A method for preparing ultrastable perovskite hollow nanocrystals with high fluorescence quantum yield
By preparing hollow perovskite nanocrystals with high fluorescence quantum yield, the problem of poor stability of perovskite quantum dots was solved, achieving higher fluorescence quantum yield and stability, and enhancing photocatalytic performance and adsorption capacity.
Patent Information
- Application Number
- CN202411115658.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Metal halide perovskite quantum dots exhibit poor stability in environments such as humidity, oxygen-rich conditions, high temperatures, and light exposure, leading to performance degradation and limiting their promotion and development in practical applications.
Precursor solutions A, B, and C were prepared using specific steps, and clean hollow perovskite nanocrystals were obtained by centrifugation. The specific steps included mixing organic cationic ligands, lead source, halogen source, and noncoordinate solvent, controlling the reaction temperature and vacuum, and finally removing reaction waste by antisolvent centrifugation.
It improves the fluorescence quantum yield and stability of perovskite nanocrystals, enhances the adsorption capacity and photocatalytic performance of substances, provides more active sites, is suitable for loading other substances and constructing heterostructures, and improves the separation efficiency of photogenerated electrons and holes.
Smart Images

Figure CN119020030B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of nanoluminescent materials and display lighting, specifically to a method for preparing perovskite hollow nanocrystals with high fluorescence quantum yield and ultra-stable properties. Background Technology
[0002] Halide perovskite nanocrystals exhibit numerous remarkable optoelectronic properties, making them truly remarkable. Firstly, they possess a wide color gamut, capable of displaying a rich variety of colors, while also exhibiting a remarkably narrow full width at half maximum (FWHM). This narrow FWHM results in extremely high purity of emitted light, significantly enhancing color recognition. Secondly, they possess a low nucleation temperature. This advantage greatly reduces the difficulty and cost of fabrication, creating highly favorable conditions for large-scale production. Furthermore, their tunable fluorescence emission peaks, with adjustable composition and size, are a major highlight. This characteristic provides them with exceptional flexibility and customizability, allowing for highly precise tailoring of light at specific wavelengths to meet diverse practical needs. Because of these excellent optoelectronic properties, halide perovskite nanocrystals can efficiently absorb and convert solar energy, offering new possibilities for energy acquisition and utilization. In the field of light-emitting diodes (LEDs), their superior color characteristics enable them to emit bright and pure light, bringing new opportunities to lighting and display technologies.
[0003] Despite significant advancements in the synthesis, characterization, theoretical development, and device applications of metal halide perovskite quantum dots (QDs), their poor stability remains a persistent and unresolved issue. When QDs are exposed to prolonged environments characterized by humidity, oxygen richness, high temperatures, and light, they typically undergo degradation. This leads to severe performance decline during storage, characterization, and processing, significantly hindering their widespread adoption and further development in practical applications.
[0004] Hollow nanocrystals have attracted considerable and widespread attention in many fields of materials science today. This is mainly due to their unique geometry, which endows them with distinctive properties. For example, their large surface area provides more active sites, enabling more efficient interaction with external substances. Their high load-bearing capacity makes them perform well under various pressures and loads, while their low density gives them an advantage in applications with strict weight requirements. Furthermore, hollow nanocrystals have enormous potential applications in catalysis, energy storage, drug delivery processes, and molecular separation technologies. To date, many hollow nanostructured materials, such as noble metals, metal oxides, hydroxides, and chalcogenides, have been reported. However, research and reports on hollow metal halide perovskite nanocrystals remain scarce. Summary of the Invention
[0005] This invention provides a method for preparing perovskite hollow nanocrystals with high fluorescence quantum yield and ultrastability, comprising the following steps:
[0006] S1: Prepare precursor solution A;
[0007] S2: Prepare precursor solution B;
[0008] S3: Prepare precursor solution C;
[0009] S4: Preparation of initial perovskite hollow nanocrystal solution;
[0010] S5: Obtain a clean, hollow perovskite nanostructure.
