Plastic material with low expansion coefficient and high impact strength as well as preparation method and application thereof
A near-zero coefficient of thermal expansion and high impact strength plastic material prepared through specific components and processes solves the problems of dimensional instability and insufficient strength of existing materials under high and low temperature cycling, and is suitable for plastic parts of high-power charging piles.
Patent Information
- Application Number
- CN202410885551.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-26
AI Technical Summary
Existing plastic materials with low linear expansion coefficients exhibit poor dimensional stability under high and low temperature cycling and insufficient impact strength, failing to meet the requirements for high-power fast charging piles.
A plastic material with near-zero expansion coefficient and high impact strength is prepared by combining coupling agents, antioxidants, lubricants, reinforcing materials and heat-shrinkable fillers (such as Hf2W3O12 whiskers) with resin through a specific process, and the material properties are improved by electron beam irradiation and annealing treatment.
It has a stable near-zero coefficient of thermal expansion and an impact strength of up to 45KJ/m2 within a temperature range of -30℃ to 150℃, making it suitable for plastic parts of high-power charging piles and improving the dimensional stability and strength of the material.
Smart Images

Figure BDA0004925951610000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy vehicle charging piles, and in particular to a plastic material with a low expansion coefficient and high impact strength, and a preparation method and use thereof. Background Art
[0002] Energy is increasingly scarce today. Electric vehicles have broad market prospects due to their advantages of low energy consumption, low noise, low carbon emissions, and high safety. Therefore, electric vehicle charging stations - charging piles have also been vigorously promoted. Since charging piles are high-power energy conversion devices, a large amount of heat will be generated inside the charging piles during charging. Therefore, it is necessary to consider the dimensional stability of each plastic component in the charging pile under high and low temperature cycle conditions. If the dimensional change is too large, it will cause excessive temperature drift and damage to the electrical components inside the charging pile, thereby reducing the working efficiency and service life of the charging pile. In addition, when using existing charging piles, some drivers may not be proficient in driving skills, resulting in accidents where the rear of the car collides with the front side wall of the charging pile when reversing, which not only damages the charging pile, but also causes safety hazards such as fire. Therefore, providing a plastic material with a near-zero expansion coefficient and high impact strength for charging piles is one of the technical problems that technicians in this field need to solve.
[0003] In the prior art, for example, Chinese patent (CN116120747A) discloses a thermally conductive ultra-low linear expansion coefficient PPS composite material for plastic cavity filters and a preparation method thereof. Although the linear expansion coefficient of the prepared PPS composite material is relatively low between -30 and 150°C (the minimum is 14 μm / m·°C), the notched impact strength of this material is also low (only 6 to 11 kJ / m 2 ). Chinese patent (CN115594917A) discloses a low linear expansion coefficient polypropylene composite material and its preparation method. The prepared polypropylene composite material has a relatively high notched impact strength at -30 to 80°C (about 18 to 40 kJ / m 2 ), but the linear expansion coefficient of this polypropylene composite material is also high (minimum 25μm / m·℃) (high linear expansion coefficient). In summary, the current research and development of low linear expansion coefficient plastic materials still cannot fully meet the actual use requirements of low expansion coefficient and high impact strength of high-power fast charging piles. Therefore, it is very necessary to provide a low expansion coefficient and high impact strength plastic material. Summary of the invention
[0004] The purpose of the present invention is to solve the problem that the current low linear expansion coefficient plastic still cannot have both low expansion coefficient and high impact strength. The present invention provides a new plastic material with the characteristics of near-zero expansion coefficient and high impact strength, which solves the above problem.
[0005] To achieve the above object, the present invention is implemented by the following technical solutions:
[0006] The invention provides a plastic material with low expansion coefficient and high impact strength. The plastic material comprises the following components in weight fractions: 0.1-0.5wt% of coupling agent, 0.1-0.5wt% of antioxidant, 0.1-0.5wt% of lubricant, 2.0-5.0wt% of reinforcing material, 30.0-50.0wt% of heat shrink filler and resin remainder.
