Production method of pigment carbon black for high-blackness ink
By using high-temperature combustion and quench treatment combined with ozone oxidation technology in carbon black production, the problem of difficult dispersion and poor stability of pigmented carbon black in ink applications is solved, and the performance of high blackness and high gloss is achieved, which meets high standards. Application requirements.
Patent Information
- Application Number
- CN202411129590.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-19
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
Pigmented carbon black is prone to difficult dispersion, high viscosity, poor stability and unstable carbon black quality in ink application systems, resulting in performance fluctuations, mainly due to the excessive fluctuation range of carbon black quality indicators.
A method of producing pigment carbon black for high-black inks is adopted. By heating the filtered air and mixing it with natural gas to burn, injecting raw oil for incomplete combustion and cracking, then terminating the reaction and activation through the quench section, using ozone Perform surface oxidation treatment, finally dry and crushed to ensure high blackness and stability of carbon black particles.
The ink performance with high blackness and high gloss is achieved, the problems of difficulty in dispersion and poor stability are solved, the application requirements of high standards of ink are met, and the content of harmful substances and heavy metals are reduced through the selection of anthracene oil and potassium carbonate.
Smart Images

Figure CN119019866A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon black production, and in particular to a method for producing pigment carbon black for high-blackness ink. Background Art
[0002] Carbon black is a kind of amorphous carbon, with a basic particle size between 8-100nm. It has excellent rubber reinforcement, coloring, conductivity or antistatic and ultraviolet absorption functions. It is the earliest nano-scale material developed and applied by humans. Carbon black is a light, loose and extremely fine black powder in its natural state. The specific surface area is very large, ranging from tens to thousands of m2 / g. It is a product obtained by incomplete combustion or thermal decomposition of hydrocarbon organic matter under certain conditions.
[0003] Carbon black can be divided into two categories according to its use, namely rubber carbon black and special carbon black.
[0004] Rubber carbon black improves the excellent reinforcement performance of rubber materials and has a very wide range of applications in the tire field. Special carbon black can be divided into pigment carbon black and conductive carbon black according to its use. The former is a black inorganic pigment and has corresponding products in many application fields, such as carbon black for inks, carbon black for coatings, carbon black for sealants, carbon black for masterbatches, and carbon black for chemical fibers.
[0005] As downstream application requirements continue to increase, carbon black production technology has developed to varying degrees. Technical research on pigment carbon black often achieves the improvement of carbon black's own indicators or the actual application performance of coatings, inks, etc. through conventional technical research.
[0006] In the prior art, pigment carbon black is prone to being difficult to disperse, having high viscosity, poor stability, and unstable carbon black quality in the ink application system. During the ink application process, the performance fluctuates, which is directly related to the excessive fluctuation range of the quality indicators of carbon black. Summary of the invention
[0007] The object of the present invention is to provide a method for producing high-blackness ink pigment carbon black to solve the following technical problems:
[0008] Pigment carbon black is prone to being difficult to disperse, having high viscosity, poor stability, and unstable carbon black quality in the ink application system. During the ink application process, the performance fluctuates, which is directly related to the excessive fluctuation range of carbon black's quality indicators.