[0011] Furthermore, step S1 specifically includes:
[0012] Salt A, organic cationic ligand, and noncoordination solvent are thoroughly mixed. The mixing process must be carried out under strict protection of inert gas or vacuum, and the mixture must be stirred continuously for a predetermined time at a specific temperature to successfully obtain a clear and transparent precursor solution A.
[0013] Furthermore, step S2 specifically includes:
[0014] The lead source, halogen source, and non-coordinated solvent are mixed and subjected to vacuum treatment. The mixture is then reacted at a predetermined temperature for a specific time. An inert gas is then introduced to continue the reaction, followed by raising the temperature to a certain level and reacting for a further time. Finally, a specific amount of organic anionic and organic cationic ligands are added, and the mixture is heated and stirred for a certain period. Precursor solution B is obtained only when the solution becomes clear and transparent.
[0015] Furthermore, step S3 specifically includes:
[0016] A cationic salt is added to a mixed solvent consisting of an amphoteric ligand, oleic acid, and a nonpolar solvent. The mixture is stirred for a specific time under a pre-set temperature and vacuum environment. Then, an inert gas is introduced and the mixture is stirred thoroughly. The temperature is then increased and the mixture is reacted for a certain time to obtain the precursor solution C.
[0017] Furthermore, step S4 specifically includes:
[0018] A predetermined amount of precursor solution A is added to precursor solution B. The mixture is reacted at a certain temperature for a certain time. Then, the temperature is increased, and precursor solution C is added. The mixture is reacted at a certain temperature for a certain time. The solution is then rapidly cooled to room temperature to obtain the initial perovskite hollow nanocrystal solution.
[0019] Furthermore, step S5 specifically includes:
[0020] A predetermined amount of antisolvent was added to the solution prepared in S4 and centrifuged. Subsequently, the obtained precipitate was added to a solvent and dispersed again. The above centrifugation steps were repeated multiple times to completely remove the reaction waste generated during the synthesis of the perovskite hollow structure, and finally a clean perovskite nanostructure with a hollow structure was successfully obtained.
[0021] Further, in step S1, salt A is selected from one or more combinations of cesium salts, methylamine salts, and formamidine salts. Specifically, the cesium salt is one of cesium carbonate, cesium sulfate, cesium bicarbonate, cesium stearate, cesium acetate, and cesium nitrate. The methylamine salt is one of methylamine carbonate, methylamine sulfate, methylamine bicarbonate, methylamine stearate, methylamine acetate, and methylamine nitrate. The formamidine salt is one of formamidine carbonate, formamidine sulfate, formamidine bicarbonate, formamidine stearate, formamidine acetate, and formamidine nitrate. The organic cationic ligand is one or more of octanoic acid, oleic acid, stearic acid, caprylic acid, and trioctylphosphine oxide. The non-coordinating solvent can be one or more combinations of octadecene, octane, and dodecane, but is not limited to. The vacuum level is 10 mTorr-600 mTorr, and the inert gas used in the reaction is nitrogen or argon; the specific temperature is 45-230℃; the stirring time is 20-210 min; and the stirring speed is 200 rpm-800 rpm. The concentration of precursor solution A is 0.018-0.682 g / mL.