[0007] The material of the present invention is a plastic material with a near-zero thermal expansion coefficient and high impact strength, which can solve the problems of high thermal expansion coefficient, large dimensional change at high temperature and low impact strength of existing plastic materials used in charging piles.
[0008] Furthermore, a plastic material with low expansion coefficient and high impact strength: the coupling agent is selected from at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570; the antioxidant is selected from at least one of sodium sulfate, sodium pyrosulfite, sodium bisulfate, and sodium thiosulfate; the lubricant is selected from natural paraffin and / or graphite.
[0009] Preferably, the coupling agent is a mixture of three coupling agents: silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570, and the three are mixed in a weight ratio of 1:1:1.
[0010] Preferably, the antioxidant is a mixture of sodium sulfate, sodium metabisulfite, sodium bisulfate and sodium thiosulfate in a weight ratio of 1:1:1:1.
[0011] Preferably, the lubricant is a mixture of natural paraffin and graphite, which are mixed in a ratio of 1:1 by mass.
[0012] Furthermore, a plastic material with low expansion coefficient and high impact strength: the reinforcing material is short-cut silk, and the length of the short-cut silk is 200-500 μm and the diameter is 13-20 nm.
[0013] Further, a plastic material with low expansion coefficient and high impact strength: the heat shrink filler is selected from Hf2W3O with a diameter of 20 to 50 nm. 12 Whiskers have a large negative thermal expansion coefficient.
[0014] Furthermore, a plastic material with low expansion coefficient and high impact strength: the Hf2W3O 12 The method for preparing whiskers comprises the following steps:
[0015] S1, refining and degumming silk to obtain silk fibroin fibers;
[0016] S2, immersing the silk fiber in a mixed solution containing HfCl4 and WCl4, and then drying and calcining to obtain Hf2W3O4 having a negative thermal expansion coefficient. 12 Whiskers.
[0017] Furthermore, a plastic material with low expansion coefficient and high impact strength: the Hf2W3O 12 The method for preparing whiskers comprises the following specific steps:
[0018] S1, soaking the silk in hot water at 120-150° C. and ultrasonically vibrating for 24-48 hours to perform refining and degumming to obtain silk fibroin fibers;
[0019] S2, immersing the silk fiber in a mixed solution containing HfCl4 and WCl4 for 5 to 10 minutes, and then drying at 80 to 100°C for 8 to 24 hours, and then placing it in a vacuum furnace and passing high-purity oxygen at 1000 to 1200°C for 2 to 4 hours, thereby preparing Hf2W3O with a negative thermal expansion coefficient 12 Whiskers; wherein: the mixed solution contains 1.0 to 10.0 wt% HfCl4 and 1.0 to 10.0 wt% WCl4.
[0020] Furthermore, a plastic material with low expansion coefficient and high impact strength: the resin includes PC resin and PMMA resin, and the weight ratio of the PC resin to the PMMA resin is (3-5): (1-2).
[0021] Specifically, the melt flow rate of the PC resin selected in the present invention has a melt index of 10 to 25 g / 10 min when tested at 300° C. / 1.2 Kg; the melt flow rate of the PMMA resin selected has a melt index of 6 to 12 g / 10 min when tested at 300° C. / 1.2 Kg.
[0022] The present invention also provides a method for preparing a plastic material with low expansion coefficient and high impact strength. The method comprises the following steps:
[0023] S1. Mix the components of the plastic material uniformly according to the proportion;
[0024] Specifically, the components are mixed uniformly in a low-speed mixer at room temperature, the stirring time is set to 30 to 60 minutes, and the stirring speed is set to 10 to 20 revolutions per minute;
[0025] S2, blending and granulating the mixed materials through an extruder to obtain the plastic material.
[0026] Among them: the aspect ratio of the extruder is 44:1, the screw diameter is 36mm; the extrusion process is set as: temperature 200-220°C, main engine speed 300-400rpm, and the extruded strips are cooled and granulated through a water tank.