[0009] The purpose of the present invention can be achieved through the following technical solutions:
[0010] A method for producing carbon black pigment for high-blackness ink comprises the following steps:
[0011] S1, the filtered air is pressurized by a fan and heated by a preheater and then sent into the combustion chamber;
[0012] S2, natural gas is introduced into the combustion chamber to mix with hot air and fully burn, and the hot flue gas after combustion flows through the reaction throat section at a high speed;
[0013] S3, after the raw oil and the additive are fully mixed, they are radially sprayed into the hot flue gas through the throat section, and the raw oil reacts to generate flue gas rich in carbon black particles;
[0014] S4, passing the flue gas containing carbon black through a horizontal extremely cold section to rapidly cool down the flue gas so as to terminate the reaction, passing through a vertical extremely cold section to activate the carbon black particles, and passing through an air preheater to cool down the flue gas;
[0015] S5. The carbon black flue gas that has passed through the secondary quenching section is mostly collected by a cyclone separator, and the remaining small amount of carbon black flue gas is passed through the tertiary quenching section, and a collection bag filter is used to separate the carbon black and tail gas. The tail gas is sent to the tail gas power station by a fan for power generation;
[0016] S6, crushing the collected carbon black through an air multi-stage crusher and conveying it to a pneumatic bag filter using a relay fan;
[0017] S7, the carbon black collected by the pneumatic bag filter is granulated by a dry granulator, ozone is introduced for surface oxidation treatment, and then enters a dryer for drying;
[0018] S8. After the carbon black particles pass through the screening machine, they enter the finished product storage tank and are packaged to obtain the product.
[0019] Preferably, in S1, in order to ensure the purity of the produced carbon black, the air can be filtered at multiple stages according to actual conditions, and the filtered air further improves the combustion efficiency and ensures that the temperature in the reaction furnace is more stable;
[0020] Use a three-layer filter with a filter size of less than 1μm to filter the air and remove dust and impurities in the air;
[0021] Then the pressure is increased to 0.15-0.19Mpa by the Roots blower, and then heated to 700℃ by the 800℃ high temperature air preheater and sent to the combustion chamber. The air delivery flow is 5000-8000Nm 3 / h.
[0022] Preferably, in S2, the flow rate of the natural gas during transportation is 400-800 Nm 3 / h, pressure is 70-80kpa;
[0023] The temperature of the combustion chamber is 1800-1900°C.
[0024] The stability of natural gas flow is the key to ensuring the quality of pigment carbon black. Stable natural gas flow ensures its full combustion and stable temperature. The high-pressure shear force of natural gas and preheated air further cracks the crude oil to form carbon black.
[0025] Preferably, in S3, the flow rate of the raw oil radially sprayed into the hot flue gas through the throat section is 1200-1500 kg / h, and the flow rate of the additive is 6-12 kg / h;
[0026] The crude oil undergoes incomplete combustion and cracking reaction in the reaction section to generate carbon black, and the reaction pressure is 50-70kpa.
[0027] Preferably, the raw oil is anthracene oil and the additive is potassium carbonate.
[0028] Anthracene oil as a raw material oil has lower content of polycyclic aromatic hydrocarbons (harmful substances) in the product after high-temperature reaction than coal tar. Anthracene oil is a part of coal tar components. The fraction of 280-360°C is obtained by distilling tar. It has low asphaltene content and stable oil quality. As a raw material oil for pigment carbon black, it can improve the blackness and tinting power of the product and reduce the content of heavy metals.
[0029] Potassium carbonate is used as an additive. The potassium ions in it combine with the carbon ions in the raw oil to form a chelate, which inhibits the growth of the carbon black structure and controls the structure of the carbon black. The additive and the raw oil are fully mixed before being sprayed into the throat, which is conducive to the uniform distribution of the carbon black structure and improves the quality stability of the product.
[0030] Preferably, in S4, when the flue gas rich in carbon black particles passes through the horizontal extremely cold section, deionized water with a flow rate of 1000-2500 kg / h and a pressure of 1.6-2.3 MPa is directly sprayed into it for vaporization and rapid cooling to terminate the reaction;
[0031] When passing through the vertical extreme cold section, medium-pressure steam with a flow rate of 800-1300kg / h and a pressure of 1.2-2Mpa is sprayed into it to activate the carbon black particles, increase the content of oxygen-containing functional groups on the surface of the carbon black, and improve the blackness and tinting strength of the carbon black;
[0032] Preferably, in S4, the carbon black flue gas passing through the vertical ultra-cold section then passes through 800°C and 350°C air preheaters in sequence, and the temperature drops to 350°C.
