Polyvinyl alcohol film and optical film prepared from same

By regulating the alkalinization and polymerization degree of polyvinyl alcohol film, controlling its storage modulus and softening point temperature, the fracture problem of polyvinyl alcohol film during stretching is solved, and the red light leakage rate of the polarizing film is reduced, thereby achieving Improved mechanical strength and optical properties.

CN119019796APending Publication Date: 2024-11-26CHANG CHUN PETROCHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310659561.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2023-06-06
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The polyvinyl alcohol film is prone to break during stretching, and the prior art is difficult to effectively solve this problem. At the same time, the red light leakage rate of the polarizing film is also relatively high.

Method used

By regulating the alkalinization and polymerization of the polyvinyl alcohol film, controlling its storage modulus and softening point temperature in a specific temperature range, ensuring the mechanical strength and optical properties of the polyvinyl alcohol film during tensile. Specific measures include in water The storage modulus in the range of 30°C to 55°C has a turning point temperature of 37 to 40°C, a alkalinization degree of 95 mol% or more, a softening point temperature of 45°C or less, and a polarization is prepared by specific film making steps and treatment methods. membrane.

Benefits of technology

The fracture problem of the polyvinyl alcohol film during stretching is significantly improved, and the red light leakage rate is reduced by less than 5% in the polarizing film, thereby improving the mechanical strength and optical properties of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019796A_ABST
    Figure CN119019796A_ABST
Patent Text Reader

Abstract

The present invention relates to a polyvinyl alcohol film and an optical film prepared therefrom, the polyvinyl alcohol film comprising a polyvinyl alcohol resin having an alkalization degree of more than 95 mol%, the storage modulus (E ') of the polyvinyl alcohol film in water at a temperature of 30-55 DEG C having a turning point temperature of 37-40 DEG C. The polyvinyl alcohol film disclosed by the invention has the characteristic that the film is not easy to break when the film is stretched, and the optical film prepared from the polyvinyl alcohol film has the characteristic of less red light leakage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyvinyl alcohol (PVA) product, in particular to a polyvinyl alcohol film and an optical film made therefrom, but not limited thereto. Background Art

[0002] Polyvinyl alcohol (PVA) film is a hydrophilic material obtained by coating and drying an aqueous solution containing polyvinyl alcohol polymer and a plasticizer. It has high transparency, mechanical strength, water solubility, good processability and other properties. It has been widely used in various optical films for packaging materials or electronic products, such as polarizing films.

[0003] The polarizing film obtained by processing the polyvinyl alcohol film through the polarizing process (manufacturing process) has the characteristic of only allowing light in a specific direction to pass through, and can thereby control the brightness of the light passing through; based on this characteristic, the polarizing film is used in various displays, glasses and wearable devices. The so-called polarizing process generally includes steps such as swelling, stretching and dyeing; specifically, the polyvinyl alcohol film will be placed in a solution to carry out the aforementioned steps, so that the dye molecules diffuse into the molecules in the polyvinyl alcohol film, and through stretching, a relatively regular arrangement is obtained, so that the polarizing film can absorb the light component parallel to its arrangement direction, and allow the light component in the vertical direction to pass through, thereby generating polarization characteristics. However, when manufacturing polarizing films, polyvinyl alcohol films often have the problem of breaking due to stretching.

[0004] Prior art such as Taiwan Invention Patent Publication No. 201817576 discloses a polyvinyl alcohol-based film, which utilizes the following steps to prepare a polyvinyl alcohol-based film and control the ratio of its elastic modulus to thickness to improve the problem of film breakage: a film-forming step, in which an aqueous solution of a polyvinyl alcohol-based resin is film-formed using a continuous casting method; a drying step, in which a hot roller is used to dry the film obtained by film-forming; and a heat treatment step, in which the dried film is heat-treated; in the drying step, the temperature at which the film obtained by film-forming is dried, that is, the surface temperature of the hottest hot roller among the multiple hot rollers used, is 100-115°C; in the drying step, the contact time between the hottest hot roller and the film obtained by film-forming is 4-30 seconds; the heat treatment step is a step of cooling the dried film to below 50°C and then heating it at 60-99°C.

[0005] In addition, the polarizing film should have suitable optical properties. For this purpose, the prior art also discloses improving the optical properties by changing the structure of polyvinyl alcohol or adding functional groups (such as cationic groups). The prior art, such as Taiwan Invention Patent Publication No. 201719207, discloses a polarizing film with good polarization performance and less leakage of red light in the orthogonal polarization state and a method for manufacturing the same. Summary of the invention

[0006] In the prior art, when using polyvinyl alcohol film to prepare optical films, the film often breaks when stretched. In response to this, the inventors have found that by adjusting the polyvinyl alcohol film so that its storage modulus (E') in a specific temperature range has a turning point temperature within a specific range, the problem of the polyvinyl alcohol film being easily broken when stretched can be improved.

[0007] Specifically, the present invention provides a polyvinyl alcohol film, which comprises a polyvinyl alcohol resin with a basicity of 95 mol % or more; wherein the storage modulus (E') of the polyvinyl alcohol film in water at 30°C to 55°C has a turning point temperature of 37 to 40°C.

[0008] In one or more embodiments, the polyvinyl alcohol film has a softening point temperature, and the softening point temperature is less than or equal to 45°C.

[0009] In one or more embodiments, the basicity of the polyvinyl alcohol resin is greater than 99.90 mol %.

[0010] In one or more embodiments, the basicity of the polyvinyl alcohol resin is greater than 99.95 mol %.

[0011] In one or more embodiments, the basicity of the polyvinyl alcohol resin is greater than 99.97 mol %.

[0012] In one or more embodiments, the average degree of polymerization of the polyvinyl alcohol resin is 2000-3300.

[0013] In one or more embodiments, the average degree of polymerization of the polyvinyl alcohol resin is 2400-3300.

[0014] In one or more embodiments, the polyvinyl alcohol film has a thickness of 40 to 75 μm.

[0015] Another aspect of the present invention provides an optical film, which is made from the polyvinyl alcohol film.