[0027] The present invention also provides a use of a plastic material with a low expansion coefficient and high impact strength: the above-mentioned plastic material can be used to manufacture plastic parts for charging piles, and the manufacturing method thereof comprises the following steps:
[0028] S1. Plasticizing, injection-filling, and pressure-maintaining the plastic material to obtain a preformed plastic component for a charging pile;
[0029] S2, irradiating the preform with an electron beam;
[0030] S3. Annealing the irradiated preform to obtain plastic parts for charging piles.
[0031] Further, a use of a plastic material with a low expansion coefficient and high impact strength: the manufacturing method of the plastic parts for the charging pile comprises the following specific steps:
[0032] S1. Plasticizing, injection-filling, and pressure-maintaining the plastic material using an injection molding machine to obtain a preformed plastic component for a charging pile;
[0033] Among them: the plasticizing temperature is 240-285°C, the injection pressure is set to 80-130MPa, the injection time is set to 1-5 seconds, the holding pressure is set to 40-50MPa, and the holding time is set to 30-90 seconds;
[0034] S2. The preformed plastic parts for the charging pile are subjected to electron beam irradiation using an electron electrostatic accelerator;
[0035] The irradiation process is set as follows: voltage 1.0-3.0 mV, current 0.2-1.0 mA, power 0.2-3.0 kW, irradiation time 10-30 seconds;
[0036] S3. Immerse the irradiated preform in hot water at 100 to 120° C. for 10 to 20 minutes for annealing, and then cool naturally to room temperature to obtain plastic parts for charging piles.
[0037] Specifically, in the manufacturing process of the plastic parts for charging piles: after the plastic parts for charging piles are irradiated with electron beams, a macromolecular cross-linking reaction will occur to form a network structure, and after annealing, the residual internal stress can be eliminated. The plastic parts for charging piles are injection molded using a hot runner mold.
[0038] Beneficial effects of the present invention:
[0039] (1) The material of the present invention is a plastic material with a near-zero thermal expansion coefficient and high impact strength, which has a stable near-zero thermal expansion coefficient of 0±1×10 -6 / ℃, its impact strength reaches 45KJ / m 2 At the same time, the plastic material of the present invention has high strength and fluidity, and is suitable for high-power charging piles with high requirements for dimensional stability.
[0040] (2) The heat shrinkable filler (Hf2W3O 12 Whiskers have a negative thermal expansion coefficient, which can offset the positive thermal expansion coefficient of the resin (PC resin and PMMA resin), further making the expansion coefficient of the obtained plastic material lower.
[0041] (3) The plastic material of the present invention accurately controls the proportion of each component, and the heat shrink filler (Hf2W3O 12 The optimized ratio of whiskers to resin can control the thermal expansion coefficient of the plastic material to near zero. The plastic material of the present invention also utilizes the toughness of silk and improves the impact strength of the material by adding short chopped silk, so that the manufactured charging pile plastic product has the dual advantages of high impact strength and low expansion coefficient.
[0042] (4) The method of manufacturing plastic parts for charging piles of the present invention also adopts an irradiation process, which uses the strong radioactivity of the irradiation to cause the macromolecular chains of the resin (PC resin and PMMA resin) to undergo a cross-linking reaction, thereby making them insoluble and infusible. DETAILED DESCRIPTION
[0043] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Example 1
[0045] Provided is a plastic material with a low expansion coefficient and high impact strength, the plastic material comprising the following components by weight: 0.1 wt% of a coupling agent, 0.1 wt% of an antioxidant, 0.1 wt% of a lubricant, 2.0 wt% of a reinforcing material, 30.0 wt% of a heat shrink filler, and a resin balance (67.7 wt%);
[0046] Among them: the coupling agent is silane coupling agent KH550, the antioxidant is sodium sulfate, the lubricant is natural paraffin, the reinforcing material is short-cut silk with a diameter of 13-20nm and a length of 200-500μm, and the heat shrinkable filler is Hf2W3O with a diameter of 20-50nm. 12 For whiskers, the resin is a mixture of PC resin and PMMA resin in a weight ratio of 3:1;
[0047] Wherein, the Hf2W3O 12 The method for preparing whiskers comprises the following specific steps:
[0048] S1, soaking the silk in hot water at 150° C. and ultrasonically vibrating for 24 hours to perform refining and degumming to obtain silk fibroin fibers;
[0049] S2, immersing the above-mentioned silk fiber in a mixed solution containing HfCl4 and WCl4 (specifically containing 5.0wt% HfCl4 and 5.0wt% WCl4) for 5 minutes, and then drying at 80°C for 24 hours, and then placing it in a vacuum furnace and passing high-purity oxygen at 1200°C for 2 hours to obtain Hf2W3O4 with a negative thermal expansion coefficient. 12 Whiskers.
