Polyvinyl alcohol film and optical film prepared from same

By regulating the dissolution amount and storage modulus curve slope value of the polyvinyl alcohol film, the fracture problem of the polyvinyl alcohol film during stretching and the insufficient optical performance of the polarizing film are solved, and high monomer transmission and low red light leakage are achieved. Preparation of polarizing films with a ratio.

CN119019797APending Publication Date: 2024-11-26CHANG CHUN PETROCHEMICAL CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202410636343.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The conventional polyvinyl alcohol film is prone to break when preparing the polarizing film, and the obtained polarizing film has a low transmittance and a high red light leakage rate.

Method used

By controlling the polyvinyl alcohol film to soak in water at a specific temperature and time, the curve slope value of its dissolution amount and storage modulus is controlled, ensuring that the extension tension of the polyvinyl alcohol film is moderate when stretched, thereby improving the optical performance of the polarizing film.

Benefits of technology

It effectively reduces the risk of fracture of the polyvinyl alcohol film when stretching, and improves the monomer transmittance of the polarizing film and reduces the red light leakage rate, achieving efficient optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019797A_ABST
    Figure CN119019797A_ABST
Patent Text Reader

Abstract

The invention relates to a polyvinyl alcohol film and an optical film prepared from the same. The polyvinyl alcohol film comprises polyvinyl alcohol resin; wherein the polyvinyl alcohol film has a polyvinyl alcohol dissolution amount of 0.20 to 9.00 ppm / m < 2 > when soaked in water at 40 DEG C for 1 minute; and the polyvinyl alcohol film has a curve of storage modulus (E ') relative to temperature measured in water at a temperature rise rate of 1 DEG C / min from 30 DEG C to 65 DEG C, the curve having a slope value in an interval of 45 DEG C to 55 DEG C, the absolute value of the slope value being 0.20 to 0.70 MPa / DEG C. The polyvinyl alcohol film disclosed by the invention is low in extension tension, so that the polyvinyl alcohol film is not easy to break during stretching, and the optical film prepared from the polyvinyl alcohol film has the characteristics of high monomer transmittance and low red light leakage rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyvinyl alcohol (PVA) product, in particular to a polyvinyl alcohol film and an optical film made therefrom, but not limited thereto. Background Art

[0002] Polyvinyl alcohol (PVA) film is a hydrophilic material obtained by coating and drying an aqueous solution containing polyvinyl alcohol polymer and a plasticizer. It has high transparency, mechanical strength, water solubility, good processability and other properties. It has been widely used in various optical films for packaging materials or electronic products, such as polarizing films.

[0003] The polarizing film obtained by processing the polyvinyl alcohol film through the polarization process has the property of only allowing light in a specific direction to pass through, and can thereby control the brightness of the light passing through; based on this property, the polarizing film is used in various displays, glasses and wearable devices, becoming an indispensable component. The so-called polarizing process generally includes steps such as swelling, stretching and dyeing; specifically, the polyvinyl alcohol film will be placed in a solution to carry out the aforementioned steps, allowing the dye molecules to diffuse into the molecules in the polyvinyl alcohol film, and through stretching to obtain a relatively regular arrangement, so that the polarizing film can absorb the light component parallel to its arrangement direction and allow the light component in the vertical direction to pass through, thereby generating polarization characteristics. However, the existing polyvinyl alcohol film often has excessive extension tension, which can easily cause film breakage when preparing the polarizing film.

[0004] Prior art, such as Taiwan Invention Patent Publication No. 202233739, discloses a polyvinyl alcohol film, in which on at least one side of the polyvinyl alcohol film, the average value of the positive silicon fragment ion detection intensity obtained by positive ion analysis based on time-of-flight secondary ion mass spectrometry is 0.001 to 0.01; wherein, the average value of the positive silicon fragment ion detection intensity is on an arbitrary straight line parallel to the TD direction of the polyvinyl alcohol film, and the polyvinyl alcohol film is divided into 6 equal points in the TD direction, and the average value of the positive silicon fragment ion detection intensity obtained by positive ion analysis based on time-of-flight secondary ion mass spectrometry is used as a technical means to achieve that tensile fracture is not likely to occur during uniaxial stretching.

[0005] In addition, the prior art also discloses that the characteristics of the polarizing film can be improved by changing the structure of polyvinyl alcohol and adjusting the process of polyvinyl alcohol film or polarizing film; for example, Taiwan Invention Patent Publication No. 201719207 discloses a polarizing film with good polarization performance and less leakage of red light in the orthogonal polarization state. In addition, the suspected technology such as Taiwan Invention Patent Publication No. 202400694 also discloses a polyvinyl alcohol film with good elongation and not easy to break during the manufacture of polarizing film, so that a high degree of elongation can be obtained to obtain a polarizing film with high polarization; and because the dissolution and precipitation of polyvinyl alcohol resin can be suppressed during the manufacture of polarizing film, the pollution of polarizing film manufacturing equipment can be suppressed, and then the manufacture can be carried out with a high yield. Summary of the invention

[0006] In the prior art, when a polyvinyl alcohol film is used to prepare a polarizing film, the polyvinyl alcohol film is often prone to film breakage during the preparation of the polarizing film due to excessive stretching tension, and the polarizing film prepared from the polyvinyl alcohol film also often has problems of low monomer transmittance and high red light leakage rate. In this regard, the inventors have found that by regulating the polyvinyl alcohol film so that it has a specific amount of polyvinyl alcohol dissolved when immersed in water at a specific temperature and time, and the storage modulus (E') relative to temperature curve measured under specific conditions has a specific slope value absolute value within a specific temperature range, the problem of the polyvinyl alcohol film being prone to film breakage during stretching can be improved, thereby improving the low monomer transmittance and high red light leakage rate of the subsequently prepared polarizing film.

[0007] Specifically, the present invention provides a polyvinyl alcohol film, comprising: a polyvinyl alcohol resin; wherein the polyvinyl alcohol film has a polyvinyl alcohol dissolution amount of 0.20 to 9.00 ppm / m after being immersed in 40° C. water for 1 minute. 2 ; and the storage modulus (E') curve relative to temperature of the polyvinyl alcohol film in water is measured at a heating rate of 1°C / min from 30°C to 65°C, and the curve has a slope value in the range of 45°C to 55°C, and the absolute value of the slope value is 0.20 to 0.70 MPa / °C.

[0008] According to some embodiments of the present invention, the dissolution amount of polyvinyl alcohol is 1.60 to 7.20 ppm / m 2 ; and the absolute value of the slope is 0.20 to 0.60 MPa / ℃.

[0009] According to some embodiments of the present invention, the absolute value of the slope is 0.25 to 0.60 MPa / °C.

[0010] According to some embodiments of the present invention, the absolute value of the slope is 0.35 to 0.55 MPa / °C.

[0011] According to some embodiments of the present invention, the polyvinyl alcohol film has a storage modulus (E') of 5.00 to 14.00 MPa at 45° C.; and the polyvinyl alcohol film has a storage modulus (E') of 3.00 to 7.00 MPa at 55° C.

[0012] According to some embodiments of the present invention, the polyvinyl alcohol film has a storage modulus (E') of 8.00 to 11.50 MPa at 45° C.; and the polyvinyl alcohol film has a storage modulus (E') of 4.00 to 6.00 MPa at 55° C.

[0013] According to some embodiments of the present invention, the polyvinyl alcohol film has an extension tension of 13.0 to 30.0 N / mm when immersed in a 2 wt. % boric acid aqueous solution at 50° C. for 30 seconds. 2 .

[0014] According to some embodiments of the present invention, the polyvinyl alcohol resin has an average degree of polymerization of 1500 to 3500.

[0015] According to some embodiments of the present invention, the polyvinyl alcohol resin has a polymer dispersity index (PDI) less than or equal to 3.5.

[0016] According to some embodiments of the present invention, the polyvinyl alcohol film has a thickness of 45 to 75 μm.

[0017] Another aspect of the present invention provides an optical film, which is made from the polyvinyl alcohol film.