[0016] In one or more embodiments, the optical film is a polarizing film.

[0017] In one or more embodiments, the red light leakage rate of the polarizing film is less than 5%.

[0018] The polyvinyl alcohol film of the present invention can be used for various purposes, especially for optical films, such as polarizing films. The polyvinyl alcohol film obtained based on the technical content of the present invention can significantly improve the situation of film breakage when used to prepare optical films.

[0019] In addition, the inventors of the present invention have also discovered that when the polyvinyl alcohol film is further regulated to have a specific softening point temperature, the optical film produced therefrom has the characteristic of less red light leakage in a crossed nicol state. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is a curve diagram showing the change of storage modulus (E') of a polyvinyl alcohol film in water as a function of temperature according to an embodiment of the present invention;

[0021] Figures 2 to 4 is a schematic diagram of a sample preparation method for analyzing the turning point temperature of a polyvinyl alcohol film according to an embodiment of the present invention;

[0022] Figure 5 is a graph showing dimension change versus temperature in a softening point temperature analysis of a polyvinyl alcohol film according to an embodiment of the present invention;

[0023] Figure 6 FIG. 4 is a schematic diagram of sample preparation of a polyvinyl alcohol film for red light leakage evaluation according to an embodiment of the present invention. DETAILED DESCRIPTION

[0024] In order to make the description of the present invention more detailed and complete, the following is an illustrative description of the implementation and specific embodiments of the present invention, but this is not the only form of implementing or using the specific embodiments of the present invention. In this specification and patent scope, unless the context otherwise states, "a", "an" and "the" may also be interpreted as plural.

[0025] Although the numerical ranges and parameters used to define the present invention are approximate values, the relevant numerical values ​​in the specific embodiments have been presented as accurately as possible. However, any numerical value inherently inevitably contains standard deviations caused by individual testing methods. Here, the term "about" means that the actual value falls within the acceptable standard error of the mean value, which is determined by those with ordinary knowledge in the field to which the present invention belongs.

[0026] [Polyvinyl alcohol film]

[0027] In one aspect, the present invention provides a polyvinyl alcohol film, comprising a polyvinyl alcohol resin having a basicity of 95 mol% or more; wherein the storage modulus (E') of the polyvinyl alcohol film in water at 30°C to 55°C has a turning point temperature of 37 to 40°C. According to some embodiments, the thickness of the polyvinyl alcohol film of the present invention is 40 to 75 μm. Specifically, the range of any two of the following values, for example: 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm or 80 μm, the aforementioned values ​​are only illustrative and not restrictive.

[0028] The "modulus" described in this article is a physical property used to analyze the relationship between stress and strain in material mechanics, which is the ratio of stress to strain. If the stress applied to the material is a positive force, the modulus obtained is represented by E. The "storage modulus (E')" is the stored internal energy converted from the material absorbing the applied energy, which is usually used to recover deformation and maintain the original appearance of the material. It is related to the elastic characteristics of the material. It can also reflect the rigidity of the material. From a molecular point of view, the higher the E', the stronger the intermolecular force. For polyvinyl alcohol, the higher the E', the higher the crystallinity and the degree of molecular chain entanglement.

[0029] The "storage modulus (E') in water in the range of 30°C to 55°C has a turning point temperature (hereinafter referred to as the E' turning point temperature)" described in this article is obtained by immersing the polyvinyl alcohol film in water and measuring the change in E' of the polyvinyl alcohol film in a temperature increase mode; because a large amount of water is absorbed by the film, it forms hydrogen bonds with the -OH groups of the polyvinyl alcohol, causing the molecular chains of the polyvinyl alcohol to swell and separate, resulting in a reduction in the entanglement between the molecular chains; therefore, the E' analysis of polyvinyl alcohol immersed in water can be used to evaluate the change in crystallinity in the film at different temperatures. Furthermore, the E' change curve of the polyvinyl alcohol film in water with temperature has the following characteristics: Figure 1 The characteristic of the change curve between 30℃ and 55℃ is that there are two different slopes, and the intersection of the tangents of the two slopes is the E' turning point, and the corresponding temperature is the E' turning point temperature (such as Figure 1 (where the arrow points).

[0030] The physical meaning of the E' turning point temperature includes that it is the temperature at which the crystals in the polyvinyl alcohol film begin to dissolve in large quantities; if the E' turning point temperature is higher, it shows that the average crystal particles in the film are larger, so a large amount of crystal dissolution occurs only at relatively high temperatures. The inventors have found that when the E' turning point temperature is higher than 40°C, the polyvinyl alcohol film is prone to breakage during the swelling and stretching process in the polarizer process. Without being limited by a specific theory, it is speculated that the film may be easily damaged because the stress is excessively concentrated in the undissolved crystalline area. When the E' turning point temperature is less than 37°C, the crystal particles are too small, resulting in insufficient mechanical strength of the film, and the film is too soft and easy to break during swelling and stretching.

[0031] Therefore, in order to improve the situation that the polyvinyl alcohol film is easy to break during stretching, the E' turning point temperature needs to be controlled within a specific range; specifically, the E' of the polyvinyl alcohol film of the present invention in the range of 30°C to 55°C in water (the temperature range of the first stretching in the polarizer manufacturing process) has a turning point temperature of 37 to 40°C, such as but not limited to: 37°C, 37.1°C, 37.3°C, 37.5°C, 37.7°C, 37.9°C, 38°C, 38.1°C, 38.3°C, 38.5°C, 38.7°C, 38.9°C, 39°C, 39.1°C, 39.3°C, 39.5°C, 39.7°C, 39.9°C or 40°C. It should be noted that when the measuring temperature is greater than 55°C, the polyvinyl alcohol film may cause a sharp change in its physical properties due to the complete disappearance of crystals, so when analyzing the turning point temperature, the set analysis temperature range should avoid exceeding 55°C.

