Preparation method of steel for mine truck spoke with thickness of more than 18mm

Through KR desulfurization, converter, LF refining, RH refining and air-rolling and cooling technology, combined with reasonable alloy composition design and rolling process, the problem of tissue uniformity in the thickness direction is solved, and steel for spokes of mine trucks with thickness specifications of more than 18mm is realized High strength and low temperature impact toughness meet the transportation needs of open-pit mines and reduce production costs.

CN119020667APending Publication Date: 2024-11-26BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411101483.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing steel for spokes for mining trucks with a thickness of more than 18mm is difficult to control the structure uniformity in the thickness direction, which cannot meet the large-scale development needs of open-pit mine transport trucks, and the production costs are high or the manufacturing costs are low but the performance is insufficient.

Method used

KR desulfurization, converter, LF refining and RH refining processes are used to form high-purity continuous casting blanks, and combined with controlled air-rolling and cooling technology, the heating and rolling temperature of the slab are controlled, the grain size is refined, the grain boundary area is increased, and the grain boundary area is improved through reasonable alloys. Component designs such as C: 0.06-0.08%, Si: 0.03-0.10%, Mn: 0.70-1.00%, Nb: 0.010-0.030%, Ti: 0.010-0.020%, cooling speed and temperature are controlled, and 2250mm hot rolling mill is used. Rolling.

Benefits of technology

It has achieved high strength, good plasticity and low-temperature impact toughness of steel for spokes of mine trucks above 18mm, and satisfies the yield strength of 380-480MPa, tensile strength of 460-600MPa, elongation ≥30, and low-temperature impact toughness ≥200J in -20℃ Performance requirements reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020667A_ABST
    Figure CN119020667A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of steel for a mine truck spoke with the thickness of more than 18mm. The preparation method comprises the following steps: a steelmaking process; a controlled rolling air cooling process; the steel comprises the following components in percentage by mass: 0.06%-0.08% of C, 0.03%-0.10% of Si, 0.70%-1.00% of Mn, less than or equal to 0.015% of P, less than or equal to 0.005% of S, 0.020%-0.050% of Alt, 0.010%-0.030% of Nb, 0.010%-0.020% of Ti, less than or equal to 70 ppm of N and the balance of Fe and inevitable impurities. Through reasonable alloying component design and a matched controlled rolling and controlled cooling process, the problem that the thickness center structure of a product is not uniform is effectively solved, the product has high strength and good plasticity and low-temperature impact toughness, and the service requirement under the severe environment on a mine is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled automobile steel preparation, and in particular relates to a method for preparing steel with a thickness of more than 18 mm for mining truck wheel spokes. Background Art

[0002] Wheels are an important part of the vehicle's driving system. They not only bear the vehicle's load and weight, but also bear lateral forces, driving (braking) torque, and various stresses generated during driving. Steel wheels are widely used in trucks due to their outstanding cost-effectiveness. Open-pit mining transport trucks mainly use steel wheels. In order to improve transportation efficiency, the load capacity of mining trucks continues to rise, which puts more stringent requirements on the thickness, size and performance of wheel steel. At present, the market is in urgent need of mining truck wheel steel products with a thickness of more than 18mm, a tensile strength of more than 460MPa, and good plasticity and low-temperature toughness. The greater the thickness of the product, the smaller its rolling compression ratio, the more uneven the cooling in the thickness direction, and the more difficult it is to control the uniformity of the microstructure in the thickness direction. The key issue in the preparation of thick-gauge high-strength wheel steel is how to achieve fine and uniform structure in the thickness direction.

[0003] The current status of production of thick-gauge high-strength steel for wheels is studied as follows:

[0004] Patent search A steel for mining wheels with good low-temperature impact performance and a production method. The method adopts a composition design of C: 0.06-0.10%, Si: ≤0.20%, Mn: 0.30-0.80%, P: ≤0.008%, S≤0.002%, Als: 0.045-0.065%, Nb: 0.025-0.045%, combined with a controlled rolling and controlled cooling process, and successfully developed a steel for mining wheels with good low-temperature impact performance. The product has a lower yield strength of ≥315MPa, a tensile strength of 490-610MPa, an elongation of A≥35%, and an impact energy AKV≥180 at -40℃. The method described in the patent adopts a low C+Mn+Nb composition system, mainly improving product performance through the expensive element Nb, and the product alloy manufacturing cost is relatively high; in addition, the maximum production thickness of its product is 18.0mm, which cannot fully meet the current development needs of mining trucks.