[0018] According to some embodiments of the present invention, the optical film is a polarizing film.

[0019] According to some embodiments of the present invention, the polarizing film has a single body transmittance greater than or equal to 42.5%, and a red light leakage rate less than 5.0%.

[0020] The polyvinyl alcohol film of the present invention can be used for a variety of purposes, especially for optical films, such as polarizing films. The polyvinyl alcohol film obtained based on the technical content of the present invention has a small extension tension during the polarizing film manufacturing process, so it is not easy to break the film. In addition, the polarizing film made from the polyvinyl alcohol film has a low red light leakage rate and a high monomer transmittance.

[0021] Furthermore, the inventors of the present invention have also found that by controlling the polyvinyl alcohol film to have a specific range of storage modulus (E') at temperatures of 45° C. and 55° C., the red light leakage rate of the polarizing film made from the polyvinyl alcohol film can be further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] To make the above and other purposes, features, advantages and embodiments of the present application more understandable, the accompanying drawings are described as follows:

[0023] Figures 1 to 4 FIG. 4 is a schematic diagram of the absolute value of the slope of a storage modulus (E′) versus temperature curve of a polyvinyl alcohol film according to an embodiment of the present invention.

[0024] Figure 5 , 6 6A and 6B are schematic diagrams of analyzing the single body transmittance and red light leakage rate of the polarizing film corresponding to the polyvinyl alcohol film according to an embodiment of the present invention.

[0025] Figure 7 FIG. 4 is a schematic diagram of sampling of a polarizing film corresponding to a polyvinyl alcohol film when analyzing red light leakage rate according to an embodiment of the present invention. DETAILED DESCRIPTION

[0026] In order to make the description of the present invention more detailed and complete, the following provides an illustrative description of the implementation mode and specific examples of the present invention, but this is not the only form of implementing or using the specific examples of the present invention. In this specification and claims, unless the context otherwise states, "a", "an" and "the" may also be interpreted as plural.

[0027] Although the numerical ranges and parameters used to define the present invention are approximate values, the relevant numerical values ​​in the specific embodiments have been presented as accurately as possible. However, any numerical value inherently inevitably contains standard deviations caused by individual testing methods. Here, the term "about" means that the actual value falls within the acceptable standard error of the mean value, which is determined by ordinary technicians in the field to which the present invention belongs.

[0028] [Polyvinyl alcohol film]

[0029] In one aspect, the present invention provides a polyvinyl alcohol film, comprising: a polyvinyl alcohol resin; wherein the polyvinyl alcohol dissolution amount of the polyvinyl alcohol film after being immersed in 40° C. water for 1 minute is 0.20 to 9.00 ppm / m 2 ; and the polyvinyl alcohol film is heated in water from 30°C to 65°C at a heating rate of 1°C / min to obtain a storage modulus (E')-to-temperature curve, the curve having a slope value in the range of 45°C to 55°C, and the absolute value of the slope value is 0.20 to 0.70 MPa / °C. According to some embodiments of the present invention, the polyvinyl alcohol film has a thickness of 45 to 75 μm; specifically, for example, the following values ​​or ranges between any two thereof, for example: 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm and 75 μm, the aforementioned values ​​are for illustration only and are not restrictive.

[0030] The "modulus" mentioned in this article is a physical property used to analyze the relationship between stress and strain in material mechanics. It is the ratio of stress to strain. If the stress applied to the material is a positive force, the modulus obtained is represented by E. The "storage modulus (E')" is the stored internal energy converted from the material absorbing the applied energy. It is usually used to restore deformation and maintain the original appearance of the material. It is related to the elastic characteristics of the material.

[0031] The "storage modulus (E') versus temperature curve of the polyvinyl alcohol film measured in water at a heating rate of 1°C / min from 30°C to 65°C (hereinafter referred to as the storage modulus versus temperature curve)" described herein has the following characteristics: Figure 1 The dual slope characteristics shown in the figure, where the slope value after the turning point temperature (such as Figure 1 The absolute value of the slope (indicated by the middle dotted line) characterizes the rate at which the crystals in the polyvinyl alcohol film are dissolved in water during the heating process. Since the heating rate during the analysis is fixed, the larger the absolute value of the slope value, the faster the crystal dissolves in the same time. It can be seen that the crystals in the polyvinyl alcohol film are smaller and more uniform. Without being limited by a specific theory, it is believed that the crystals in the polyvinyl alcohol film have a moderate size and uniformity, which is helpful for stretching and dyeing in the polarizing film process, so that a polarizing film with high monomer transmittance and low red light leakage rate can be prepared; further, moderate crystals can reduce the extension tension during stretching, thereby reducing the occurrence of film breakage. The inventors have found that if the absolute value of the slope value is too large, the polyvinyl alcohol film will be easily broken due to insufficient mechanical strength; if the absolute value of the slope value is too small, the polyvinyl alcohol film will have too much residual crystal dissolution (that is, the crystals are not completely dissolved, and the remaining crystals) so that the extension tension is too large, and the film is prone to breakage.

[0032] Therefore, in order to improve the problem that the polyvinyl alcohol film is easy to break due to excessive extension tension during stretching and the subsequent polarizing film has low monomer transmittance and high red light leakage rate, it is necessary to control the absolute value of the slope value within a specific range; specifically, the polyvinyl alcohol film is heated from 30°C to 65°C in water at a heating rate of 1°C / min to measure a storage modulus (E') relative temperature curve, and the curve has a slope value in the range of 45°C to 55°C, and the absolute value of the slope value is 0.20 to 0.70 MPa / °C, such as the following values ​​or any two thereof The range between: 0.20MPa / ℃, 0.25MPa / ℃, 0.30MPa / ℃, 0.35MPa / ℃, 0.40MPa / ℃, 0.45MPa / ℃, 0.50MPa / ℃, 0.55MPa / ℃, 0.60MPa / ℃, 0.65MPa / ℃ and 0.70MPa / ℃; preferably 0.20MPa / ℃ to 0.60MPa / ℃; more preferably 0.25MPa / ℃ to 0.60MPa / ℃; and particularly preferably 0.35MPa / ℃ to 0.60MPa / ℃. It should be noted that when the analysis temperature is greater than 55℃, the physical properties of the polyvinyl alcohol film may change drastically due to the complete disappearance of crystallization. Therefore, when analyzing the absolute value of the slope value, the set analysis temperature interval should avoid exceeding 55℃.

[0033] In addition, regarding the analysis method of the absolute value of the slope value, since the polyvinyl alcohol film absorbs water (even moisture in the air) and affects its crystal state and molecular arrangement, before measuring the storage modulus (E') relative temperature curve of the polyvinyl alcohol film, the moisture content of each polyethylene film to be measured can be adjusted to be consistent through pre-treatment, so that the state to be measured of each polyethylene film is consistent. The moisture content can usually be adjusted to about 8 to 9wt%, but this is not limited to this in this article.

[0034] The "dissolution amount of polyvinyl alcohol" described herein refers to the phenomenon that polyvinyl alcohol will dissolve after the polyvinyl alcohol film is immersed in water; and, as the temperature of the water increases and the immersion time increases, the amount of polyvinyl alcohol dissolved will increase. The temperature of the dye bath in the dyeing tank is generally about 20 to 45°C, so when the polyvinyl alcohol film is dyed, polyvinyl alcohol will also dissolve. Without being limited by a specific theory, it is believed that the dissolution amount of polyvinyl alcohol is related to the amount of polyvinyl alcohol that can diffuse freely in the amorphous region within the polyvinyl alcohol film: the higher the dissolution amount of polyvinyl alcohol, the more polyvinyl alcohol that can diffuse freely, which means that the structure of the amorphous region within the polyvinyl alcohol film is loose and not tight, and relatively speaking, the dyeing solution is also easier to diffuse into the polyvinyl alcohol film through the loose structure and adsorb around the polyvinyl alcohol. The inventors have found that if the dissolution amount of polyvinyl alcohol is too high, the polyvinyl alcohol film will easily absorb too much dyeing liquid, causing the color of the subsequently prepared polarizing film to be too dark and the monomer transmittance to be too low; if the dissolution amount of polyvinyl alcohol is too low, the polyvinyl alcohol film will not be easy to stretch and dye, which will easily cause the monomer transmittance of the subsequently prepared polarizing film to be too low.

