by a film blowing machine. During the blow molding process, the die temperature is controlled at 200°C, the film output is 26kg / h, the pulling speed is 360mm / s, and the film thickness is 25μm.
[0052] Example 5
[0053] It is basically the same as Example 4, except that: the addition amount of the composite cross-linking agent in step (2) is 5 ppm; and the film thickness in step (5) is 5 μm.
[0054] Example 6
[0055] It is basically the same as Example 4, except that: the addition amount of the composite cross-linking agent in step (2) is 5000 ppm; and the film thickness in step (5) is 50 μm.
[0056] Comparative Example 1
[0057] A method for reducing the haze of a high-density polyethylene film comprises the following steps:
[0058] (1) Select high-density polyethylene pellets or powder; wherein the density of high-density polyethylene is 0.975 g / cm 3 The melt index at 190°C under a load of 5kg is 50g / 10min, the ratio of weight-average molecular weight to number-average molecular weight is 35, there is no obvious double peak or multi-peak in the molecular weight distribution, the residual magnesium element is less than 50ppm, and the loss factor is reduced from greater than 1.51 to less than 1.35 in the dynamic viscosity test at 190°C and 0.1rad / s.
[0059] (2) High-density polyethylene pellets or powder are fed into an extruder for melt extrusion and granulation to obtain high-density polyethylene pellets; during this period, the temperature of the extruder is controlled at 210° C. and the extrusion flow rate is 95 kg / h; the parameters of the extruder are as follows: the screw diameter is 51.4 mm and the aspect ratio is 40:1.
[0060] (3) The high-density polyethylene particles are blown into a high-density polyethylene film by a film blowing machine. During the blow molding process, the die temperature is controlled at 200°C, the film output is 26kg / h, the pulling speed is 360mm / s, and the film thickness is 25μm.
[0061] Comparative Example 2
[0062] The method is basically the same as Example 4, except that the composite cross-linking agent is replaced by diisopropyl peroxide.
[0063] Comparative Example 3
[0064] The method is basically the same as Example 4, except that the composite cross-linking agent is replaced by di-tert-butyl peroxide.
[0065] Comparative Example 4
[0066] The method is basically the same as Example 4, except that the composite cross-linking agent is replaced by 2-phenylimidazole.
[0067] Haze test
[0068] 1. The high-density polyethylene films in Examples 1-5 and Comparative Examples 1-4 were used as test objects, and the haze of the films was measured according to the standard of GB / T2410-2008. No crosslinking agent was added in Comparative Example 1, which was used as a reference. The specific results are shown in the following table.
[0069] Table 1 Haze
[0070] category Haze(%) Haze reduction percentage (%) Example 1 80.6 7.6 Example 2 76.1 12.7 Example 3 72.1 17.3 Example 4 64.1 26.5 Example 5 83.5 4.2 Comparative Example 1 87.2 0 Comparative Example 2 73.8 15.4 Comparative Example 3 74.5 14.6 Comparative Example 4 72.7 16.6
[0071] It can be seen from the above table that: as the content of the composite cross-linking agent increases, the haze of the film gradually decreases; compared with the single use of diisopropyl peroxide / di-tert-butyl peroxide / 2-phenylimidazole, the combined use of the three can further reduce the haze of the film.
[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for reducing the haze of a high-density polyethylene film, characterized in that: The following steps are involved: (1) Select high-density polyethylene pellets or powder; (2) selecting diisopropyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole as composite cross-linking agents; (3) uniformly mixing the high-density polyethylene and the composite cross-linking agent to obtain a mixture; (4) feeding the mixed material into an extruder for melt extrusion and granulation to obtain high-density polyethylene particles; (5) The high-density polyethylene particles are blown into shape by a film blowing machine to produce a high-density polyethylene film.
2. The method for reducing the haze of a high-density polyethylene film according to claim 1, characterized in that: In step (1), the high-density polyethylene is an ethylene copolymer or an ethylene homopolymer.
3. The method for reducing the haze of a high-density polyethylene film according to claim 2, characterized in that: The density of the high-density polyethylene is 0.935-0.975 g / cm 3 The melt index at 190°C under a load of 5kg is 0.05-50g / 10min, the ratio of weight-average molecular weight to number-average molecular weight is 20-35, there is no obvious double peak or multi-peak in the molecular weight distribution, the residual magnesium element is less than 50ppm, and the loss factor is reduced from more than 1.51 to less than 1.35 in the dynamic viscosity test at 190°C and 0.1rad / s.
4. The method for reducing haze of high-density polyethylene film according to claim 1, characterized in that: In step (2), the mass ratio of diisophenyl peroxide, di-tert-butyl peroxide and 2-phenylimidazole is (0-2):(0-4):(0-3).
5. The method for reducing haze of high-density polyethylene film according to claim 1, characterized in that: In step (3), the added amount of the composite cross-linking agent is 1-5000 ppm.
6. The method for reducing haze of high-density polyethylene film according to claim 5, characterized in that: The added amount of the composite cross-linking agent is 25-200 ppm.
7. The method for reducing haze of high-density polyethylene film according to claim 1, characterized in that: In step (4), the temperature of the extruder is 130-350° C., and the extrusion flow rate is 95 kg / h; the parameters of the extruder are as follows: the screw diameter is 51.4 mm, and the aspect ratio is 40:
1.
8. The method for reducing haze of high-density polyethylene film according to claim 1, characterized in that: In step (5), the blow molding process is as follows: the die temperature is controlled at 200°C, the film output is 26kg / h, the pulling speed is 360mm / s, and the film thickness is 5-50μm.
9. The method for reducing haze of a high-density polyethylene film according to claim 8, characterized in that: The film thickness is 22 μm.