[0032] In addition, regarding the aforementioned measurement method of the E' turning point temperature, since the polyethylene film will absorb water (even moisture in the air) and affect its crystal state, molecular arrangement and other states, before measuring the E' turning point temperature of the polyethylene film, the moisture content of each polyethylene film to be measured can be adjusted to be consistent through pre-treatment, so that the state to be measured of each polyethylene film is consistent. The moisture content can usually be adjusted to about 8 to 9wt%, but this is not limited to this in this article.

[0033] The "basicity" described herein is a measured value obtained according to the JIS K 6726 (1994) standard test method. In one or more embodiments, the basicity of the polyvinyl alcohol-based resin is 95 mol% or more to obtain better optical properties, such as: 95 mol% or more, 95.5 mol% or more, 96 mol% or more, 96.5 mol% or more, 97 mol% or more, 97.5 mol% or more, 98 mol% or more, 98.5 mol% or more, 99 mol% or more or 99.5 mol% or more; if the basicity of the polyvinyl alcohol-based resin is 95 mol% or more, the mechanical strength and optical properties of the film can be enhanced. According to one embodiment of the present invention, the basicity of the polyvinyl alcohol-based resin of the present invention is greater than 99.90 mol%, for example, greater than 99.90 mol%, greater than 99.92 mol%, greater than 99.94 mol%, greater than 99.96 mol% or greater than 99.98 mol%; preferably, the basicity of the polyvinyl alcohol-based resin is greater than 99.95 mol%, for example, greater than 99.95 mol%, greater than 99.97 mol% or greater than 99.99 mol%; more preferably, the basicity of the polyvinyl alcohol-based resin is greater than 99.97 mol%, for example, greater than 99.97 mol%, greater than 99.98 mol% or greater than 99.99 mo1%.

[0034] According to one or more embodiments, the polyvinyl alcohol film of the present invention has a softening point temperature, which is less than or equal to 45°C. The "softening point temperature" described herein refers to the temperature (i.e., the transition temperature) when the film size begins to change significantly after a fixed positive force is applied to the material and the temperature is gradually increased. The softening point temperature can be regarded as the temperature at which the molecular chains in the amorphous region begin to move significantly under the action of a fixed positive force, which reflects the mechanical properties of the amorphous region. The higher the softening point temperature, the more energy the molecular chains in the amorphous region require to move significantly. It is believed that when the softening point temperature of the polyvinyl alcohol film is too high, it means that the molecular chains in the amorphous region are not easy to move, which may cause the iodine ions used for dyeing the polyvinyl alcohol film to be difficult to enter the amorphous region and adsorb on the polymer chains during the swelling and stretching step of the polarizer process, making the dyeing of the polyvinyl alcohol film difficult, which in turn leads to the problem of red light leakage in the prepared polarizer.

[0035] Therefore, in order to improve the red light leakage of the polarizer, the softening point temperature must be controlled to be less than or equal to a specific value; specifically, the polyvinyl alcohol film of the present invention has a softening point temperature less than or equal to 45°C, for example: less than or equal to 45°C, less than or equal to 44.5°C, less than or equal to 44°C, less than or equal to 43.5°C, less than or equal to 43°C, less than or equal to 42.5°C, less than or equal to 42°C, less than or equal to 41.5°C, less than or equal to 41°C, less than or equal to 40.5°C, less than or equal to 40°C or less than or equal to 35.5°C.

[0036] In one or more embodiments, the average degree of polymerization of the polyvinyl alcohol resin is 2000 to 3300, such as in the range of any two of the following values, for example: 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200 or 3300; preferably, the degree of polymerization of the polyvinyl alcohol resin is 2400 to 3300, for example: 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200 or 3300. The "average degree of polymerization" described herein is measured according to the JISK 6726 (1994) standard test method.

[0037] The above-mentioned E' turning point temperature and softening point temperature can be adjusted by adjusting the particle size, alkalinity and average polymerization degree of the resin raw material of the polyethylene film. In addition, it can also be adjusted by adjusting the stirring temperature and time of the raw materials during the preparation process, the flow temperature of the dissolved material and the maximum temperature of the oven drying, but it is not limited to this.

[0038] [Method for producing polyvinyl alcohol film]

[0039] The method for manufacturing the polyvinyl alcohol film of the present invention generally comprises the following steps: (a) a dissolution process: heating a polyvinyl alcohol resin to dissolve it, and adjusting the concentration of the polyvinyl alcohol resin to form a polyvinyl alcohol casting solution; (b) a casting process: casting the polyvinyl alcohol casting solution onto a casting drum, and obtaining a polyvinyl alcohol preformed film after peeling off from the casting drum; (c) a hot roller process: obtaining a polyvinyl alcohol film semi-finished product after the polyvinyl alcohol preformed film is contacted with a plurality of hot rollers; (d) an oven process: placing the polyvinyl alcohol film semi-finished product in an oven to dry it, thereby obtaining a polyvinyl alcohol film finished product; and depending on the situation, it may further comprise (e) a temperature and humidity control process: placing the polyvinyl alcohol film finished product in a temperature and humidity control box to adjust the temperature and humidity.

[0040] [Dissolution process]

[0041] According to some embodiments, the dissolution process mainly involves stirring the polyvinyl alcohol resin, solvent, plasticizer, etc. while raising the temperature to 130 to 165°C, and after the resin is evenly dissolved, adjusting the resin to an appropriate concentration to obtain a polyvinyl alcohol casting solution. The appropriate concentration of the resin is about 20wt% to 50wt%, for example: 20wt%, 30wt%, 40wt% or 50wt%; if the resin concentration is too low, the subsequent drying load of the film becomes high; conversely, if the resin concentration is too high, the viscosity is too high, which will make film making difficult.