[0035] Therefore, in order to improve the monomer transmittance of the polarizing film made of the polyvinyl alcohol film, the dissolution amount of the polyvinyl alcohol needs to be controlled within a specific range; specifically, the polyvinyl alcohol dissolution amount of the polyvinyl alcohol film immersed in 40°C water for 1 minute is 0.20 to 9.00 ppm / m 2 , for example, the following values ​​or the range between any two of them: 0.20ppm / m 2 、1.00ppm / m 2 , 1.60ppm / m 2 , 2.40ppm / m 2 、3.20ppm / m 2 , 4.00ppm / m 2 , 4.80ppm / m 2 , 5.60ppm / m 2 、6.40ppm / m 2 、7.20ppm / m 2 、8.00ppm / m 2 and 9.00ppm / m 2 ; preferably 1.60ppm / m 2 Up to 7.20ppm / m 2 .

[0036] The "storage modulus (E') of the polyvinyl alcohol film at 45°C (hereinafter referred to as the storage modulus at 45°C)" described herein can characterize the degree of residual crystallization of the polyvinyl alcohol film in water at a temperature of 45°C. Without being limited by a specific theory, it is believed that the degree of dye adsorption in the dyeing step in the polarizing film manufacturing process is related to the storage modulus at 45°C. The inventors have found that the larger the storage modulus at 45°C, the higher the degree of residual crystallization of the polyvinyl alcohol film in water at 45°C, and therefore the lower the degree of dye adsorption, that is, the less the amount of dye adsorption. When the polyvinyl alcohol film adsorbs less dye, the amount of I-5 generated after stretching in the stretching tank is too low, resulting in the final polarizing film being more prone to red light leakage.

[0037] Therefore, controlling the storage modulus of the polyvinyl alcohol film at 45°C within a specific range can improve the red light leakage rate of the polarizing film obtained; specifically, the storage modulus (E') of the polyvinyl alcohol film at 45°C is 5.00 to 14.00 MPa, such as the following values ​​or the range between any two of them: 5.00 MPa, 5.50 MPa, 6.00 MPa, 6.50 MPa, 7.00 MPa, 7.50 MPa, 8.00 MPa, 8.50 MPa, 9.00 MPa, 9.50 MPa, 10.00 MPa, 10.50 MPa, 11.00 MPa, 11.50 MPa, 12.00 MPa, 12.50 MPa, 13.00 MPa, 13.50 MPa and 14.00 MPa; preferably 8.00 to 11.50 MPa.

[0038] The "storage modulus (E') of the polyvinyl alcohol film at 55°C (hereinafter referred to as the storage modulus at 55°C)" described in this article can characterize the degree of residual crystallization of the polyvinyl alcohol film in water at a temperature of 55°C. In the production of polarizing films, they are usually stretched at 55°C and immersed in a boric acid solution. Without being limited by a specific theory, it is believed that the degree of residual crystallization of the original film in the extension step in the polarizing film production process is related to the storage modulus at 55°C. The inventors have found that the larger the storage modulus at 55°C, the higher the residual degree of the original polyvinyl alcohol film, which results in less boric acid crosslinking. When the amount of boric acid crosslinking is less, the dye adsorbed by the polyvinyl alcohol film will be more easily washed away and lost, and the I generated after extension will be - The amount of 5 generated is too low, resulting in the final polarizing film being more prone to red light leakage.

[0039] Therefore, controlling the storage modulus of the polyvinyl alcohol film at 55°C within a specific range can improve the red light leakage rate of the polarizing film obtained; specifically, the storage modulus (E') of the polyvinyl alcohol film at 55°C is 3.00 to 7.00 MPa, such as the following values ​​or the range between any two of them: 3.00 MPa, 3.50 MPa, 4.00 MPa, 4.50 MPa, 5.00 MPa, 5.50 MPa, 6.00 MPa, 6.50 MPa and 7.00 MPa; preferably 4.00 to 6.00 MPa.

[0040] According to some preferred embodiments of the present invention, the polyvinyl alcohol film has a lower extension tension, which can reduce the situation of film breakage due to excessive extension tension when preparing a polarizing film; specifically, the polyvinyl alcohol film has an extension tension of 13.0 to 30.0 N / mm when immersed in a 2 wt.% boric acid aqueous solution at 50°C for 30 seconds. 2 , for example, the following values ​​or the range between any two of them: 13.0N / mm 2 , 15.0N / mm 2 、17.0N / mm 2 、19.0N / mm 2 , 21.0N / mm 2 , 23.0N / mm 2 , 25.0N / mm 2 , 27.0N / mm 2 , 29.0N / mm 2 and 30.0N / mm 2 .

[0041] The "average degree of polymerization" described herein is measured according to the JIS K 6726 (1994) standard test method. Without being limited by a particular theory, it is believed that the average degree of polymerization of the polyvinyl alcohol film is related to the size of the generated crystalline particles. The inventors have found that if the average degree of polymerization is too high, the polyvinyl alcohol chain segments are difficult to move due to their long length, resulting in a less uniform size of the generated crystalline particles, which in turn makes it difficult for the polyvinyl alcohol to dissolve; if the average degree of polymerization is too low, it is difficult to generate crystals, and the crystalline particles are also less uniform, which makes it easier for the polyvinyl alcohol to dissolve. Therefore, in order to form crystalline particles of uniform size, the average degree of polymerization of the polyvinyl alcohol film needs to be controlled within a specific range; specifically, the polyvinyl alcohol resin has an average degree of polymerization of 1500 to 3500, specifically, for example, the following values ​​or the range between any two thereof: 1500, 1700, 1900, 2100, 2300, 2500, 2700, 2900, 3100, 3300 and 3500.

[0042] The "Polymer Dispersity Index (PDI)" described herein is used to describe the molecular weight distribution of the polyvinyl alcohol resin, which is the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn). According to some preferred embodiments of the present invention, the polyvinyl alcohol resin has a polymer dispersity index of less than or equal to 3.5, for example less than or equal to 3.5, less than or equal to 3.3, less than or equal to 3.1, less than or equal to 2.9, less than or equal to 2.7, less than or equal to 2.5 or less than or equal to 2.3. Without being limited by a particular theory, the inventors have found that if the polymer dispersity index is too high, the polyvinyl alcohol film is more likely to have small molecules of polyvinyl alcohol dissolved, resulting in an excessively high amount of polyvinyl alcohol dissolved.

[0043] As mentioned above, the polyvinyl alcohol film of the present invention is a film obtained by processing and shaping a film-forming material containing a polyvinyl alcohol resin. During the film manufacturing, a plasticizer, a surfactant, or other known additives may be added as the film-forming material.

[0044] The polyvinyl alcohol resin used is obtained by polymerizing vinyl ester resin monomers to form a polyvinyl ester resin with an average degree of polymerization of 1500 to 3500 and a polymer dispersibility index of less than or equal to 3.5, and then undergoing a saponification reaction to obtain the polyvinyl alcohol resin. The vinyl ester monomers may be, for example, vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl octanoate, vinyl laurate, vinyl stearate, vinyl benzoate, trimethylacetic acid vinyl, 2,2,4,4-tetramethylvalerate vinyl, and tert-valerate vinyl, but the present invention is not limited thereto; for example, vinyl acetate. Among them, the vinyl ester polymer is preferably a polymer obtained by using one or more vinyl ester monomers as monomers; and a polymer obtained by using one vinyl ester monomer as a monomer is more preferred. In addition, the vinyl ester polymer may also be a copolymer of one or more vinyl ester monomers and other copolymerizable monomers.