[0022] Further, in step S2, the lead source can be, but is not limited to, one or more of lead acetate, lead fluoride, lead hydrated cation, lead stearate, lead carbonate, lead nitrate, lead bromide, lead iodide, lead chloride, lead oleate, lead arsenate, lead chromate, lead molybdate, lead tungstate, lead vanadate, lead titanate, lead silicate, lead borate, lead formate, lead propionate, lead butyrate, lead valerate, lead hexanoate, lead octanoate, lead nonanoate, lead decanoate, lead laurate, lead myristate, lead palmitate, lead stearate, lead maleate, lead fumarate, lead tartrate, and lead citrate; the halogen source can be, but is not limited to, one or more of hydrobromic acid, hydroiodic acid, hydrochloric acid, and octadecyl dimethyl ammonium halide; the noncoordinating solvent can be, but is not limited to, one or more of octadecene, octane, and dodecane; the inert gas used in the reaction process is nitrogen or argon; organic anion The ionic ligand can be, but is not limited to, one or more of oleic acid, stearic acid, oxalic acid, mercaptopropionic acid, dodecyl mercaptoacetic acid, undecenoic acid, octanoic acid, and trioctylphosphine oxide; the organic cationic ligand can be, but is not limited to, one or more of oleylamine, dodecylamine, hexadecylamine, trioctylamine, tributylamine, ethylenediamine, propylenediamine, butyldiamine, pentanediamine, hexamethylenediamine, octyldiamine, decanediamine, aniline, benzylamine, dihexylamine, trioctylphosphine, dioctylamine, and octylamine; the set temperature is 40-60℃, the vacuum degree is 1mTorr-500mTorr, the reaction time is 0.5-1 hour, after purging with inert gas, the temperature is raised to 80-160℃, and the reaction time is 0.5-1 hour; after adding the organic anionic and organic cationic ligands, the temperature is heated to 170-200℃ and stirred for 0.5-1 hour. The concentration of precursor solution B is 0.005-0.874 g / mL.
[0023] Further, in step S3, the cation salt is one or more of rubidium carbonate, tin iodide, potassium carbonate, sodium carbonate, iron halide, manganese halide, nickel halide, copper halide, zinc halide, indium halide, strontium halide, and calcium halide; the amphoteric ligand is one or more of sulfobetaine, phosphocholine, lysine, arginine, serine, threonine, aspartic acid, iminodibenzoic acid, glutamic acid, tyrosine, tryptophan, glutathione, taurine, betaine, imidazole, pyrrolidone carboxylic acid, 3-indolepropionic acid, 4-aminobutyric acid, pentaminovalerate, 5-hydroxytryptophan, diethanolamine, and triethanolamine.
[0024] The preset temperature is room temperature - 200℃, the vacuum degree is 5mTorr-800mTorr, the specific stirring time is 40min-250min, the inert gas is nitrogen or argon, the stirring time after introducing the inert gas is 25min-175min, the temperature is raised to 70-300℃, and the reaction time is 25min-175min.
[0025] The nonpolar solvent is octadecene, the concentration of the amphoteric ligand is 0.025-0.173 mmol, and the concentration of precursor solution C is 0.005-0.847 g / mL. The volume ratio of the amphoteric ligand to the nonpolar solvent is 0.55-2.34.
[0026] Furthermore, in step S4, the reaction temperature of A and B is 100-220℃ and the reaction time is 5s-175min; the reaction temperature after the addition of precursor liquid C is 80-250℃ and the reaction time is 10s-180min.
[0027] Further, in step S5, the volume ratio of the antisolvent to the solvent is 0.2-2:1. The solvent is one of toluene, n-hexane, cyclohexane, benzene, and octane, and the antisolvent is one or more of methyl acetate, ethyl acetate, ethanol, and acetone. The concentration of the nanostructures in the perovskite is 3-48 mg / mL. Each centrifugation is performed at 800-10000 rpm for 1-30 min.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] Perovskite nanocrystals possess numerous advantages, including narrow emission peak width at half maximum (FWHM), high fluorescence quantum yield, tunable color, adjustable band gap, high quantum efficiency, strong photoluminescence, quantum confinement effect, and long carrier lifetime. Furthermore, they are low-cost, abundant, and readily synthesized into various compounds. Compared to traditional perovskite nanocrystals, hollow perovskite nanocrystals exhibit higher fluorescence quantum yield and greater fluorescence stability, while providing more active sites. This enhances adsorption capacity and reactivity, and their hierarchical shells effectively scatter incident light, thereby improving photocatalytic performance. More importantly, hollow perovskite nanocrystals can support a wider range of other substances, and the selection of materials with excellent charge separation and transport properties or the construction of heterostructures on the shells facilitates the separation of photogenerated electrons and holes, further improving related performance. Attached Figure Description
[0030] Figure 1 The image shows the transmission electron microscope (TEM) morphology of the hollow nanostructure obtained by the preparation method of the perovskite hollow nanocrystal with high fluorescence quantum yield according to the present invention.