[0042] In one or more embodiments, the polyvinyl alcohol resin used in the aforementioned dissolution process is obtained by polymerizing vinyl ester resin monomers to form a polyvinyl ester resin with an average degree of polymerization of 2000 to 3300, and then performing a saponification reaction to obtain a polyvinyl alcohol resin with a basicity greater than 95 mol%. In addition, the vinyl ester resin monomer can be a vinyl ester such as vinyl formate, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate or vinyl octanoate, or a combination thereof, which is not limited in the present invention. Preferably, vinyl acetate is used. In addition, copolymers formed by copolymerization of olefin compounds or acrylate derivatives with the aforementioned vinyl ester resin monomers can also be used. Among them, the olefin compound can be ethylene, propylene or butene, etc., which is not limited in the present invention; the addition amount of the olefin compound can be but not limited to 2 mol% to 4 mol%, such as 2 mol%, 2.5 mol%, 3 mol%, 3.5 mol% or 4 mol%, etc. The acrylate derivative may be acrylic acid, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate or n-butyl acrylate, etc., which is not limited in the present invention.

[0043] The polyvinyl alcohol resin is in granular form. When the particle size of the polyvinyl alcohol resin is larger (i.e., the mesh size is smaller), it is easier to cause incomplete dissolution of the resin crystals of the raw material, which affects the size and crystallinity of the finished product, making the crystal particles of the finished product larger and the crystallinity higher. In one or more embodiments, the particle size is defined by the mesh size, which is greater than or equal to 20 meshes, for example: greater than or equal to 20 meshes, greater than or equal to 30 meshes, or greater than or equal to 40 meshes.

[0044] In one or more embodiments, the solvent used in the aforementioned dissolution process can be used as long as it can dissolve the polyvinyl alcohol resin, so it is not limited in the present invention. As the solvent, for example, but not limited to: water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylenediamine, diethylenetriamine, etc., the above solvents can be used alone or in combination of two or more. Considering the environment and economic aspects, water is preferably used as the solvent in the present invention.

[0045] In one or more embodiments, the "plasticizer" described herein may be, but is not limited to, glycerol, ethylene glycol, propylene glycol, diethylene glycol, diglycerol, triethylene glycol, tetraethylene glycol or trimethylolpropane, or a combination of any of the aforementioned plasticizers; glycerol is preferred in the present invention. In one or more embodiments, the amount of the plasticizer added relative to the weight of the polyvinyl alcohol resin is 5wt% to 15wt%, specifically, for example but not limited to 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt% and 15wt%, and in a preferred embodiment, the amount of the plasticizer added relative to the weight of the polyvinyl alcohol resin is 10wt%.

[0046] In addition to the above-mentioned plasticizers, other additives may be further added in the dissolution process as needed, including but not limited to surfactants, etc.; the surfactants include but are not limited to cationic, anionic or non-ionic surfactants, and specifically may be but are not limited to: carboxylate type such as potassium laurate, sulfate ester type such as sodium laureth sulfate, sulfonate type such as dodecylbenzenesulfonate, alkylphenyl ether type such as polyoxyethylene octylphenyl ether, alcohol phenyl ether type such as polyethylene glycol monooctylphenyl ether, alkyl ester type such as polyoxyethylene laurate, alkylamine type such as polyoxyethylene laurylamine ether, alkylamide type such as polyoxyethylene lauramide, polypropylene glycol ether type such as polyoxyethylene polyoxypropylene ether, lauric acid diethanolamide, oleyl diethanolamide, allylphenyl ether type such as polyoxyalkylene allylphenyl ether, or sodium lauryl alcohol polyoxyethylene ether sulfate, etc.

[0047] In one or more embodiments, the temperature for dissolving the polyvinyl alcohol resin aqueous solution is preferably 130 to 165° C., such as any two of the following values, for example: 130° C., 135° C., 140° C., 145° C., 150° C., 155° C., 160° C. or 165° C. It is believed that the dissolution temperature affects the dissolution of the polyvinyl alcohol resin and the dispersion of the additives; when the dissolution temperature is too low, the E' turning point temperature and the softening point temperature of the finished film will also be too high; however, when the dissolution temperature is too high, the finished film may be partially yellowed.

[0048] In one or more embodiments, the time for dissolving the polyvinyl alcohol resin aqueous solution is preferably 1 to 5 hours, such as the range of any two of the following values, specifically for example: 1 hour, 2 hours, 3 hours, 4 hours or 5 hours. It is believed that if the dissolution time is too short, the dissolution of the polyvinyl alcohol resin and the dispersion of the additives are poor, so that the E' turning point temperature and the softening point temperature of the finished film are too high.

[0049] [Casting process]

[0050] According to some embodiments, the casting process mainly involves conveying the polyvinyl alcohol casting solution to a twin-screw extruder, mixing and defoaming the solution again in the extruder (for example, but not limited to, defoaming the solution using a twin-screw extruder), and then spitting the solution out from the T-slit die lip and casting the solution onto a rotating high-temperature casting drum (or casting roller), an endless belt, or the like as a support to form a film, thereby obtaining a polyvinyl alcohol preformed film. In one or more embodiments, during the casting process, the conveying temperature of the polyvinyl alcohol casting solution during conveying is preferably controlled to be at least 90° C. or above, for example, but not limited to, 90, 91, 92, 93, 94, 95, 96, 97, 98, or 99° C.; in addition, the polyvinyl alcohol casting solution after being mixed and defoamed again in the extruder must also be controlled to be at least 90° C. or above, for example, but not limited to, 90, 91, 92, 93, 94, 95, 96, 97, or 98° C.

[0051] In one or more embodiments, when the polyvinyl alcohol casting solution is cast onto the rotating high-temperature casting drum, the temperature of the casting drum is preferably 85 to 95° C., and the polyvinyl alcohol stays on the casting drum for preferably 0.6 to 1.2 minutes.

[0052] [Hot Roller Process]

[0053] According to some embodiments, the hot roller process mainly involves drying the upper and lower surfaces of the polyvinyl alcohol preformed film peeled off from the casting drum by contacting a plurality of hot rollers to obtain a polyvinyl alcohol film semi-finished product. The temperature of the plurality of hot rollers (e.g., 15 hot rollers) gradually decreases from high to low, and the starting hot roller is the hottest one among all the hot rollers (e.g., but not limited to, 90 to 99°C, specifically, for example, but not limited to, 90, 91, 92, 93, 94, 95, 96, 97, 98 or 99°C), and the temperature of the final hot roller is the coldest one among all the hot rollers (e.g., but not limited to, 30 to 50°C, specifically, for example, but not limited to, 30, 35, 40, 45 or 50°C).