[0045] The copolymerizable monomers may be, for example, olefin compounds having a carbon number of 3 to 30, such as ethylene, propylene, 1-butene, isobutylene, etc., and the addition amount thereof may be, for example, but not limited to, 2 to 4 mol%, such as 2.0, 2.5, 3.0, 3.5 or 4.0 mol%, etc.; acrylic acid or its salts; acrylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tertiary butyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, octadecyl acrylate, etc.; methacrylic acid or its salts; methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tertiary butyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, octadecyl methacrylate, etc.; acrylamide derivatives such as acrylamide, N-methylacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, diacetoneacrylamide, acrylamidepropanesulfonic acid or its salts, acrylamidepropyldimethylamine or its salts, N-hydroxymethylacrylamide or its derivatives; methacrylamide derivatives such as methacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, methacrylamidepropanesulfonic acid or its salts, methacrylamidepropyldimethylamine or its salts, N-hydroxymethylmethacrylamide or its derivatives; N-vinylamides such as N-vinylformamide, N-vinylacetamide, N-vinylpyrrolidone; methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether , tertiary butyl vinyl ether, dodecyl vinyl ether, stearyl vinyl ether and other vinyl ethers; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; maleic acid or its salts, esters or anhydrides; itaconic acid or its salts, esters or anhydrides; maleic acid and its salts or esters, vinyl silicon-based compounds such as vinyl trimethoxysilane, isopropynyl acetate, etc.; vinyl silicon-based compounds such as vinyl trimethoxysilane; isopropenyl acetate, etc. In addition, the vinyl ester polymer may have structural units derived from one or more of these copolymerizable monomers.

[0046] The basicity of the polyvinyl alcohol resin used is 95.00 mol% or more, wherein the basicity is a measured value obtained according to the JIS K 6726 (1994) standard test method. In one or more embodiments, the basicity is, for example, 95.00 mol% or more, 96.00 mol% or more, 97.00 mol% or more, 98.00 mol% or more, 99.00 mol% or more, or 99.50 mol% or more. Preferably, the basicity is 99.95 mol% or more, more preferably 99.97 mol% or more, for example, 99.97 mol% or more, 99.98 mol% or more, or 99.99 mol% or more.

[0047] According to some embodiments of the present invention, the "plasticizer" described herein may specifically be, but not limited to, glycerol, ethylene glycol, propylene glycol, diethylene glycol, diglycerol, triethylene glycol, tetraethylene glycol or trimethylolpropane, or a combination of any of the aforementioned plasticizers; glycerol is preferred in the present invention. In one or more embodiments, the amount of the plasticizer added relative to the weight of the polyvinyl alcohol resin is 5 to 15 wt.%, specifically, for example but not limited to 6 wt.%, 7 wt.%, 8 wt.%, 9 wt.%, 10 wt.%, 11 wt.%, 12 wt.%, 13 wt.%, 14 wt.% and 15 wt.%; in a preferred embodiment, the amount of the plasticizer added relative to the weight of the polyvinyl alcohol resin is 10 wt.%.

[0048] In addition to the above-mentioned plasticizers, other additives may be further added in the dissolution process as needed, including but not limited to surfactants, etc.; the surfactants include but are not limited to cationic, anionic or non-ionic surfactants, and specifically may be but are not limited to: carboxylate type such as potassium laurate, sulfate ester type such as sodium laureth sulfate, sulfonate type such as dodecylbenzenesulfonate, alkylphenyl ether type such as polyoxyethylene octylphenyl ether, alcohol phenyl ether type such as polyethylene glycol monooctylphenyl ether, alkyl ester type such as polyoxyethylene laurate, alkylamine type such as polyoxyethylene laurylamine ether, alkylamide type such as polyoxyethylene lauramide, polypropylene glycol ether type such as polyoxyethylene polyoxypropylene ether, lauric acid diethanolamide, oleyl diethanolamide, allylphenyl ether type such as polyoxyalkylene allylphenyl ether, or sodium lauryl alcohol polyoxyethylene ether sulfate, etc. The amount of the surfactant added is 600 to 3000 ppm relative to the weight of the polyvinyl alcohol resin, but is not limited thereto.

[0049] Furthermore, the polyvinyl alcohol film may further contain components such as a water-soluble polymer, a defoaming agent, an antioxidant, a UV absorber, a lubricant, other polymer compounds or a combination thereof, within a range not hindering the effects of the present invention.

[0050] [Method for producing polyvinyl alcohol film]

[0051] The method for manufacturing the polyvinyl alcohol film of the present invention generally comprises the following steps: (a) a dissolution process: heating and dissolving a film-forming material of a polyvinyl alcohol-based resin, and adjusting the concentration of the polyvinyl alcohol-based resin to form a polyvinyl alcohol casting solution; (b) a casting process: casting the polyvinyl alcohol casting solution onto a casting drum, and obtaining a polyvinyl alcohol preformed film after peeling off from the casting drum; (c) a hot roller process: contacting the polyvinyl alcohol preformed film with a plurality of hot rollers to obtain a polyvinyl alcohol preformed film; (d) a heat treatment process: placing the polyvinyl alcohol preformed film into a heat treatment device for heat treatment to obtain a polyvinyl alcohol semi-finished film; and (e) a temperature and humidity control process: placing the polyvinyl alcohol semi-finished film in a temperature and humidity control box to adjust the temperature and humidity to obtain a polyvinyl alcohol finished film.

[0052] <Dissolution Process>

[0053] According to some embodiments of the present invention, the dissolution process mainly comprises raising the temperature of a film-forming material such as a polyvinyl alcohol-based resin having a degree of polymerization of 1500 to 3500 and an average polymer dispersion index of less than or equal to 3.5, a solvent, a plasticizer, etc. to 140°C to 160°C, such as but not limited to 140°C, 150°C or 160°C, while stirring, and the dissolution time is 1 to 3 hours, such as 1 hour, 2 hours or 3 hours; after uniform dissolution, a polyvinyl alcohol aqueous solution is formed, and the concentration of the polyvinyl alcohol aqueous solution is adjusted to 25 to 35wt.%, such as but not limited to 25wt.%, 30wt.% or 35wt.%, to obtain a polyvinyl alcohol casting solution.

[0054] According to some embodiments of the present invention, the solvent used in the aforementioned dissolution process can be used as long as it can dissolve the polyvinyl alcohol resin, so it is not limited in the present invention. As the solvent, for example, but not limited to: water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylenediamine, diethylenetriamine, etc., the above solvents can be used alone or in combination of two or more. Considering the environment and economy, water is preferably used as the solvent in the present invention.

[0055] <Casting Process>

[0056] According to some embodiments of the present invention, the casting process mainly involves conveying the polyvinyl alcohol casting solution to an extruder for remixing and defoaming (for example, but not limited to, using a double-screw extruder for defoaming), and then discharging from a T-slit die lip and casting onto a rotating casting drum (or casting roller) to form a film, and the temperature of the casting drum is 88°C to 98°C, for example, but not limited to: 90°C, 93°C or 96°C, thereby obtaining a polyvinyl alcohol primary film. According to some embodiments of the present invention, in the casting process, the temperature of the polyvinyl alcohol casting solution after remixing and defoaming in an extruder must be controlled to be at least 90°C or above, for example, but not limited to: 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C or 98°C. According to other embodiments of the present invention, when the polyvinyl alcohol casting solution is cast onto the rotating casting drum, the temperature of the casting drum is preferably 85 to 95° C., and the polyvinyl alcohol stays on the casting drum for preferably 0.6 to 1.2 minutes.

[0057] <Hot Roller Process>

[0058] According to some embodiments of the present invention, the hot roller process mainly involves drying the upper and lower surfaces of the polyvinyl alcohol initially formed film after peeling off the casting drum through contact with multiple hot rollers to further obtain a polyvinyl alcohol initially finished film; wherein the temperatures of the multiple hot rollers (for example, 13 hot rollers) gradually decrease from high to low, and the starting hot roller is the hottest one among all the hot rollers, for example but not limited to 90°C to 99°C, and specifically may be for example but not limited to 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C or 99°C, preferably 95°C; the temperature of the final hot roller is the coldest one among all the hot rollers, for example but not limited to 30°C to 40°C.