[0050] Preparation: The method for preparing the plastic material with low expansion coefficient and high impact strength of the above-mentioned embodiment 1 comprises the following steps:
[0051] S1. According to the proportion, the components of the plastic material are mixed uniformly in a low-speed mixer at room temperature, the stirring time is set to 30 minutes, and the stirring speed is set to 10 rpm;
[0052] S2. The uniformly mixed materials are blended and granulated through a twin-screw extruder to obtain the plastic material; wherein the aspect ratio of the twin-screw extruder is 44:1 and the screw diameter is 36 mm; the extrusion process is set as follows: temperature 200°C, main engine speed 300 rpm, and the long strips extruded from the die are cooled and granulated through a water tank.
[0053] Application: The plastic material of the above-mentioned embodiment 1 is used to manufacture plastic parts for charging piles, and the manufacturing method thereof comprises the following steps:
[0054] S1. Plasticizing, injection-filling, and pressure-maintaining the obtained plastic material using an injection molding machine to obtain a preformed plastic component for a charging pile;
[0055] Among them: the plasticizing temperature is 240℃, the injection pressure is set to 80MPa, the injection time is set to 1 second, the holding pressure is set to 40MPa, and the holding time is set to 30 seconds;
[0056] S2. The above-mentioned plastic component preform for the charging pile is subjected to electron beam irradiation using an electron electrostatic accelerator;
[0057] The irradiation process was set as follows: voltage 1mV, current 0.2mA, power 0.2kW, and irradiation time 10 seconds;
[0058] S3. Immerse the irradiated preform in 100° C. hot water for 10 minutes for annealing, and then cool naturally to room temperature to obtain plastic parts for charging piles.
[0059] Example 2
[0060] Provided is a plastic material with a low expansion coefficient and high impact strength, the plastic material comprising the following components by weight: 0.25wt% coupling agent, 0.25wt% antioxidant, 0.25wt% lubricant, 3.5wt% reinforcing material, 40.0wt% heat shrink filler and a resin balance;
[0061] Among them: the coupling agent is silane coupling agent KH560, the antioxidant is sodium thiosulfate, the lubricant is graphite, the reinforcing material is short-cut silk with a diameter of 13-20nm and a length of 200-500μm, and the heat shrinkable filler is Hf2W3O with a diameter of 20-50nm. 12 For whiskers, the resin is a mixture of PC resin and PMMA resin in a weight ratio of 4.5:1.5;
[0062] Wherein, the Hf2W3O 12 The method for preparing whiskers comprises the following specific steps:
[0063] S1, soaking the silk in hot water at 125° C. and ultrasonically vibrating for 36 hours to perform refining and degumming to obtain silk fibroin fibers;
[0064] S2, immersing the above-mentioned silk fiber in a mixed solution containing HfCl4 and WCl4 (specifically containing 2.0wt% HfCl4 and 2.0wt% WCl4) for 10 minutes, and then drying at 90°C for 12 hours, and then placing it in a vacuum furnace and passing high-purity oxygen at 1100°C for 3 hours to obtain Hf2W3O4 with a negative thermal expansion coefficient. 12 Whiskers.
[0065] Preparation: The method for preparing the plastic material with low expansion coefficient and high impact strength of the above-mentioned embodiment 2 comprises the following steps:
[0066] S1. According to the proportion, the components of the plastic material are mixed uniformly in a low-speed mixer at room temperature, the stirring time is set to 45 minutes, and the stirring speed is set to 20 rpm;
[0067] S2. The above-mentioned uniformly mixed materials are blended and granulated through a twin-screw extruder to obtain the plastic material; wherein the aspect ratio of the twin-screw extruder is 44:1 and the screw diameter is 36 mm; the extrusion process is set as follows: temperature 210°C, main engine speed 350rpm, and the long strips extruded from the die are cooled and granulated through a water tank.