[0031] Figure 2 This is a high-resolution transmission electron microscope image of the hollow nanostructure obtained by a method for preparing perovskite hollow nanocrystals with high fluorescence quantum yield according to the present invention.
[0032] Figure 3 The fluorescence absorption diagram of the hollow nanostructure obtained by the preparation method of high fluorescence quantum yield ultrastable perovskite hollow nanocrystals according to the present invention is shown.
[0033] Figure 4 The fluorescence quantum yield of hollow nanostructures obtained by a method for preparing ultrastable perovskite hollow nanocrystals with high fluorescence quantum yield according to the present invention;
[0034] Figure 5 The figure shows the fluorescence stability of the hollow nanostructures obtained by the high fluorescence quantum yield ultrastable perovskite hollow nanostructure preparation method according to the present invention. Detailed Implementation
[0035] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.
[0036] Example 1
[0037] A method for preparing perovskite hollow nanocrystals with high fluorescence quantum yield and ultrastability includes the following steps:
[0038] S1: Preparation of precursor solution A
[0039] 3 mmol of cesium acetate, 1.25 mL of oleic acid, 1 mL of octanoic acid and octadecene were thoroughly mixed. The mixing process was carried out under a tight vacuum of 100 mTorr at 150 °C for 60 min and the stirring speed was 200 rpm to obtain a clear and transparent cesium precursor solution with a concentration of 0.043 g / mL.
[0040] S2: Preparation of precursor solution B
[0041] 0.76 mmol of lead bromide, 1 mL of hydrobromic acid, and 10 mL of octadecene were thoroughly mixed. The mixture was evacuated for 30 min to obtain an anhydrous and oxygen-free environment with a vacuum degree of 50 mTorr. The reaction temperature was 60 °C and the reaction time was 45 min. Nitrogen gas was then introduced, and the temperature was raised to 120 °C and the reaction time was 60 min. Then, 1 mL of oleic acid and 1 mL of oleylamine were added, and the mixture was heated to 170 °C and stirred for 30 min to obtain a clear and transparent lead bromide precursor solution of 0.022 g / mL.
[0042] S3: Prepare precursor solution C
[0043] 0.54 mmol of rubidium carbonate was added to a mixed solvent consisting of 0.18 mmol of sulfobetaine, oleic acid, and 10 mL of octadecene. The mixture was evacuated for 0.5 h to obtain an anhydrous and oxygen-free environment with a vacuum of 129 mTorr. The mixture was stirred at 100 °C for 60 min, then nitrogen was introduced and stirred thoroughly for 30 min. The temperature was then increased to 120 °C and the reaction time was 60 min to obtain a clear and transparent rubidium carbonate precursor solution of 0.017 g / mL.
[0044] S4: Preparation of initial perovskite hollow nanocrystal solution
[0045] 1.5 mL of cesium precursor solution was injected into 10 mL of lead bromide precursor solution and reacted at 150 °C for 10 seconds. Then the temperature was increased to 180 °C, and 0.8 mL of rubidium carbonate precursor solution was added. The reaction was carried out at 180 °C for 30 seconds. The solution was then cooled to room temperature by an ice-water bath to obtain a hollow perovskite nanocrystal solution.
[0046] S5: Obtaining clean, hollow perovskite nanostructures
[0047] Take 5 mL of the solution prepared by LS4, add 10 mL of ethyl acetate to it, and centrifuge at 8000 rpm for 8 min. Then, add the obtained precipitate to toluene for further dispersion. Repeat the above centrifugation steps several times to completely remove the reaction waste generated during the synthesis of the perovskite hollow structure, and finally successfully obtain a clean perovskite nanostructure with a hollow structure.