[0033] Preferably, in S5, the temperature of the carbon black flue gas drops to 260° C. when passing through three rapid cooling stages.
[0034] Preferably, in S7, the carbon black collected by the pneumatic bag filter is granulated by a granulator, and then ozone is introduced, and the highly oxidizing ozone reacts with the carbon black to form oxidized functional groups on the surface of the carbon black, thereby further improving the surface activity of the carbon black and making it easier to disperse;
[0035] The oxidized carbon black enters the dryer for drying to remove moisture and ozone in the production process; the advantage of ozone oxidation post-treatment is that ozone does not cause corrosion damage to the equipment, and after ozone oxidation, it decomposes into oxygen at high temperature, which does not pollute the environment, does not generate solid impurities, and improves the quality of pigment carbon black.
[0036] Beneficial effects of the present invention:
[0037] (1) The present invention uses anthracene oil as raw material for pigment carbon black for high-blackness ink, natural gas as fuel and high-temperature filtered air for full mixing and combustion to provide reaction heat energy, collects most of the carbon black through secondary cooling, and completes the collection of intermediate carbon black through tertiary rapid cooling to 260°C; then dry granulates, introduces ozone for oxidation treatment to increase the content of oxygen-containing functional groups on the surface of carbon black particles, collects and packages the product after drying; the product is tested for ink application in gravure ink, and the blackness can reach above 270, the glossiness is high, and excellent application performance is shown; the problem of difficult dispersion, high viscosity and poor stability of pigment carbon black in ink application system in the prior art is solved, and high blackness and high gloss performance are provided for terminal ink application, meeting the high standard requirements of pigment carbon black ink application field
[0038] (2) The present invention uses anthracene oil as raw material oil. Compared with coal tar after high-temperature reaction, the content of polycyclic aromatic hydrocarbons (harmful substances) in the product is lower. Anthracene oil is a part of the coal tar component. The fraction of 280-360°C is obtained by distilling tar. The asphaltene content is low and the oil quality is stable. As the raw material oil of pigment carbon black, it can improve the blackness and tinting power of the product and reduce the content of heavy metals.
[0039] (3) The present invention uses potassium carbonate as an additive, wherein the potassium ions combine with the carbon ions in the feedstock oil to form a chelate, inhibiting the growth of the carbon black structure and controlling the structure of the carbon black. The additive and the feedstock oil are fully mixed before being sprayed into the throat, which is beneficial to the uniform distribution of the carbon black structure and improving the quality stability of the product;
[0040] (4) The present invention uses carbon black collected by a pneumatic bag filter, which is granulated by a granulator and then ozone is introduced. The highly oxidizing ozone reacts with the carbon black to form oxidized functional groups on the surface of the carbon black, thereby further improving the surface activity of the carbon black and making it easier to disperse. The oxidized carbon black is dried in a dryer to remove moisture and ozone in the production process. The advantage of ozone oxidation post-treatment is that ozone does not cause corrosion damage to equipment, and after ozone oxidation, it is decomposed into oxygen at high temperature, which does not pollute the environment and does not generate solid impurities, thereby improving the quality of pigment carbon black. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The present invention will be further described below in conjunction with the accompanying drawings.