[0059] <Heat Treatment Process>

[0060] According to some embodiments of the present invention, the heat treatment process mainly involves heating and drying the polyvinyl alcohol preliminary finished film in the film thickness direction after being peeled off from the self-heating roller by heat radiation, thereby obtaining a polyvinyl alcohol semi-finished film; wherein, the heat treatment preferably uses infrared rays, and the film surface temperature of the polyvinyl alcohol preliminary finished film during infrared heating is 80°C to 120°C, such as the following values ​​or the range between any two of them: 80°C, 90°C, 100°C, 110°C and 120°C, and the heating time is 25 to 35 seconds, such as the following values ​​or the range between any two of them: 25 seconds, 27 seconds, 29 seconds, 31 seconds, 33 seconds and 35 seconds. Without being limited by a specific theory, the inventors have found that if the film surface temperature of the polyvinyl alcohol pre-finished film is too high during heating, the size of the generated crystal particles will be larger and the crystal distribution will be uneven; if it is too low, the size of the crystal particles will be smaller or even difficult to form crystals, and the aforementioned two conditions will have a negative impact on the absolute value of the slope of the storage modulus relative temperature curve of the subsequently obtained polyvinyl alcohol film.

[0061] <Temperature and humidity control process>

[0062] According to some embodiments of the present invention, the polyvinyl alcohol semi-finished film is placed in a temperature and humidity control box for a specific time and its temperature and relative humidity are adjusted to facilitate recrystallization; wherein the temperature of the temperature and humidity control box can be controlled to be 60°C to 80°C, specifically for example, the following values ​​or the range between any two of them: 60°C, 70°C and 80°C; the relative humidity can be controlled to be 60% to 80%, specifically for example, the following values ​​or the range between any two of them: 60%, 70% and 80%; and the time can be controlled to be 3 to 8 minutes, specifically for example, the following values ​​or the range between any two of them: 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes and 8 minutes. Without being limited by a specific theory, the inventors have found that by increasing the temperature and relative humidity, the recrystallization and rearrangement of polyvinyl alcohol can be accelerated to improve the compactness of the structure in the polyvinyl alcohol film, affecting the absolute value of its slope value and the dissolution amount of the polyvinyl alcohol.

[0063] [Optical film and method for producing the same]

[0064] Another object of the present invention is to provide an optical film, which is made from the aforementioned polyvinyl alcohol film. The "optical film" mentioned herein can be a polarizing film, a phase difference film, a viewing angle enhancement film or a brightness enhancement film, etc., especially a polarizing film.

[0065] According to some embodiments of the present invention, the polarizing film has a monomer transmittance greater than or equal to 42.5%, for example greater than or equal to 42.5%, greater than or equal to 43.0% or greater than or equal to 43.5%; and has a red light leakage rate less than 5.0%, for example less than 5.0%, less than 4.5%, less than 4.0%, less than 3.5%, less than 3.0%, less than 2.5%, less than 2.0%, less than 1.5% or less than 1.0%.

[0066] According to some embodiments of the present invention, the "method for manufacturing an optical film" described herein refers to a method for manufacturing a polarizing film, and further refers to manufacturing a polyvinyl alcohol film into a polarizing film. The manufacturing method includes a dyeing step for adsorbing iodine ions, a boric acid treatment step, and a water washing step; a uniaxial stretching step can be performed in the boric acid treatment step or in a stage before the step. Preferably, a swelling step for swelling the polyvinyl alcohol film with water can be provided before the dyeing step. In addition, a final drying step is usually provided after the water washing step.

[0067] In the swelling step, the polyvinyl alcohol film is immersed in a treatment bath (e.g., pure water) at a temperature of, for example, 30° C. to 55° C. to wash the film surface and perform swelling treatment. The swelling treatment time is generally 5 to 300 seconds, preferably 20 to 240 seconds. According to some embodiments, a plurality of guide rollers are arranged in the swelling tank containing the treatment bath to transport the polyvinyl alcohol film. Next, the polyvinyl alcohol film is stretched in the machine direction (MD) to 1.05 to 2.5 times of the original length, and then the dyeing step is performed.

[0068] In the dyeing step, the polyvinyl alcohol film after the above-mentioned swelling step is immersed in a dyeing tank containing a dyeing bath. The conditions of the dyeing treatment can be determined based on the range within which the iodine is adsorbed on the polyvinyl alcohol film without causing adverse conditions such as extreme dissolution and devitrification of the film. The dyeing bath in the dyeing step is, for example, an aqueous solution containing iodine and potassium iodide. The concentration of iodine in the dyeing bath is preferably 0.01-0.5wt%, and the concentration of potassium iodide is preferably 0.01-10wt%. A specific example may be, but is not limited to, an aqueous solution of iodine with a concentration of 0.037wt% and potassium iodide with a concentration of 1.85wt%. In addition, other iodides such as zinc iodide can also be used instead of potassium iodide, or other iodides can be used in addition to potassium iodide. The temperature of the dyeing bath is usually set to 20 to 45°C, for example, it is carried out under the condition of 40°C, and the dyeing treatment time (dyeing time) is usually 10 to 600 seconds, preferably 30 to 200 seconds. Next, the polyvinyl alcohol film is stretched along a machine direction to 2 to 4 times of its original length, and then subjected to a boric acid treatment and a stretching step.

[0069] In the boric acid treatment and extension step, the iodine-dyed polyvinyl alcohol film is treated with an aqueous solution containing boric acid to make it cross-linked, and the adsorbed iodine is fixed in the resin. This step is usually carried out by immersing the polyvinyl alcohol film after the dyeing step in a fixing tank containing a treatment bath containing boric acid. The boric acid treatment bath preferably contains iodide in addition to boric acid. The iodide used can be potassium iodide or zinc iodide, for example, an aqueous solution containing boric acid and potassium iodide at a concentration of 5.5wt%. In addition, compounds other than iodide can also coexist in the boric acid treatment bath, such as zinc chloride, cobalt chloride, zirconium chloride, sodium thiosulfate, potassium sulfite, sodium sulfite, potassium sulfate, sodium sulfate, etc. The boric acid treatment and extension step is usually carried out at 50-70°C, for example, at 55°C, and the treatment time is usually 10-600 seconds, preferably 20-300 seconds, and more preferably 20-100 seconds. Next, the polyvinyl alcohol film is stretched along the mechanical direction to more than 3 times of its original length before proceeding to subsequent steps; the upper limit of the stretching ratio is not particularly limited, but is preferably less than 8 times, for example, stretched to include but not limited to 3.3 times or more, such as 3.3 to 8.0 times, more preferably 3.5 to 6.0 times, and particularly preferably 4.0 to 5.5 times.

[0070] After the polyvinyl alcohol film is subjected to the above steps and the subsequent washing and drying steps, a polarizing film is formed. In the washing and drying steps, the iodine solution and boric acid remaining on the film surface are washed with water or an aqueous solution containing iodide, for example, but not limited to, a potassium iodide aqueous solution with a concentration of 5.5wt% is used for washing. Then, a drying step is performed, for example, but not limited to, drying in an oven at a temperature of 60°C for 5 minutes, to form a polarizing film.

[0071] Furthermore, the polarizing film includes a protective layer attached to at least one side of the polarizing film. The protective layer is preferably a component having functions such as preventing the surface of the polarizing film from being worn. According to different embodiments, the protective layer can be disposed on only one side of the polarizing film, or on both sides of the polarizing film. The protective layer can be a protective film of a transparent resin material; the transparent resin can be an acrylic resin such as methyl methacrylate resin, an olefin resin, a polyvinyl chloride resin, a cellulose resin, a styrene resin, an acrylonitrile-butadiene-styrene copolymer resin, an acrylonitrile-styrene copolymer resin, a polyvinyl acetate resin, a polyvinylidene chloride resin, a polyamide resin, a polyacetal resin, a polycarbonate resin, a modified polyphenylene ether resin, a polyester resin (polybutylene terephthalate resin, polyethylene terephthalate resin, etc.), a polysulfone resin, a polyethersulfone resin, a polyarylate resin, a polyamide-imide resin, a polyimide resin, an epoxy resin, an oxetane resin, etc.; preferably, a cellulose resin is used, for example, triacetate cellulose (TAC).