[0054] [Oven process]

[0055] According to some embodiments, the oven process mainly uses an oven to dry the upper and lower surfaces of the polyvinyl alcohol film semi-finished product after peeling off the hot roller with hot air to obtain a polyvinyl alcohol film finished product.

[0056] In one or more embodiments, the oven is preferably a floating oven, and its temperature is controlled between 100°C and 120°C, specifically, the range between any two of the following values, for example: 100, 105, 110, 115 or 120°C. Recrystallization of polyvinyl alcohol occurs during the oven drying process. It is believed that the highest temperature in this section will affect the effect of recrystallization. Too high a temperature may result in too large crystal particles and too high a crystallinity, while too low a temperature may result in too small crystal particles and too low a crystallinity. In addition, since the polyvinyl alcohol arrangement in the film is fixed before entering the oven, the adjustment of the temperature has no significant effect on the softening point temperature.

[0057] [Temperature and humidity control process]

[0058] According to an embodiment of the present invention, after the polyvinyl alcohol film product has completed the above-mentioned process, it can be further placed in a temperature and humidity control box to adjust the temperature and humidity.

[0059] In one or more embodiments, the temperature of the temperature and humidity control box is between 35 and 45°C, specifically in the range between any two of the following values, for example: 35, 40 or 45°C, preferably 45°C. In one or more embodiments, the relative humidity of the temperature and humidity control box is preferably between 40 and 60%, specifically in the range between any two of the following values, for example: 40, 45, 50, 55 or 60%. In one or more embodiments, the polyvinyl alcohol film is preferably placed in the temperature and humidity control box for 20 to 40 minutes, for example: 20, 25, 30, 35 or 40 minutes. In one or more embodiments, for example, the polyvinyl alcohol film is placed in a temperature and humidity control box with a temperature of 45°C and a relative humidity of 50% for 40 minutes.

[0060] [Optical film and method for producing the same]

[0061] Another object of the present invention is to provide an optical film, which is made from the aforementioned polyvinyl alcohol film. The "optical film" described herein may be a polarizing film, a phase difference film, a viewing angle enhancement film or a brightness enhancement film, etc., in particular a polarizing film. According to some embodiments, the "method for manufacturing an optical film" described in this case refers to a method for manufacturing a polarizing film, and further, the polyvinyl alcohol film is manufactured into a polarizing film, and the situation of breakage caused by stretching / extension during the preparation process and the degree of red light leakage of the finished film are evaluated. The manufacturing method includes a dyeing step for adsorbing iodine ions, a boric acid treatment step and a water washing step; a uniaxial stretching extension step may be implemented in the boric acid treatment step or in a stage before the step. Preferably, a swelling step for swelling the polyvinyl alcohol film with water may be provided before the dyeing step. In addition, a final drying step is usually provided after the water washing step.

[0062] In the swelling step, the polyvinyl alcohol film is immersed in a treatment bath (e.g., pure water) at a temperature of 30°C to 55°C for washing and swelling of the film surface. The swelling treatment time is generally 5 to 300 seconds, preferably 20 to 240 seconds. According to some embodiments, a plurality of guide rollers are arranged in the swelling tank containing the treatment bath to transport the polyvinyl alcohol film. Subsequently, the polyvinyl alcohol film is stretched in the machine direction (MD) to 1.05 to 2.5 times of the original length, and then the dyeing step is performed.

[0063] In the dyeing step, the polyvinyl alcohol film after the above-mentioned swelling step is immersed in a dyeing tank containing a dyeing bath. The conditions of the dyeing treatment can be determined based on the range within which the iodine is adsorbed on the polyvinyl alcohol film without causing adverse conditions such as extreme dissolution and devitrification of the film. The dyeing bath in the dyeing step is, for example, an aqueous solution containing iodine and potassium iodide. The concentration of iodine in the dyeing bath is preferably 0.01wt% to 0.5wt%, and the concentration of potassium iodide is preferably 0.01wt% to 10wt%. A specific example may be, but is not limited to, an aqueous solution of iodine with a concentration of 0.037wt% and potassium iodide with a concentration of 1.85wt%. In addition, other iodides such as zinc iodide can also be used instead of potassium iodide, or other iodides can be used in addition to potassium iodide. The temperature of the dyeing bath is usually 20 to 40°C, for example 20, 30 or 40°C, and the time of the dyeing treatment (dyeing time) is usually 10 to 600 seconds, preferably 30 to 200 seconds. Next, the polyvinyl alcohol film is stretched along a machine direction to 2 to 4 times of its original length, and then subjected to a boric acid treatment and a stretching step.

[0064] In the boric acid treatment and extension step, the iodine-dyed polyvinyl alcohol film is treated with an aqueous solution containing boric acid to make it cross-linked, and the adsorbed iodine is fixed in the resin. This step is usually carried out by immersing the polyvinyl alcohol film after the dyeing step in a fixing tank containing a treatment bath containing boric acid. The boric acid treatment bath preferably contains iodide in addition to boric acid. The iodide used can be potassium iodide or zinc iodide, for example, an aqueous solution containing boric acid and potassium iodide at a concentration of 5.5wt%. In addition, compounds other than iodide can also coexist in the boric acid treatment bath, such as zinc chloride, cobalt chloride, zirconium chloride, sodium thiosulfate, potassium sulfite, sodium sulfite, potassium sulfate, sodium sulfate, etc. The boric acid treatment and extension step is usually carried out at 50-70°C, for example, at 55°C, and the treatment time is usually 10-600 seconds, preferably 20-300 seconds, and more preferably 20-100 seconds. Next, the polyvinyl alcohol film is stretched along the mechanical direction to more than 3 times of its original length before proceeding to subsequent steps; the upper limit of the stretching ratio is not particularly limited, but is preferably less than 8 times, for example, stretched to include but not limited to 3.3 times or more, such as 3.3 to 8.0 times, more preferably 3.5 to 6.0 times, and particularly preferably 4.0 to 5.5 times.