[0042] Figure 1 The present invention is a schematic flow chart of a method for producing carbon black pigment for high-blackness ink. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Example 1
[0045] See also Figure 1 As shown, the present invention is a method for producing a high-blackness ink pigment carbon black, comprising the following steps:
[0046] S1, the filtered air is pressurized by a fan and heated by a preheater and then sent into the combustion chamber;
[0047] Specifically, in this embodiment, a three-layer filter screen with a size of less than 1 μm is used to filter the air to remove dust and impurities in the air;
[0048] Then the pressure is increased to 0.16Mpa by the Roots blower, and it is heated to 700℃ by the 800℃ high-temperature air preheater and sent to the combustion chamber. The air delivery flow is 6000Nm 3 / h;
[0049] S2, natural gas is introduced into the combustion chamber to mix with hot air and fully burn, and the hot flue gas after combustion flows through the reaction throat section at a high speed;
[0050] Specifically, in this embodiment, the flow rate of natural gas during transportation is 500Nm 3 / h, pressure is 75kpa;
[0051] The combustion chamber temperature is 1850°C;
[0052] S3, after the raw oil and the additive are fully mixed, they are radially sprayed into the hot flue gas through the throat section, and the raw oil reacts to generate flue gas rich in carbon black particles;
[0053] Specifically, in this embodiment, the flow rate of the raw oil radially sprayed into the hot flue gas through the throat section is 1350 kg / h, the flow rate of the additive is 8 kg / h, the weight ratio of the amount of raw oil to the amount of the additive potassium carbonate is 450:0.01, and the water content of the raw oil is less than 1%;
[0054] The crude oil undergoes incomplete combustion and cracking reaction in the reaction section to generate carbon black, and the reaction pressure is 65kpa;
[0055] The raw material oil is anthracene oil, and the additive is potassium carbonate;
[0056] S4, passing the flue gas containing carbon black through a horizontal extremely cold section to rapidly cool down the flue gas so as to terminate the reaction, passing through a vertical extremely cold section to activate the carbon black particles, and passing through an air preheater to cool down the flue gas;
[0057] Specifically, in this embodiment, when passing through the horizontal extremely cold section, deionized water with a flow rate of 1800 kg / h and a pressure of 1.9 MPa is directly sprayed therein to vaporize and rapidly cool down to terminate the reaction;
[0058] When passing through the vertical extremely cold section, medium-pressure steam with a flow rate of 900kg / h and a pressure of 1.6Mpa is sprayed into it to activate the carbon black particles;
[0059] The carbon black flue gas passing through the vertical extreme cold section then passes through the 800℃ and 350℃ air preheaters in sequence, and the temperature drops to 350℃;
[0060] S5. The carbon black flue gas that has passed through the secondary quenching section is mostly collected by a cyclone separator, and the remaining small amount of carbon black flue gas is passed through the tertiary quenching section, and a collection bag filter is used to separate the carbon black and tail gas. The tail gas is sent to the tail gas power station by a fan for power generation;
[0061] Specifically, in this embodiment, the temperature of the carbon black flue gas drops to 260°C when passing through the three quenching stages, and the three quenching stages use a 260°C low-temperature air preheater;
[0062] S6, crushing the collected carbon black through an air multi-stage crusher and conveying it to a pneumatic bag filter using a relay fan;
[0063] S7, the carbon black collected by the pneumatic bag filter is granulated by a dry granulator, ozone is introduced for surface oxidation treatment, and then enters a dryer for drying;
[0064] Specifically, in this embodiment, the carbon black collected by the pneumatic bag filter is granulated by a granulator, and then ozone is introduced. The highly oxidizing ozone reacts with the carbon black to form oxidized functional groups on the surface of the carbon black.
[0065] S8. After the carbon black particles pass through a 35-mesh screening machine, they enter the finished product storage tank and are packaged to obtain the product.