[0072] Example

[0073] Hereinafter, the present invention will be further described with detailed description and specific examples. However, it should be understood that these specific examples are only used to help the present invention to be more easily understood and are not used to limit the scope of the present invention.

[0074] 1. Preparation of polyvinyl alcohol film

[0075] Herein, the present invention provides a non-limiting method for preparing polyvinyl alcohol films. According to a method similar to the method disclosed below, non-limiting example polyvinyl alcohol films (Examples 1 to 11) and comparative example polyvinyl alcohol films (Comparative Examples 1 to 6) were prepared.

[0076] The following are the main steps common to the present embodiment and the comparative example in manufacturing the polyvinyl alcohol film, and the following Table 1 will show in detail the differences in one or more process parameters between the present embodiment and the comparative example: Dissolution process: First, add 1800 kg of polyvinyl alcohol resin with a specific average degree of polymerization and polymer dispersibility index (the specific average degree of polymerization and polymer dispersibility index are shown in Table 1), 4000 kg of water, and 180 kg of glycerol into a dissolution tank, raise the dissolution temperature to 150° C. while stirring and dissolve for 2 hours, and adjust the concentration of the polyvinyl alcohol aqueous solution to 30 wt.% after the dissolution is uniform to obtain a polyvinyl alcohol casting solution. The polyvinyl alcohol resin in the embodiment and the comparative example is a polyvinyl alcohol resin polymerized from vinyl acetate and unmodified (i.e., not containing other comonomers) and having a basicity of 99.95 mol%. Casting process: The polyvinyl alcohol casting solution is transported to the extruder for mixing and defoaming again, and the temperature of the polyvinyl alcohol casting solution is controlled at 98°C. It is then extruded from the T-slit die lip and cast onto a rotating casting drum to form a film. The temperature of the casting drum is 96°C, thereby forming a polyvinyl alcohol primary film. Hot roller process: After the polyvinyl alcohol preformed film is peeled off from the casting drum, the upper and lower surfaces of the polyvinyl alcohol preformed film are contact dried by 13 hot rollers with the temperature decreasing gradually; among them, the first hot roller is the hottest one among all the hot rollers, which is 95°C; the 13th hot roller is the coldest one among all the hot rollers, which is 30°C, to obtain the polyvinyl alcohol preformed film. Heat treatment process: Then, the polyvinyl alcohol pre-finished film was dried by infrared heating for 30 seconds, and the film surface temperature during infrared heating was controlled within a specific range (the specific film surface temperature during heating is shown in Table 1) to obtain a polyvinyl alcohol semi-finished film. Temperature and humidity control process: Subsequently, the semi-finished polyvinyl alcohol film is placed in a temperature and humidity control box for recrystallization at a specific temperature and relative humidity for a specific time (the specific temperature, relative humidity and time are shown in Table 1) to obtain a polyvinyl alcohol finished film, and the polyvinyl alcohol finished film has a specific thickness (the specific thickness is shown in Table 1).

[0077] Table 1

[0078] 2. Preparation of polarizing film

[0079] Here, the present invention provides a non-limiting method for preparing a polarizing film from a polyvinyl alcohol film. According to the method disclosed below, non-limiting example polyvinyl alcohol films (Examples 1 to 11) and comparative example polyvinyl alcohol films (Comparative Examples 1 to 6) were prepared into corresponding polarizing films.

[0080] The following are the main steps for preparing polarizers from the polyvinyl alcohol film of the embodiment of the present invention and the comparative example: after unwinding the polyvinyl alcohol film, let it enter the swelling tank filled with 30°C pure water to wash and swell the film surface; after the polyvinyl alcohol film is stretched to 1.2 times of the original length in the mechanical direction, it then enters the dyeing tank controlled at 45°C and containing an aqueous solution of 0.037wt.% iodine and 1.85wt.% potassium iodide for dyeing, and at the same time, the polyvinyl alcohol film is extended to 3.4 times of the original length in the mechanical direction; after dyeing, it enters the extension tank controlled at 55°C and containing an aqueous solution of 5.5wt.% boric acid and potassium iodide, and after the polyvinyl alcohol film is extended to 6 times of the original length in the mechanical direction, the iodine solution and boric acid remaining on the film surface are washed with an aqueous solution containing 5.5wt.% potassium iodide. Then, it is dried in a 60°C oven for 5 minutes, and the upper and lower surfaces are bonded with triacetyl cellulose protective films and dried to form a polarizing film.

[0081] 3. Analytical methods

[0082] Here, the present invention provides analysis and testing methods for the polyvinyl alcohol films of Examples 1 to 11 and Comparative Examples 1 to 6.

[0083] Average degree of polymerization

[0084] The method for measuring the average degree of polymerization in the present invention is based on the JIS K 6726 (1994) standard method.

[0085] Polymer Dispersibility Index (PDI)

[0086] Gel Permeation Chromatography (GPC) was used to measure the peak molecular weight and polymer dispersibility index of the polyvinyl alcohol resin.

[0087] Instrument and brand: (1) Waters 515 HPLC pump; (2) Waters 717plus autosampler; (3) Waters 2414 refractive index detector, detection temperature is 36°C; (4)Analytical column: Waters' Ultrahydrogel Guard Column, 6μm,6mm*40mm,1K-500K, Waters Ultrahydrogel 120 Column, 6μm,7.8mm*300mm,100-5K, Waters Ultrahydrogel 250 Column, 6μm,7.8mm*300mm,1K-80K, Waters Ultrahydrogel 500 Column, 10μm,7.8mm*300mm,5K-400K, Waters Ultrahydrogel 1000 Column, 12μm,7.8mm*300mm,10K-1M.

[0088] Test conditions: (1) Analytical flow rate: 0.413 mL / min; (2) Running liquid: 0.85wt.% sodium nitrate aqueous solution; (3) Column oven temperature: 36°C; (4) Standard: polyethylene glycol (PEG), peak molecular weight (Mp) = 1608000 / 1039000 / 545000 / 117900 / 66200 / 28330 / 16100 / 3860 / 1450 / 610 / 194; (5) Analysis sample configuration: 0.08 g of the polyvinyl alcohol resin to be measured, 17 g of a 0.85 wt.% sodium nitrate aqueous solution, and a 0.45 μm PTFE syringe filter; (6) Injection volume: 210 μL; (7) Test time: 106 minutes.

[0089] Data processing: The weight average molecular weight (Mw) and number average molecular weight (Mn) of the polyvinyl alcohol resin were calculated, and the polymer dispersibility index (PDI) was calculated according to the following formula: PDI = Mw / Mn.

[0090] Storage modulus (E'), and the absolute value of the slope of its curve versus temperature

[0091] Instrument and brand: TA Instruments DMA 850

[0092] Sample preparation method: Cut the polyvinyl alcohol film into a rectangle with a length of 5 cm in the machine direction (MD) and 5 mm in the width direction (TD). Before loading the film, adjust the moisture content of the polyvinyl alcohol film to 8 to 9 wt.% to make the polyvinyl alcohol film uniform. Figure 2 , clamp one end of the polyvinyl alcohol film 2 with a dovetail clip 3 weighing about 1.11g, and insert the other end into the immersion stretching fixture 1, so that a part of the polyvinyl alcohol film 2 is placed between the fixed axis 1a and the lower fixed axis 1b, so that the lower end 3a of the dovetail clip 3 is 1cm away from the immersion stretching fixture 1 ( Figure 2 The distance a) shown in FIG. 1 is a distance between the upper end 2a of the polyvinyl alcohol film 2 and the upper end of the immersion stretching fixture 1, and a reserved space is provided; then, the upper fixing shaft 1a is locked to fix the polyvinyl alcohol film 2. Next, refer to Figure 3 , vertically place the entire immersion stretching fixture 1 together with the polyvinyl alcohol film 2 and dovetail clamp 3 held by it into a 100mL beaker 4 filled with pure water so that the liquid level of the beaker is located on the upper fixed axis, and control the temperature of the beaker 4 in a 30℃ constant temperature water tank (not shown in the figure) to allow the polyvinyl alcohol film 2 to swell under a load (the weight of the dovetail clamp 3) for 20 minutes. Finally, refer to Figure 4 , take out the immersion and stretching fixture 1 from the beaker 4 and keep it upright, use the weight of the dovetail clamp 3 to stretch the polyvinyl alcohol film 2, and after ensuring that the polyvinyl alcohol film 2 is centered, lock the lower fixed axis 1b of the immersion and stretching fixture 1, and then remove the excess polyvinyl alcohol film 2c (i.e. Figure 4 The grid-like part in the middle is cut off, and the sample is the polyvinyl alcohol film 2b that is swollen under load and clamped in the immersion and stretching fixture 1.