[0068] Application: The plastic material of the above-mentioned embodiment 2 is used to manufacture plastic parts for charging piles, and the manufacturing method thereof comprises the following steps:
[0069] S1. Plasticizing, injection-filling, and pressure-maintaining the obtained plastic material using an injection molding machine to obtain a preformed plastic component for a charging pile;
[0070] Among them: the plasticizing temperature is 260℃, the injection pressure is set to 100MPa, the injection time is set to 3 seconds, the holding pressure is set to 45MPa, and the holding time is set to 60 seconds;
[0071] S2. The above-mentioned plastic component preform for the charging pile is subjected to electron beam irradiation using an electron electrostatic accelerator;
[0072] The irradiation process was set as follows: voltage 2.0 mV, current 0.6 mA, power 1.5 kW, and irradiation time 20 seconds;
[0073] S3. Immerse the irradiated preform in hot water at 110° C. for 15 minutes for annealing, and then cool naturally to room temperature to obtain plastic parts for charging piles.
[0074] Example 3
[0075] Provided is a plastic material with a low expansion coefficient and high impact strength, the plastic material comprising the following components by weight: 0.5wt% coupling agent, 0.5wt% antioxidant, 0.5wt% lubricant, 5.0wt% reinforcing material, 50.0wt% heat shrink filler and the remainder of resin;
[0076] Wherein: the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570, and the three are mixed in a weight ratio of 1:1:1;
[0077] The antioxidant is a mixture of sodium sulfate, sodium pyrosulfite, sodium bisulfate and sodium thiosulfate in a weight ratio of 1:1:1:1;
[0078] The lubricant is a mixture of natural paraffin and graphite in a 1:1 mass ratio;
[0079] The reinforcing material is selected from short-cut silk with a diameter of 13-20 nm and a length of 200-500 μm; the heat-shrinkable filler is selected from Hf2W3O 12 Whiskers; the resin is a mixture of PC resin and PMMA resin in a weight ratio of 5:2;
[0080] Wherein, the Hf2W3O 12 The method for preparing whiskers comprises the following specific steps:
[0081] S1, soaking the silk in hot water at 140° C. and ultrasonically vibrating for 48 hours to perform refining and degumming to obtain silk fibroin fibers;
[0082] S2, immersing the above-mentioned silk fiber in a mixed solution containing HfCl4 and WCl4 (specifically containing 8.0wt% HfCl4 and 8.0wt% WCl4) for 7 minutes, and then drying at 100°C for 8 hours, and then placing it in a vacuum furnace and passing high-purity oxygen at 1000°C for 4 hours to obtain Hf2W3O4 with a negative thermal expansion coefficient. 12 Whiskers.
[0083] Preparation: The preparation method of the plastic material with low expansion coefficient and high impact strength of the above-mentioned embodiment 3 comprises the following steps:
[0084] S1. According to the proportion, the components of the plastic material are mixed uniformly in a low-speed mixer at room temperature, the stirring time is set to 60 minutes, and the stirring speed is set to 15 rpm;
[0085] S2. The above-mentioned uniformly mixed materials are blended and granulated through a twin-screw extruder to obtain the plastic material; wherein the aspect ratio of the twin-screw extruder is 44:1 and the screw diameter is 36 mm; the extrusion process is set as follows: temperature 200°C, main engine speed 400rpm, and the long strips extruded from the die are cooled and granulated through a water tank.