[0066] Example 2
[0067] A method for producing carbon black pigment for high-blackness ink comprises the following steps:
[0068] S1, the filtered air is pressurized by a fan and heated by a preheater and then sent into the combustion chamber;
[0069] Specifically, in this embodiment, a three-layer filter screen with a size of less than 1 μm is used to filter the air to remove dust and impurities in the air;
[0070] Then the pressure is increased to 0.15Mpa by the Roots blower, and it is heated to 700℃ by the 800℃ high-temperature air preheater and sent to the combustion chamber. The air delivery flow is 5000Nm 3 / h;
[0071] S2, natural gas is introduced into the combustion chamber to mix with hot air and fully burn, and the hot flue gas after combustion flows through the reaction throat section at a high speed;
[0072] Specifically, in this embodiment, the flow rate of natural gas during transportation is 400Nm 3 / h, pressure is 70kpa;
[0073] The combustion chamber temperature is 1800°C;
[0074] S3, after the raw oil and the additive are fully mixed, they are radially sprayed into the hot flue gas through the throat section, and the raw oil reacts to generate flue gas rich in carbon black particles;
[0075] Specifically, in this embodiment, the flow rate of the raw oil radially sprayed into the hot flue gas through the throat section is 1200 kg / h, the flow rate of the additive is 6 kg / h, the weight ratio of the amount of raw oil to the amount of the additive potassium carbonate is 450:0.01, and the water content of the raw oil is less than 1%;
[0076] The crude oil undergoes incomplete combustion and cracking reaction in the reaction section to generate carbon black, and the reaction pressure is 50kpa;
[0077] The raw material oil is anthracene oil, and the additive is potassium carbonate;
[0078] S4, passing the flue gas containing carbon black through a horizontal extremely cold section to rapidly cool down the flue gas so as to terminate the reaction, passing through a vertical extremely cold section to activate the carbon black particles, and passing through an air preheater to cool down the flue gas;
[0079] Specifically, in this embodiment, when passing through the horizontal extremely cold section, deionized water with a flow rate of 1000 kg / h and a pressure of 1.6 MPa is directly sprayed therein to vaporize and rapidly cool down to terminate the reaction;
[0080] When passing through the vertical extremely cold section, medium-pressure steam with a flow rate of 800kg / h and a pressure of 1.2Mpa is sprayed into it to activate the carbon black particles;
[0081] The carbon black flue gas passing through the vertical extreme cold section then passes through the 800℃ and 350℃ air preheaters in sequence, and the temperature drops to 350℃;
[0082] S5. The carbon black flue gas that has passed through the secondary quenching section is mostly collected by a cyclone separator, and the remaining small amount of carbon black flue gas is passed through the tertiary quenching section, and a collection bag filter is used to separate the carbon black and tail gas. The tail gas is sent to the tail gas power station by a fan for power generation;
[0083] Specifically, in this embodiment, the temperature of the carbon black flue gas drops to 260°C when passing through the three quenching stages, and the three quenching stages use a 260°C low-temperature air preheater;
[0084] S6, crushing the collected carbon black through an air multi-stage crusher and conveying it to a pneumatic bag filter using a relay fan;
[0085] S7, the carbon black collected by the pneumatic bag filter is granulated by a dry granulator, ozone is introduced for surface oxidation treatment, and then enters a dryer for drying;
[0086] Specifically, in this embodiment, the carbon black collected by the pneumatic bag filter is granulated by a granulator, and then ozone is introduced. The highly oxidizing ozone reacts with the carbon black to form oxidized functional groups on the surface of the carbon black.
[0087] S8. After the carbon black particles pass through a 35-mesh screening machine, they enter the finished product storage tank and are packaged to obtain the product.