[0093] Test conditions: The upper sample is still fixed in the immersion and stretching fixture, and the oscillation heating mode is selected. The sample and the immersion and stretching fixture holding it are placed in an immersion tank filled with deionized water. The frequency is set to 1Hz, the amplitude is set to 200μm, the holding pressure (force track) is set to 200%, and the temperature is set to measure from 30℃ to 65℃. Before the analysis, the film is stretched with a static force of 0.15N before starting the analysis at a heating rate of 1℃ / min and drawing a curve of the storage modulus (E') relative to the temperature change. Among them, the thermocouple sensing end is placed at a height of 5mm from the bottom of the water tank.

[0094] Data processing: Change the coordinate axis of the storage modulus (E') to a linear coordinate axis, use the slope analysis built into the software included with the instrument, set the analysis temperature range to 45°C to 55°C, the software will automatically calculate the slope value, and then take the absolute value of the slope value.

[0095] Storage modulus (E') at 45°C and 55°C: The storage modulus (E') versus temperature curve on the aforementioned linear coordinate axis, the values ​​of the storage modulus (E') are obtained at 45°C and 55°C.

[0096] Dissolution of polyvinyl alcohol

[0097] Test drug configuration: (1) Boric acid solution: Weigh 20.00 g of boric acid into a 500 mL transparent quantitative bottle, first dissolve it with a small amount of deionized water (DI water), and then add deionized water to the 500 mL horizontal scale line. (2) Iodine solution: Weigh 1.27 g of solid iodine and 2.50 g of potassium iodide into a 100 mL brown quantitative bottle, first dissolve them with a small amount of deionized water (DI water), and then add deionized water to the 100 mL horizontal scale line.

[0098] Preparation of calibration curve: PVA resin with an average degree of polymerization of 2400, a basicity of 99.90 mol% and a polymer dispersibility index of 2.2 was dried at 105°C for 3 hours until absolutely dry, and then PVA resin standards with concentrations of 100ppm, 50ppm, 25ppm, 12.5ppm, 6.25ppm, 3.125ppm, 1.5625ppm and 0.78125ppm were prepared, and the absorbance at 670nm was analyzed to establish the calibration curve. 20g of the standard was placed in a frosted serum bottle, and 15mL of boric acid solution, 3mL of iodine solution and 12mL of deionized water were added in sequence, shaken to mix evenly and then left for 15 minutes.

[0099] Test conditions: 1L of deionized water is placed in a serum bottle, and the serum bottle is placed in a constant temperature water bath at 40°C. Cut the polyvinyl alcohol film into 20 test pieces with a length of 5cm in the machine direction (MD) and 5cm in the width direction (TD). Each test piece is immersed in the deionized water in the serum bottle, and taken out after immersion for 1 minute. A total of 20 test pieces are immersed continuously. Then the serum bottle is taken out from the constant temperature bath, cooled to 25°C, and the weight of the solution in the serum bottle is recorded. Weigh 20g of the solution in the serum bottle, place it in a frosted serum bottle, add 15mL of boric acid solution, 3mL of iodine solution and 12mL of deionized water in sequence, shake it to mix it evenly and place it for 15 minutes; then, use an ultraviolet-visible spectroscopy (UV-vis) to analyze the absorbance of the solution at 670nm, and bring the obtained result into the calibration curve to back-calculate the concentration to obtain the dissolution amount of polyvinyl alcohol.

[0100] Thickness of polyvinyl alcohol film

[0101] Instrument and brand: Mitutoyo 543-391B

[0102] Test method: Before analysis, confirm that the scale of the contact test probe on the platform is 0, then place the polyvinyl alcohol film to be tested flat on the platform, pull up the probe and gently place it on the polyvinyl alcohol film to read the thickness value.

[0103] 4. Evaluation methods and results

[0104] Here, the present invention provides evaluation methods for polyvinyl alcohol films and polarizing films of embodiments and comparative examples, and corresponding results thereof with the above-mentioned analysis contents.

[0105] Extension tension evaluation

[0106] Instrument and brand: Hongda tensile testing machine HT-9102

[0107] Sample preparation method: polyvinyl alcohol film was cut into rectangular test pieces with a length of 150 mm in the machine direction (MD) and 12.7 mm in the width direction (TD). The test pieces were placed in an environment with a temperature of 23°C and a relative humidity of 50% for 20 hours, and then immersed in a 2wt.% boric acid aqueous solution at a temperature of 50°C for 30 seconds, and immediately tested on the machine after immersion.

[0108] Test conditions: Fix the fixture spacing at 5cm, control the tension speed at 240mm / min, input the sample thickness and its length in the mechanical direction and width direction into the computer, and the system will automatically convert the extension tension.

[0109] Film breaking evaluation

[0110] Test conditions: 10000 m of polyvinyl alcohol film was used continuously to produce polarizing film.

[0111] Evaluation criteria: ○: No cracking occurred during the process ╳: There are more than 1 ruptures in the process

[0112] Single transmittance

[0113] Instrument and brand: JASCO spectrophotometer V-7100

[0114] Sample preparation method: Cut two square samples with a length of 2 cm in the machine direction (MD) and 2 cm in the width direction (TD) from the middle of the polarizing film width.

[0115] Test conditions: Use V-7100 spectrophotometer with integrating sphere to calibrate the visual sensitivity in the visible light field with C light source and 2° field of view according to JIS Z8722 (2009) standard method. Figure 5 As shown, overlapping samples are taken, where the machine direction MD1 of one sample is perpendicular to the machine direction MD2 of the other sample. Figure 6 As shown in A, rotate one sample clockwise so that the angle A between the mechanical directions MD1 and MD2 of the two samples is +45°, and measure the transmittance T1 of light at a wavelength of 550nm; Figure 6 As shown in B, one of the samples is rotated counterclockwise so that the angle B between the machine directions MD1 and MD2 of the two samples is -45°, and the transmittance T2 of light at a wavelength of 550nm is measured. Then the single transmittance Ts (%) = (Ts1 + Ts2) / 2 is obtained according to the following formula.

[0116] Red light leakage rate

[0117] Instrument and brand: JASCO spectrophotometer V-7100

[0118] Sample preparation method: Take the polarizing film 5 cm away from the left edge in the full width direction (such as Figure 7 The distance x shown in the figure), the middle, and 5 cm from the right side (as shown in the figure Figure 7 The distance x shown in FIG is 2 , and two square samples with a length of 2 cm in the machine direction (MD) and a length of 2 mm in the width direction (TD) are cut at each of the three positions (as shown in FIG. Figure 7 shown).

[0119] Test conditions:

[0120] Single-unit transmittance Ts (%): Based on the above-mentioned single-unit transmittance method, the single-unit transmittance Ts (%) at three positions, namely, the left side, the middle, and the right side, is detected.