[0048] Will be through Cs x TEM characterization of hollow Rb1-xPbBr3 nanocrystals revealed that the product morphology was a square frame with a side length of 10 nm and a thickness of 2 nm. Figure 1 ,2). Subsequently, high-resolution TEM characterization revealed that Cs x Rb 1- x The lattice parameter of the hollow PbBr3 nanocrystals is 0.42 nm. Figure 3 ), corresponding to the (110) crystal plane of perovskite, indicating that Cs x Rb 1- x Hollow nanocrystals in PbBr3 are cubic phases. Spectroscopic characterization revealed that Cs... x Rb 1-x The fluorescence peak of hollow PbBr3 nanocrystals is at 520 nm, with a full width at half maximum (FWHM) of 18 nm. Compared to traditional CsPbBr3 nanocrystals, Cs… x Rb 1-x Hollow nanocrystals of PbBr3 have a higher quantum yield. Figure 4 Subsequently, the purified CsPbBr3 quantum dot dispersion and the purified Cs from step 6) were combined. x Rb 1- x Hollow nanocrystalline dispersions of PbBr3 were dropped onto glass substrates, and the solvent was allowed to evaporate naturally to form thin films. These films were then immersed in water-filled beakers to test their water resistance and fluorescence stability. After 48 hours of immersion, the fluorescence of the CsPbBr3 quantum dot films was completely quenched. x Rb 1-xThe fluorescence intensity of hollow PbBr3 nanocrystals can still be maintained at over 90%. Figure 5 In summary, we have successfully prepared a high-fluorescence quantum yield, ultra-stable perovskite hollow nanocrystal, solving the problems of poor stability and low fluorescence quantum yield of perovskite nanocrystals.
[0049] Example 2
[0050] A method for preparing perovskite hollow nanocrystals with high fluorescence quantum yield and ultrastability includes the following steps:
[0051] S1: Preparation of precursor solution A
[0052] 2.8 mmol of cesium carbonate, 1.25 mL of oleic acid, 1 mL of octanoic acid and octadecene were thoroughly mixed. The mixing process was carried out under a tight 90 mTorr vacuum at 150 °C for 60 min with a stirring speed of 200 rpm to obtain a clear and transparent cesium precursor solution with a concentration of 0.052 g / mL.
[0053] S2: Preparation of precursor solution B
[0054] 0.84 mmol lead iodide, 1 mL hydrobromic acid and 10 mL octadecene were thoroughly mixed and the mixture was evacuated for 30 min to obtain an anhydrous and oxygen-free environment with a vacuum degree of 50 mTorr. The reaction temperature was 60 °C and the reaction time was 40 min. Nitrogen gas was then introduced and the temperature was raised to 150 °C and the reaction time was 45 min. Then 1 mL oleic acid and 1 mL oleylamine were added respectively, and the mixture was heated to 170 °C and stirred for 60 min to obtain a clear and transparent lead bromide precursor solution of 0.035 g / mL.
[0055] S3: Prepare precursor solution C
[0056] 0.54 mmol of tin iodide was added to a mixed solvent consisting of 0.18 mmol of pentaminovalerate, oleic acid, and 10 mL of octadecene. The mixture was evacuated for 30 min to obtain an anhydrous and oxygen-free environment with a vacuum degree of 100 mTorr. The mixture was stirred at 100 °C for 60 min, then nitrogen was introduced and stirred thoroughly for 30 min. The temperature was then increased to 120 °C and the reaction time was 60 min to obtain a clear and transparent 0.035 g / mL tin iodide precursor solution.
[0057] S4: Preparation of initial perovskite hollow nanocrystal solution
[0058] 1.5 mL of cesium precursor solution was injected into 10 mL of lead bromide precursor solution and reacted at 150 °C for 8 seconds. Then the temperature was increased to 180 °C, and 0.6 mL of tin iodide precursor solution was added. The reaction was carried out at 180 °C for 20 seconds. The solution was then cooled to room temperature by an ice-water bath to obtain a hollow perovskite nanocrystal solution.
[0059] S5: Obtaining clean, hollow perovskite nanostructures
[0060] Take 5 mL of the solution prepared by LS4, add 10 mL of ethyl acetate to it, and centrifuge at 6000 rpm for 10 min. Then, add the obtained precipitate to toluene for further dispersion. Repeat the above centrifugation steps several times to completely remove the reaction waste generated during the synthesis of the perovskite hollow structure, and finally successfully obtain a clean perovskite nanostructure with a hollow structure.