[0088] Example 3
[0089] A method for producing carbon black pigment for high-blackness ink comprises the following steps:
[0090] S1, the filtered air is pressurized by a fan and heated by a preheater and then sent into the combustion chamber;
[0091] Specifically, in this embodiment, a three-layer filter screen with a size of less than 1 μm is used to filter the air to remove dust and impurities in the air;
[0092] Then the pressure is increased to 0.19Mpa by the Roots blower, and it is heated to 700℃ by the 800℃ high-temperature air preheater and sent to the combustion chamber. The air delivery flow is 8000Nm 3 / h;
[0093] S2, natural gas is introduced into the combustion chamber to mix with hot air and fully burn, and the hot flue gas after combustion flows through the reaction throat section at a high speed;
[0094] Specifically, in this embodiment, the flow rate of natural gas during transportation is 800Nm 3 / h, pressure is 80kpa;
[0095] The combustion chamber temperature is 1900°C;
[0096] S3, after the raw oil and the additive are fully mixed, they are radially sprayed into the hot flue gas through the throat section, and the raw oil reacts to generate flue gas rich in carbon black particles;
[0097] Specifically, in this embodiment, the flow rate of the raw oil radially sprayed into the hot flue gas through the throat section is 1500 kg / h, and the flow rate of the additive is 12 kg / h;
[0098] The crude oil undergoes incomplete combustion and cracking reaction in the reaction section to generate carbon black, and the reaction pressure is 70kpa;
[0099] The raw material oil is anthracene oil, and the additive is potassium carbonate;
[0100] S4, passing the flue gas containing carbon black through a horizontal extremely cold section to rapidly cool down the flue gas so as to terminate the reaction, passing through a vertical extremely cold section to activate the carbon black particles, and passing through an air preheater to cool down the flue gas;
[0101] Specifically, in this embodiment, when passing through the horizontal extremely cold section, deionized water with a flow rate of 2500 kg / h and a pressure of 2.3 MPa is directly sprayed therein to vaporize and rapidly cool down to terminate the reaction;
[0102] When passing through the vertical extremely cold section, medium-pressure steam with a flow rate of 1300kg / h and a pressure of 2Mpa is sprayed into it to activate the carbon black particles;
[0103] The carbon black flue gas passing through the vertical extreme cold section then passes through the 800℃ and 350℃ air preheaters in sequence, and the temperature drops to 350℃;
[0104] S5. The carbon black flue gas that has passed through the secondary quenching section is mostly collected by a cyclone separator, and the remaining small amount of carbon black flue gas is passed through the tertiary quenching section, and a collection bag filter is used to separate the carbon black and tail gas. The tail gas is sent to the tail gas power station by a fan for power generation;
[0105] Specifically, in this embodiment, the temperature of the carbon black flue gas drops to 260°C when passing through the three quenching stages, and the three quenching stages use a 260°C low-temperature air preheater;
[0106] S6, crushing the collected carbon black through an air multi-stage crusher and conveying it to a pneumatic bag filter using a relay fan;
[0107] S7, the carbon black collected by the pneumatic bag filter is granulated by a dry granulator, ozone is introduced for surface oxidation treatment, and then enters a dryer for drying;
[0108] Specifically, in this embodiment, the carbon black collected by the pneumatic bag filter is granulated by a granulator, and then ozone is introduced. The highly oxidizing ozone reacts with the carbon black to form oxidized functional groups on the surface of the carbon black.
[0109] S8. After the carbon black particles pass through a 35-mesh screening machine, they enter the finished product storage tank and are packaged to obtain the product.
[0110] Test Example 1
[0111] The pigment carbon black prepared in Examples 1-3 was tested for DBP, BET specific surface area, heating loss, ash content, volatile matter, pH, and 45 μm sieve residue. The test results are as follows:
[0112] project index Testing standards DBP 52±3 GB / T3780.2 BET specific surface area 94±10 GB / T10722 Heating reduction ≤2 GB / T3780.8 Ash ≤0.5 GB / T3780.10 Volatile Matter ≥2.9 GB / T7047 pH 25±0.2 GB / T3780.7 45μm sieve residue ≤50 GB / T3780.21
[0113] Test Example 2
[0114] The carbon black pigment prepared in Examples 1-3 was used as the pigment component of the ink to test the appearance of the ink layer. The test steps were as follows:
[0115] Step 1: According to 15-30 parts of pigment carbon black, 40-60 parts of nitrocellulose resin solution, 1-4 parts of additives, and 20-30 parts of solvent, the pigment carbon black and other components are fully stirred and dispersed, and then ground to obtain a black base ink with a fineness not exceeding 10 μm;