[0121] Transmittance T700⊥(%): Take two samples at the same position and overlap them, such as Figure 5 As shown, the machine direction MD1 of one sample is perpendicular to the machine direction MD2 of the other sample. Figure 6 As shown in A, one of the samples is rotated clockwise so that the angle A between the mechanical directions MD1 and MD2 of the two samples is 45°, and the transmittance T of light at a wavelength of 700nm is measured. 45 ;like Figure 6 As shown in B, one of the samples is rotated counterclockwise so that the angle B between the mechanical directions MD1 and MD2 of the two samples is 45°, and the transmittance T- 45 . Take T 45 With T -45 The average value of is taken as the transmittance T700⊥(%) at that position.

[0122] Red light leakage rate: With the single transmittance Ts (%) as the horizontal axis and the transmittance T700⊥ (%) as the vertical axis, the analysis values ​​of the three positions are approximated as a straight line, and the transmittance T700⊥ (%) when the single transmittance Ts is 44% is obtained from the approximate straight line (that is, the orthogonal transmittance of light with a wavelength of 700nm), which is the red light leakage rate.

[0123] Evaluation criteria: Red light leakage rate less than 5% is preferred.

[0124] Furthermore, the results of the extension tension evaluation and film breaking evaluation of the polyvinyl alcohol films of Examples 1 to 11 of the present invention and Comparative Examples 1 to 6 and the monomer transmittance and red light leakage rate of the corresponding polarizing films are presented in Table 2 together with the absolute value of the slope value of the curve of the storage modulus of the polyvinyl alcohol film relative to temperature (referred to as the absolute value of the slope value in Table 2) and the dissolution amount of polyvinyl alcohol.

[0125] Table 2

[0126] According to Table 2, the absolute values ​​of the slope values ​​of the polyvinyl alcohol films of Examples 1 to 11 are all within the range of 0.20 to 0.70 MPa / °C, and the dissolution amounts of polyvinyl alcohol are all within the range of 0.20 to 9.00 ppm / m 2 In the range of 13.0 to 30.0 N / mm, it was observed that the polyvinyl alcohol films all had a relatively small extension tension of 13.0 to 30.0 N / mm. 2and good film breaking evaluation; and the polarizing films prepared from these polyvinyl alcohol films all have a high monomer transmittance greater than or equal to 42.5% and a low red light leakage rate less than 5.0%. On the contrary, if the polyvinyl alcohol films of Comparative Examples 1 to 6 do not have the absolute value of the slope value and the dissolution amount of polyvinyl alcohol in the ideal range at the same time, then these polyvinyl alcohol films and their corresponding polarizing films cannot have the above-mentioned technical effects at the same time. In view of this, only by simultaneously controlling the absolute value of the slope value of the polyvinyl alcohol film and the dissolution amount of polyvinyl alcohol within the ideal range can the problem of the polyvinyl alcohol film being easy to break during stretching due to excessive extension tension, as well as the problem of low monomer transmittance and high red light leakage rate of the polarizing film prepared therefrom, be improved.

[0127] Furthermore, the results of the red light leakage rate of the polarizing films corresponding to the polyvinyl alcohol films of Examples 1 to 11 and Comparative Examples 1 to 6 are presented in Table 3 together with the storage modulus at 45° C. and the storage modulus at 55° C. of the polyvinyl alcohol films.

[0128] Table 3

[0129] According to Table 3, when the storage modulus at 45°C of the polyvinyl alcohol film is controlled to be 5.00 to 14.00 MPa, and the storage modulus at 55°C is controlled to be 3.00 to 7.00 MPa, the polarizing film prepared from the polyvinyl alcohol film has a low red light leakage rate of less than 5.0%, such as Examples 1 to 11 and Comparative Examples 1, 3, 4 and 6. On the contrary, when the storage modulus at 45°C and the storage modulus at 55°C of the polyvinyl alcohol film are not controlled to be within the ideal range, the polarizing film prepared from the polyvinyl alcohol film has a high red light leakage rate, such as Comparative Examples 2 and 5. In view of this, when the storage modulus at 45°C and the storage modulus at 55°C of the polyvinyl alcohol film are controlled to be within the ideal range, the problem of high red light leakage rate of the polarizing film prepared from the polyvinyl alcohol film can be improved.

[0130] Herein, all ranges provided are intended to include each specific range within a given range and combinations of subranges between the given ranges. In addition, unless otherwise stated, all ranges provided herein include the endpoints of the ranges. Thus, ranges 1 to 5 specifically include 1, 2, 3, 4, and 5, as well as subranges such as 2 to 5, 3 to 5, 2 to 3, 2 to 4, 1 to 4, etc.

[0131] All publications and patent applications cited in this specification are incorporated herein by reference, and each individual publication or patent application is specifically and individually indicated to be incorporated herein by reference for any and all purposes. In the event of any inconsistency between this document and any publication or patent application incorporated herein by reference, this document controls.

Explanation of symbols

[0132] 1: Immersion tensile fixture 1a: Upper fixed axis 1b: Lower fixed axis 2: Polyvinyl alcohol film 2a: Top 2b: Polyvinyl alcohol film swollen under load 2c: Excess polyvinyl alcohol film 3: Dovetail clamp 3a: Bottom 4: Beaker a, x: distance A, B: Angle MD1, MD2: Mechanical direction

Claims

1. A polyvinyl alcohol film, comprising: Polyvinyl alcohol resin; The polyvinyl alcohol film is immersed in 40°C water for 1 minute and has a polyvinyl alcohol dissolution amount of 0.20 to 9.00 ppm / m 2 ;and The storage modulus (E') versus temperature curve of the polyvinyl alcohol film is measured when the temperature is increased from 30°C to 65°C in water at a heating rate of 1°C / min. The curve has a slope value in the range of 45°C to 55°C, and the absolute value of the slope value is 0.20 to 0.70 MPa / °C.

2. The polyvinyl alcohol film according to claim 1, wherein The dissolution amount of the polyvinyl alcohol is 1.60 to 7.20 ppm / m 2 ; and the absolute value of the slope value is 0.20 to 0.60 MPa / ℃.

3. The polyvinyl alcohol film according to claim 2, wherein The absolute value of the slope is 0.25 to 0.60 MPa / °C.

4. The polyvinyl alcohol film according to claim 3, wherein The absolute value of the slope is 0.35 to 0.55 MPa / °C.

5. The polyvinyl alcohol film according to claim 1, wherein The polyvinyl alcohol film has a storage modulus (E') of 5.00 to 14.00 MPa at 45°C; and the polyvinyl alcohol film has a storage modulus (E') of 3.00 to 7.00 MPa at 55°C.

6. The polyvinyl alcohol film according to claim 2, wherein The polyvinyl alcohol film has a storage modulus (E') of 8.00 to 11.50 MPa at 45°C; and the polyvinyl alcohol film has a storage modulus (E') of 4.00 to 6.00 MPa at 55°C.

7. The polyvinyl alcohol film according to any one of claims 1 to 6, which has an extension tension of 13.0 to 30.0 N / mm when immersed in a 2 wt.% boric acid aqueous solution at 50°C for 30 seconds. 2 .

8. The polyvinyl alcohol film according to any one of claims 1 to 6, wherein The polyvinyl alcohol resin has an average degree of polymerization of 1,500 to 3,500.

9. The polyvinyl alcohol film according to any one of claims 1 to 6, wherein The polyvinyl alcohol resin has a polymer dispersity index (PDI) of less than or equal to 3.

5.

10. The polyvinyl alcohol film according to any one of claims 1 to 6, which has a thickness of 45 to 75 μm.

11. An optical film, which is made from the polyvinyl alcohol film according to any one of claims 1 to 10.

12. The optical film according to claim 11, which is a polarizing film. 13 . The optical film of claim 12 , wherein the polarizing film has a single body transmittance greater than or equal to 42.5% and a red light leakage rate less than 5.0%.

Citation Information

Patent Citations

  • Polyvinyl alcohol film, optical film containing same and preparation method thereof

    CN115947960A

  • Optical resin film and polarizing film and liquid crystal display device using the same

    CN1916667A

  • Recording material

    JP1985245586A

  • Vinyl alcohol-based polymer film

    JP2009221462A

  • Polyvinyl alcohol film and method for producing polarizing film

    JP2022033365A