[0086] Application: The plastic material of the above-mentioned embodiment 3 is used to manufacture plastic parts for charging piles, and the manufacturing method thereof comprises the following steps:
[0087] S1. Plasticizing, injection-filling, and pressure-maintaining the obtained plastic material using an injection molding machine to obtain a preformed plastic component for a charging pile;
[0088] Among them: the plasticizing temperature is 285℃, the injection pressure is set to 130MPa, the injection time is set to 5 seconds, the holding pressure is set to 50MPa, and the holding time is set to 90 seconds;
[0089] S2. The above-mentioned plastic component preform for the charging pile is subjected to electron beam irradiation using an electron electrostatic accelerator;
[0090] The irradiation process was set as follows: voltage 3.0 mV, current 1.0 mA, power 3.0 kW, and irradiation time 30 seconds;
[0091] S3. Immerse the irradiated preform in hot water at 120° C. for 20 minutes for annealing, and then cool naturally to room temperature to obtain plastic parts for charging piles.
[0092] Comparative Example 1
[0093] A plastic material is provided, which comprises the following components in weight fractions: 0.1 wt% of a coupling agent, 0.1 wt% of an antioxidant, 0.1 wt% of a lubricant, 2.0 wt% of a reinforcing material, 25.0 wt% of a heat shrinkable filler and a resin balance (72.7 wt%).
[0094] The difference between Comparative Example 1 and Example 1 is that the content of the heat shrinkable filler in Comparative Example 1 is lower than that in Example 1, and the content of the resin is higher than that in Example 1.
[0095] Comparative Example 2
[0096] A plastic material is provided, comprising the following components in weight fractions: 0.5 wt% coupling agent, 0.5 wt% antioxidant, 0.5 wt% lubricant, 5.0 wt% reinforcing material, 55.0 wt% heat shrink filler and the remainder of resin (38.5 wt%).
[0097] The difference between Comparative Example 2 and Example 3 is that the content of the heat shrinkable filler in Comparative Example 2 is higher than that in Example 3, while the content of the resin is lower than that in Example 3.
[0098] Comparative Example 3
[0099] The difference between Comparative Example 3 and Example 1 is that the manufacturing method of the plastic parts for the charging pile provided in Comparative Example 3 does not perform annealing and shaping treatment, and the rest is the same as Example 1.
[0100] Comparative Example 4
[0101] The difference between Comparative Example 4 and Example 1 is that the manufacturing method of the plastic parts for the charging pile provided in Comparative Example 4 does not perform electron beam irradiation treatment, and the rest is the same as Example 1.
[0102] test:
[0103] (1) The linear expansion coefficient of the plastic parts for charging piles obtained in Examples 1 to 3 and Comparative Examples 1 to 4 was tested at -30 to 150° C. using the standard method for determining the linear thermal expansion coefficient of plastics (ISO 11359-2). The specific test results are shown in Table 1 below.
[0104] (2) The physical property test methods of the plastic parts for charging piles obtained in Examples 1 to 3 and Comparative Examples 1 to 4 refer to ISO standards (tensile strength ISO 527, bending strength ISO 178, impact strength ISO 180). For specific test results, see Table 1 below.
[0105] Table 1 shows the linear expansion coefficient and physical property test results of the plastic parts for charging piles obtained in Examples 1 to 3 and Comparative Examples 1 to 4
[0106]
[0107] The test results show that the material of the present invention has a stable near-zero thermal expansion coefficient in the temperature range of -30°C to 150°C, and its impact strength can reach 45KJ / m 2 .
[0108] At the same time, it can be seen from the test results of Comparative Examples 1 and 2 and Examples 1 and 3 that the plastic material of the present invention can be used to heat shrink filler (Hf2W3O 12 By optimizing the ratio of the whisker to the resin, the thermal expansion coefficient of the material can be controlled to be close to zero. It can be seen from the test results of Comparative Examples 3 and 4 that the manufacturing method of the plastic parts for the charging pile of the present invention further enhances the strength of the obtained material by adopting annealing and electron beam irradiation processes.
[0109] The above are preferred embodiments of the present invention and are only used to explain the present invention, not to limit the present invention. Any obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A plastic material with low expansion coefficient and high impact strength, It is characterized in that The plastic material comprises the following components in weight fractions: 0.1-0.5wt% coupling agent, 0.1-0.5wt% antioxidant, 0.1-0.5wt% lubricant, 2.0-5.0wt% reinforcing material, 30.0-50.0wt% heat shrink filler and the remainder of resin.