Claims
1. A perovskite hollow nanocrystalline Cs with high fluorescence quantum yield and ultrastable properties x The method for preparing Rb1-xPbBr3 is characterized by, Includes the following steps: S1: Prepare precursor solution A; Cesium acetate, oleic acid, octanoic acid and octadecene are thoroughly mixed. The mixing process must be carried out under the strict protection of inert gas or vacuum, and then the reaction is continuously stirred to successfully obtain a clear and transparent precursor liquid A. S2: Prepare precursor solution B; Lead bromide, hydrobromic acid, and octadecene were mixed and subjected to vacuum treatment to carry out the first reaction. Then, an inert gas was introduced, followed by raising the temperature to carry out the second reaction. Oleic acid and oleylamine were then added, and the mixture was heated and stirred for a certain period of time until the solution became clear and transparent, thus obtaining precursor solution B. S3: Prepare precursor solution C; Rubidium carbonate was added to a mixed solvent consisting of sulfobetaine, oleic acid, and octadecene, and a first stirring reaction was carried out. Then, an inert gas was introduced and a second stirring reaction was carried out. Subsequently, the temperature was increased to carry out a third reaction, thereby obtaining precursor solution C. S4: Preparation of initial perovskite hollow nanocrystal solution; Precursor solution A was added to precursor solution B and reacted at 100-220℃ for 5s-175min. Then the temperature was increased and precursor solution C was added. The reaction was carried out at 180-250℃ for 10s-180min. The solution was then rapidly cooled to room temperature to obtain the initial perovskite hollow nanocrystal solution. S5: Obtain a clean, hollow perovskite nanostructure; The antisolvent was added to the solution prepared in S4 and centrifuged. Then, the obtained precipitate was added to the solvent and dispersed again. The centrifugation steps were repeated multiple times to completely remove the reaction waste generated during the synthesis of the hollow perovskite structure. Finally, a clean hollow perovskite nanostructure was successfully obtained.
2. The perovskite hollow nanocrystal Cs with high fluorescence quantum yield as described in claim 1 x The method for preparing Rb1-xPbBr3 is characterized by, In step S1, the vacuum degree is 10 mTorr-600 mTorr, and the inert gas used in the reaction is nitrogen or argon; the stirring temperature is 45-230℃; the stirring time is 20-210 min; and the stirring speed is 200 rpm-800 rpm.
3. The perovskite hollow nanocrystal Cs with high fluorescence quantum yield as described in claim 1 x The method for preparing Rb1-xPbBr3 is characterized by, In step S2, the temperature of the first reaction is 40-60℃, the vacuum degree is 1mTorr-500mTorr, and the reaction time is 0.5-1 hour; after introducing an inert gas, the temperature is raised to 80-160℃ and the reaction is carried out for 0.5-1 hour; after adding oleic acid and oleylamine, the temperature is heated to 170-200℃ and stirred for 0.5-1 hour.
4. The perovskite hollow nanocrystal Cs with high fluorescence quantum yield as described in claim 1 x The method for preparing Rb1-xPbBr3 is characterized by, In step S3, the temperature of the first stirring is room temperature to 200℃, the vacuum degree during the first stirring is 5mTorr to 800mTorr, and the stirring time is 40min to 250min; the inert gas is nitrogen or argon; after the inert gas is introduced, the stirring time is 25min to 175min; the third reaction is: heating to 70-300℃, and the reaction time is 25min to 175min.
5. The perovskite hollow nanocrystal Cs with high fluorescence quantum yield as described in claim 1 x The method for preparing Rb1-xPbBr3 is characterized by, The volume ratio of antisolvent to solvent is (0.2-2):
1. The solvent is one of toluene, n-hexane, cyclohexane, benzene, or octane. The antisolvent is one or more of methyl acetate, ethyl acetate, ethanol, or acetone. The concentration of the perovskite hollow nanostructure is 3-48 mg / mL. The centrifugation speed is 800-10000 rpm and the centrifugation time is 1-30 min.