[0065] After the polyvinyl alcohol film has gone through the above steps and the subsequent washing and drying steps, a polarizing film is formed. In the washing and drying steps, the iodine solution and boric acid remaining on the film surface are washed with water or an aqueous solution containing iodide, for example but not limited to washing with a potassium iodide aqueous solution with a concentration of 5.5wt%. Then, after a drying step, for example but not limited to drying in an oven at a temperature of 60°C for 5 minutes, a polarizing film is formed. Furthermore, a protective layer can be formed on at least one side of the polarizing film to make a polarizing film product (or polarizer). In detail, the protective layer is preferably a component having functions such as preventing surface wear of the polarizing film, and comprises a transparent resin. According to different embodiments, the protective layer can be provided on only one side of the polarizing film, but is preferably formed on both sides of the polarizing film. The protective layer can be a protective film of a transparent resin material; the transparent resin can be an acrylic resin such as methyl methacrylate resin, an olefin resin, a polyvinyl chloride resin, a cellulose resin, a styrene resin, an acrylonitrile-butadiene-styrene copolymer resin, an acrylonitrile-styrene copolymer resin, a polyvinyl acetate resin, a polyvinylidene chloride resin, a polyamide resin, a polyacetal resin, a polycarbonate resin, a modified polyphenylene ether resin, a polyester resin (polybutylene terephthalate resin, polyethylene terephthalate resin, etc.), a polysulfone resin, a polyethersulfone resin, a polyarylate resin, a polyamide-imide resin, a polyimide resin, an epoxy resin, an oxetane resin, etc.; preferably, a cellulose resin is used, for example, triacetate cellulose (TAC).

[0066] Example

[0067] Hereinafter, the present invention will be further described with detailed description and specific examples. However, it should be understood that these specific examples are only used to help the present invention to be more easily understood and are not used to limit the scope of the present invention.

[0068] 1. Polyvinyl alcohol film preparation

[0069] Herein, the present invention provides a non-limiting method for preparing polyvinyl alcohol films. According to a method similar to the method disclosed below, non-limiting example polyvinyl alcohol films (Examples 1-16) and comparative example polyvinyl alcohol films (Comparative Examples 1-8) were prepared.

[0070] The following are the main steps common to the present embodiment and the comparative example in manufacturing the polyvinyl alcohol film, and the following Table 1 will show in detail the differences in one or more process parameters between the present embodiment and the comparative example: 1. First, 1800 kg of polyvinyl alcohol resin having a specific particle size, basicity and polymerization degree of 2000 to 3300 (specific polymerization degree is shown in Table 1), 4000 kg of water and 180 kg of plasticizer glycerol are added to a dissolution tank, and the dissolution temperature is raised to a specific temperature while stirring, and the dissolution time is controlled; after the dissolution is uniform, water is added to adjust the resin concentration to 30 wt % to obtain a polyvinyl alcohol casting solution (or film-making stock solution); the polyvinyl alcohol resin in the embodiment and the comparative example is a polyvinyl alcohol resin polymerized from vinyl acetate and not modified (i.e., not containing other comonomers); in addition, the specific particle size, basicity, polymerization degree, dissolution temperature and dissolution time of the polyvinyl alcohol resin are shown in Table 1. 2. The polyvinyl alcohol casting solution is conveyed to a double-screw extruder at a conveying temperature of 99°C. The solution is mixed and defoamed again by the extruder to control the temperature of the casting solution to 98°C. The casting solution is then discharged from the T-slit die lip and cast onto a rotating high-temperature casting drum for drying and film formation to form a primary formed film. 3. After the polyvinyl alcohol preformed film is peeled off from the casting drum, 15 hot rollers are used to contact the upper and lower surfaces of the dry film. The first hot roller has the highest temperature of all the hot rollers, which is 95°C; and the temperature of the subsequent hot rollers gradually decreases from high to low, and the temperature of the 15th hot roller will reach 40°C. 4. Next, the upper and lower surfaces of the polyvinyl alcohol preliminary film are dried with hot air in a floating oven to produce a polyvinyl alcohol film product. The specific maximum drying temperature of the oven is shown in Table 1. 5. Subsequently, the finished polyvinyl alcohol film is placed in a temperature and humidity control box at a temperature of 45° C. and a relative humidity of 50% for 40 minutes to obtain a polyvinyl alcohol film.

[0071] Table 1

[0072] 2. Polarizer Preparation

[0073] Here, the present invention provides a non-limiting method for preparing a polarizer from a polyvinyl alcohol film. According to the method disclosed below, non-limiting example polyvinyl alcohol films (Examples 1-16) and comparative example polyvinyl alcohol films (Comparative Examples 1-8) were prepared into corresponding polarizers.

[0074] The following are the main steps for preparing polarizers in the embodiments and comparative examples of the present invention: after unwinding the polyvinyl alcohol film, let it enter the swelling tank filled with 30°C pure water to wash and swell the film surface; after the polyvinyl alcohol film is stretched to 1.2 times of the original length in the mechanical direction, it then enters the dyeing tank controlled at 30°C and containing an aqueous solution of 0.037wt% iodine and 1.85wt% potassium iodide for dyeing, and at the same time, the polyvinyl alcohol film is extended to 3.4 times of the original length in the mechanical direction; after dyeing, it enters the extension tank controlled at 55°C and containing an aqueous solution of 5.5wt% boric acid and potassium iodide, and after the polyvinyl alcohol film is extended to 6 times of the original length in the mechanical direction, the iodine solution and boric acid remaining on the film surface are washed with an aqueous solution containing 5.5wt% potassium iodide. Then, it is dried in a 60°C oven for 5 minutes, and the upper and lower surfaces are bonded with triacetyl cellulose protective films and dried to make a polarizer.

[0075] 3. Analytical methods

[0076] Here, the present invention provides analysis and test methods for the polyvinyl alcohol films of Examples 1 to 16 and Comparative Examples 1 to 8.