2. A plastic material with low expansion coefficient and high impact strength according to claim 1, It is characterized in that The coupling agent is selected from at least one of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570; the antioxidant is selected from at least one of sodium sulfate, sodium pyrosulfite, sodium bisulfate and sodium thiosulfate; and the lubricant is selected from natural paraffin and / or graphite.
3. A plastic material with low expansion coefficient and high impact strength according to claim 1, It is characterized in that The reinforcing material is short-cut silk, and the length of the short-cut silk is 200-500 μm and the diameter is 13-20 nm.
4. A plastic material with low expansion coefficient and high impact strength according to claim 1, It is characterized in that The heat shrinkable filler is Hf with a diameter of 20 to 50 nm. 2 W 3 O 12 Whiskers.
5. A plastic material with low expansion coefficient and high impact strength according to claim 4, It is characterized in that The Hf 2 W 3 O 12 The method for preparing whiskers comprises the following steps: S1, refining and degumming silk to obtain silk fibroin fibers; S2, immersing the silk fiber in a solution containing HfCl 4 and WCl 4 The mixed solution was then dried and calcined to obtain Hf with a negative thermal expansion coefficient. 2 W 3 O 12 Whiskers.
6. A plastic material with low expansion coefficient and high impact strength according to claim 5, It is characterized in that The Hf 2 W 3 O 12 The method for preparing whiskers comprises the following steps: S1, soaking the silk in hot water at 120-150° C. and ultrasonically vibrating for 24-48 hours to perform refining and degumming to obtain silk fibroin fibers; S2, immersing the silk fiber in a solution containing HfCl 4 and WCl 4 The mixture is placed in a mixed solution of 5 to 10 minutes, and then dried at 80 to 100°C for 8 to 24 hours, and then placed in a vacuum furnace and calcined at 1000 to 1200°C for 2 to 4 hours by passing high-purity oxygen, thereby obtaining Hf with a negative thermal expansion coefficient. 2 W 3 O 12 Whiskers; Wherein: the mixed solution contains 1.0-10.0wt% HfCl 4 and 1.0~10.0wt% WCl 4 .
7. A plastic material with low expansion coefficient and high impact strength according to claim 1, It is characterized in that The resin includes PC resin and PMMA resin, and the weight ratio of the PC resin to the PMMA resin is (3-5): (1-2).
8. A method for preparing a plastic material with low expansion coefficient and high impact strength according to any one of claims 1 to 7, It is characterized in that The method comprises the following steps: S1. Mix the components of the plastic material uniformly according to the proportion; S2, blending and granulating the mixed materials through an extruder to obtain the plastic material.
9. Use of a plastic material with low expansion coefficient and high impact strength, It is characterized in that The plastic material according to any one of claims 1 to 7 is used to manufacture plastic parts for charging piles, and the manufacturing method thereof comprises the following steps: S1. Plasticizing, injection-filling, and pressure-maintaining the plastic material to obtain a preformed plastic component for a charging pile; S2, irradiating the preform with an electron beam; S3. Annealing the irradiated preform to obtain plastic parts for charging piles.
10. Use of a plastic material with low expansion coefficient and high impact strength according to claim 9, It is characterized in that The manufacturing method of the plastic parts for the charging pile comprises the following specific steps: S1. Plasticizing, injection-filling, and pressure-maintaining the plastic material using an injection molding machine to obtain a preformed plastic component for a charging pile; Among them: the plasticizing temperature is 240-285°C, the injection pressure is set to 80-130MPa, the injection time is set to 1-5 seconds, the holding pressure is set to 40-50MPa, and the holding time is set to 30-90 seconds; S2. The preformed plastic parts for the charging pile are subjected to electron beam irradiation using an electron electrostatic accelerator; The irradiation process is set as follows: voltage 1.0-3.0 mV, current 0.2-1.0 mA, power 0.2-3.0 kW, irradiation time 10-30 seconds; S3. Immerse the irradiated preform in hot water at 100 to 120° C. for 10 to 20 minutes for annealing, and then cool naturally to room temperature to obtain plastic parts for charging piles.