[0116] Step 2: Mix and stir 20-25 parts of base ink, 24-30 parts of polyurethane resin solution and 5-10 parts of solvent to obtain ink;
[0117] Step 3: Use a gravure proofing machine to print ink on a PET film and then dry it to obtain a color card;
[0118] Step 4: Use a spectrophotometer to test the color of the ink color card and a gloss meter to test the gloss. The test results are as follows:
[0119]
[0120] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A method for producing carbon black pigment for high blackness ink, characterized in that: The steps include: S1, the filtered air is pressurized by a fan and heated by a preheater and then sent into the combustion chamber; S2, natural gas is introduced into the combustion chamber to mix with hot air and fully burn, and the hot flue gas after combustion flows through the reaction throat section at a high speed; S3, after the raw oil and the additive are fully mixed, they are radially sprayed into the hot flue gas through the throat section, and the raw oil reacts to generate flue gas rich in carbon black particles; S4, passing the flue gas containing carbon black through a horizontal extremely cold section to rapidly cool down the flue gas so as to terminate the reaction, passing through a vertical extremely cold section to activate the carbon black particles, and passing through an air preheater to cool down the flue gas; S5. The carbon black flue gas that has passed through the secondary quenching section is subjected to a cyclone separator to collect most of the carbon black, and the remaining small amount of carbon black flue gas is subjected to the tertiary quenching section, and a collection bag filter is used to separate the carbon black and tail gas; S6, crushing the collected carbon black through an air multi-stage crusher and conveying it to a pneumatic bag filter using a relay fan; S7, the carbon black collected by the pneumatic bag filter is granulated by a dry granulator, ozone is introduced for surface oxidation treatment, and then enters a dryer for drying; S8. After the carbon black particles pass through the screening machine, they enter the finished product storage tank and are packaged to obtain the product.
2. The method for producing a high-blackness ink pigment carbon black according to claim 1, characterized in that: In S1, the air is blown by a Roots blower to increase its pressure to 0.15-0.19Mpa, and then heated to 700℃ by an 800℃ high-temperature air preheater before being sent to the combustion chamber. The air delivery flow rate is 5000-8000Nm 3 / h.
3. The method for producing a high-blackness ink pigment carbon black according to claim 1, characterized in that: In S2, the flow rate of the natural gas during transportation is 400-800Nm 3 / h, pressure is 70-80kpa.
4. The method for producing a high-blackness carbon black pigment for ink according to claim 3, characterized in that: The temperature of the combustion chamber is 1800-1900°C.
5. The method for producing a high-blackness carbon black pigment for ink according to claim 3, characterized in that: In S3, the flow rate of the raw oil radially sprayed into the hot flue gas through the throat section is 1200-1500 kg / h, and the flow rate of the additive is 6-12 kg / h.
6. The method for producing a high-blackness carbon black pigment for ink according to claim 5, characterized in that: In S3, the reaction pressure of the crude oil in the reaction section is 50-70 kPa.
7. A method for producing a high-blackness carbon black pigment for ink according to any one of claims 1 to 6, characterized in that: The raw material oil is anthracene oil, and the additive is potassium carbonate.
8. The method for producing a high-blackness carbon black pigment for ink according to claim 6, characterized in that: In S4, when the flue gas rich in carbon black particles passes through the horizontal ultra-cold section, desalted water with a flow rate of 1000-2500kg / h and a pressure of 1.6-2.3Mpa is directly sprayed into it for vaporization and rapid cooling to terminate the reaction.
9. The method for producing a high-blackness carbon black pigment for ink according to claim 8, characterized in that: In S4, when the flue gas rich in carbon black particles passes through the vertical ultra-cold section, medium-pressure steam with a flow rate of 800-1300kg / h and a pressure of 1.2-2Mpa is sprayed into it to activate the carbon black particles.
10. The method for producing a high-blackness carbon black pigment for ink according to claim 9, characterized in that: In S4, the carbon black flue gas passing through the vertical ultra-cold section then passes through 800℃ and 350℃ air preheaters in sequence, and the temperature drops to 350℃.