[0077] Resin particle size

[0078] Specifically, the "pass" shown in Table 1 means that the particle size of the resin raw material is substantially smaller than or equal to the hole size of the sieve used for measurement, and the so-called "residual" means that the particle size of the resin raw material is substantially larger than or equal to the hole size of the sieve used for measurement.

[0079] Alkalinity

[0080] The basicity determination method of the present invention is based on the JIS K 6726 (1994) standard method.

[0081] Average degree of polymerization

[0082] The method for measuring the average degree of polymerization in the present invention is based on the JIS K 6726 (1994) standard method.

[0083] E' turning point temperature

[0084] Instrument and brand: TA Instruments DMA 850

[0085] Sample preparation method: Cut the polyvinyl alcohol film into strips with a length of 5 cm in the machine direction (MD) and 5 mm in the width direction (TD). Before loading the film, adjust the moisture content of the polyvinyl alcohol film to 8wt% to 9wt% to make the polyvinyl alcohol film uniform. Figure 2 , clamp one end of the polyvinyl alcohol film 2 with a dovetail clip 3 of about 1.11g, and insert the other end into the immersion stretching fixture 1, so that a part of the polyvinyl alcohol film 2 is placed between the fixed axis 1a and the lower fixed axis 1b, so that the lower end 3a of the dovetail clip 3 is 1cm away from the immersion stretching fixture 1 ( Figure 2 The distance a) shown in FIG. 1 is a distance between the upper end 2a of the polyvinyl alcohol film 2 and the upper end of the immersion stretching fixture 1, and a reserved space is provided; then, the upper fixing shaft 1a is locked to fix the polyvinyl alcohol film 2. Next, refer to Figure 3 , vertically place the entire immersion stretching fixture 1 together with the polyvinyl alcohol film 2 and dovetail clamp 3 held by it into a 100mL beaker 4 filled with pure water so that the liquid level of the beaker is located on the upper fixed axis, and control the temperature of the beaker 4 in a 30℃ constant temperature water tank (not shown in the figure) to allow the polyvinyl alcohol film 2 to swell under a load (the weight of the dovetail clamp 3) for 20 minutes. Finally, refer to Figure 4 , take out the immersion and stretching fixture 1 from the beaker 4 and keep it upright, use the weight of the dovetail clamp 3 to stretch the polyvinyl alcohol film 2, and after ensuring that the polyvinyl alcohol film 2 is centered, lock the lower fixed axis 1b of the immersion and stretching fixture 1, and then remove the excess polyvinyl alcohol film 2c (i.e. Figure 4 The grid-like part in the middle is cut off, and the sample is the polyvinyl alcohol film 2b that is swollen under load and clamped in the immersion and stretching fixture 1.

[0086] Test conditions: The upper sample is still fixed in the immersion and stretching fixture, and the oscillation heating mode is selected. The sample and the immersion and stretching fixture holding it are placed in an immersion tank filled with deionized water. The frequency is set to 1Hz, the amplitude is set to 200μm, the holding pressure (force track) is set to 200%, and the temperature is set to measure from 30℃ to 65℃. Before the analysis, the film is stretched with a static force of 0.15N before starting the analysis at a heating rate of 1℃ / min and drawing a curve of the storage modulus (E') versus temperature. Among them, the thermocouple sensing end is placed at a height of 5mm from the bottom of the water tank.

[0087] Data processing: Change the coordinate axis of the storage modulus (E') to a linear coordinate axis, use the onset analysis built into the software included with the instrument, set the onset analysis temperature range to 30 to 45°C, and the software will automatically bring out the turning point temperature.

[0088] Softening point temperature

[0089] Instrument and brand: TA Instruments TMA Q400

[0090] Sample preparation method: Use a hole puncher to cut the polyvinyl alcohol film into circles with a diameter of 5 mm. Before loading the film on the machine, adjust the moisture content of the film to 8 wt % to 9 wt % to make the state of the film consistent.

[0091] Test conditions: Use a penetration probe, fix the normal force at 0.05N and the nitrogen flow rate at 100mL / min; place the concave surface of the circular sample (the concave surface is formed by the natural warping of the circular film cut by the puncher when the sample is prepared) on a quartz platform at room temperature, and then place the measuring tip of the penetration probe in the center of the sample for measurement. The analysis temperature is set at 10 to 150°C, and the heating rate is 10°C / min.

[0092] Data processing: Click the Tg analysis button in the analysis software Universal Analysis, set the analysis temperature from 15 to 120°C, and plot the temperature with dimension change. The lowest temperature analyzed by the instrument is the softening point temperature. Figure 5 As shown (the circled area is the softening point temperature).

[0093] 4. Evaluation methods and results

[0094] Here, the present invention provides evaluation methods for polyvinyl alcohol films and polarizers of Examples and Comparative Examples, and corresponding results thereof with the above-mentioned analysis contents.

[0095] Film breaking evaluation

[0096] Test conditions: 8000 m of polyvinyl alcohol film was used continuously to make polarizers.

[0097] Evaluation criteria: ◎: No cracking occurred during the process ○: One breakage occurred during the process ×: More than 1 crack occurred during the process

[0098] Furthermore, the film breaking evaluation results of the polyvinyl alcohol films of Examples 1 to 16 and Comparative Examples 1 to 8 are shown in Table 2 together with their E' inflection point temperatures.

[0099] Table 2

[0100] According to Table 2, the E' inflection point temperature parameters measured in the E' inflection point temperature analysis of the polyvinyl alcohol film samples of Examples 1 to 16 are all within the range of 37 to 40°C, and it is observed that these polyvinyl alcohol film samples all obtain good results of film breaking evaluation. On the contrary, the E' inflection point temperature parameters measured in the E' inflection point temperature analysis of the polyvinyl alcohol film samples of Comparative Examples 1 to 5 are all beyond the range of 37 to 40°C, and these polyvinyl alcohol film samples cannot obtain ideal results in film breaking evaluation. In view of this, only by controlling the storage modulus (E') of the polyvinyl alcohol film in water in the range of 30°C to 55°C to have an inflection point temperature of 37 to 40°C can the situation of easy film breaking during stretching be improved.

[0101] Red light leak evaluation

[0102] Sample preparation: The polyvinyl alcohol films of the embodiments of the present invention and the comparative examples were used to prepare polarizers according to the above polarizer manufacturing process. Figure 6 The distance x shown in the figure), the middle, and 5 cm from the right side (as shown in the figure Figure 6 Cut two pieces of 2*2cm in area at three positions of the distance x) shown in 2 Samples (such as Figure 6 Then, two polarizers cut from the same position are used as test samples.

[0103] Test instrument: Spectrophotometer Jasco V-7100.

[0104] Test method:

[0105] Transmittance Ts (%): According to JIS Z 8722 (Method for Determining Object Color), the visual sensitivity calibration is performed in the visible light field with C light source and 2 degrees of field of view. Assume that the direction of light is the x-axis, the virtual vertical normal perpendicular to the direction of light is the z-axis, and the y-axis is perpendicular to the x-axis and the z-axis. Take one of the samples at a position, place it on the yz plane, and use the direction of light as the rotation axis. Rotate the sample forward so that its slow axis (here, the MD direction) is sandwiched between the virtual vertical normal (z-axis) at +45° and measure one transmittance; and reverse the sample so that its slow axis is sandwiched between the virtual vertical normal (z-axis) at -45° and measure another transmittance. Take the average of the two to obtain Y1. Take another sample at the same position, measure two transmittances in the same way as above, and take the average of the two transmittances to obtain Y2. Then take the average of Y1 and Y2 as the transmittance Ts (%) at that position.

[0106] Transmittance T700⊥(%): Take two test samples at the same position and overlap each other, rotate one of the samples forward so that the slow axis between the two samples is +45°, and measure the transmittance T of light with a wavelength of 700nm 45; Reversely rotate one of the polarizers so that the slow axis between the polarizers is -45°, and measure the transmittance T of light with a wavelength of 700nm -45 . Take T 45 With T -45 The average value of the values ​​is taken as the transmittance T700⊥(%).

[0107] Red light leakage rate: With transmittance Ts (%) as the horizontal axis and transmittance T700⊥ (%) as the vertical axis, an approximate straight line is drawn for the analysis values ​​at the three positions, and the transmittance T700⊥ (%) when the transmittance is 44% is obtained from the approximate straight line (i.e. the orthogonal transmittance of light with a wavelength of 700nm), which is the red light leakage rate.

[0108] Evaluation criteria: The red light leakage rate (ie, the red light leakage ratio) is preferably less than 5%.

[0109] Furthermore, the red light leakage evaluation results of the polarizers of Examples 1 to 16 and Comparative Examples 1 to 8 are presented in Table 3 together with their softening point temperatures.

[0110] Table 3

[0111] According to Table 3, when the softening point temperature of the polyvinyl alcohol film is controlled to be less than or equal to 45°C, the polarizer prepared by the polyvinyl alcohol film has a red light leakage rate of less than 5%, such as Examples 1 to 16 and Comparative Examples 3, 4, 6 to 8 (although the red light leakage rate of Comparative Examples 3, 4, 6 to 8 is less than 5%, they are still considered as poor comparative examples due to poor evaluation of the upper film breaking). On the contrary, when the softening point temperature of the polyvinyl alcohol film exceeds 45°C, the polarizer prepared by the polyvinyl alcohol film has a red light leakage rate exceeding 5% (such as Comparative Examples 1, 2 and 5). In view of this, when the softening point temperature is controlled to be less than or equal to 45°C, the red light leakage problem of the polarizer prepared by the polyvinyl alcohol film can be improved.

[0112] Herein, all ranges provided are intended to include each specific range within a given range and combinations of sub-ranges between the given ranges. In addition, unless otherwise stated, all ranges provided herein include the endpoints of the ranges. Thus, ranges 1-5 specifically include 1, 2, 3, 4, and 5, as well as sub-ranges such as 2-5, 3-5, 2-3, 2-4, 1-4, etc.

[0113] All publications and patent applications cited in this specification are incorporated herein by reference, and each individual publication or patent application is specifically and individually indicated to be incorporated herein by reference for any and all purposes. In the event of any inconsistency between any publication or patent application incorporated herein by reference, this document controls. Explanation of symbols

[0114] 1 Immersion tensile fixture 1a Upper fixed shaft 1b Lower fixed shaft 2 Polyvinyl alcohol film 2a Top 2b Polyvinyl alcohol film swollen under load 2c Excess polyvinyl alcohol film 3 Dovetail clamp 3a bottom 4 beakers a distance.

Claims

1. A polyvinyl alcohol film comprising a polyvinyl alcohol resin having a basicity of 95 mol % or more; wherein: The storage modulus (E') of the polyvinyl alcohol film in water at a temperature between 30°C and 55°C has a turning point temperature of 37°C and 40°C.

2. The polyvinyl alcohol film according to claim 1, wherein The polyvinyl alcohol film has a softening point temperature, and the softening point temperature is less than or equal to 45°C.

3. The polyvinyl alcohol film according to claim 1, wherein The basicity of the polyvinyl alcohol resin is greater than 99.90 mol%.

4. The polyvinyl alcohol film according to claim 3, wherein The basicity of the polyvinyl alcohol resin is greater than 99.95 mol %.

5. The polyvinyl alcohol film according to claim 4, wherein The basicity of the polyvinyl alcohol resin is greater than 99.97 mol %.

6. The polyvinyl alcohol film according to claim 1, wherein The average polymerization degree of the polyvinyl alcohol resin is 2,000 to 3,300.

7. The polyvinyl alcohol film according to claim 1, wherein The average polymerization degree of the polyvinyl alcohol resin is 2400 to 3300.

8. The polyvinyl alcohol film according to any one of claims 1 to 3, wherein The polyvinyl alcohol film has a thickness of 40 to 75 μm.

9. An optical film made from the polyvinyl alcohol film according to any one of claims 1 to 8.

10. The optical film according to claim 9, which is a polarizing film.

11. The optical film of claim 10, wherein the red light leakage rate of the polarizing film is less than 5%.