[0005] Patent search for a 500MPa spoke steel and its production method, the method uses: C: 0.05-0.09%, Si: 0.05-0.15%, Mn: 0.5-0.8%, P: ≤0.020%, S: ≤0.012%, Als: 0.015-0.060%, Ti: 0.025-0.05%, combined with controlled rolling and controlled cooling process, successfully developed 500MPa spoke steel. The method described in the patent uses a low C+Mn+Ti component system, which has the advantage of low manufacturing cost, but the production thickness range is 2.3-12.5mm, which cannot meet the current use requirements of mining trucks.

[0006] The patent search discloses a 600MPa grade thick hot-rolled spoke steel and its manufacturing method. The method adopts C: 0.06-0.10%, Si: 0.30-0.50%, Mn: 1.0-1.2%, P: 0.030-0.060%, S≤0.005%, Alt: 0.020-0.060%, Cr: 0.60-0.90%, Ti: ≤0.05%, N: ≤0.0060%, and combines the controlled rolling and controlled cooling process to obtain a 600MPa grade hot-rolled spoke steel. The advantages of the method described in the patent are high product strength, no expensive alloy elements are added, and the manufacturing cost is relatively low. However, the thickness of the finished product produced by the patent is 8.0-14.0mm, which cannot meet the large-scale development needs of mining trucks. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing steel for mining truck wheel spokes with a thickness of more than 18 mm, which solves the problem that the existing thickness of wheel steel cannot meet the large-scale development needs of open-pit mine transport trucks. At the same time, through reasonable alloying component design and matching controlled rolling and controlled cooling process, the problem of uneven structure in the center of the product thickness is effectively solved. The product has high strength while having good plasticity and low-temperature impact toughness, meeting the service requirements in the harsh environment of the mine. The product performance meets the following requirements: yield strength 380-480MPa, tensile strength 460-600MPa, elongation ≥30, -20℃ low-temperature impact toughness ≥200J.

[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for preparing steel for mining truck wheel spokes with a thickness of 18 mm or more, comprising:

[0010] Steelmaking process: KR desulfurization, converter, LF refining, RH refining and slab continuous casting; the smelting raw materials are processed in turn by KR hot metal desulfurization pretreatment, converter top and bottom blowing, LF refining, RH refining and continuous casting to form high-purity continuous casting billets; RH refining is the key process to control non-metallic inclusions inside the product, and the specific parameters are set as follows: vacuum degree requirement ≤2.6mbar, vacuum holding time ≥10min; during RH vacuum treatment, the circulating pure degassing time is guaranteed to be ≥7min; after the RH vacuum treatment, the calcium wire is fed for calcium treatment, and the soft blowing time is guaranteed to be greater than 8min after wire feeding;

[0011] Controlled rolling air cooling process:

[0012] The heating of the slab should consider both the full solid solution of the alloy elements and the prevention of excessive grain coarsening; therefore, the heating temperature of the slab is controlled at 1280-1200℃, and the soaking time is controlled at 20-30min;

[0013] The slab temperature is high during the rough rolling stage and is in the complete recrystallization zone. It is an important process for refining the coarse grains of the slab and a key link in achieving uniformity of the product thickness. The two necessary conditions for using recrystallization to refine the grain size are high temperature and large deformation. Therefore, the rough rolling of the slab adopts 3+3 rolling for a total of 6 passes, and the reduction of the first pass is controlled at 35-40mm.

[0014] Avoid partial recrystallization zone in the finishing rolling stage, and control rolling in the non-recrystallization zone; partial recrystallization zone is prone to mixed crystal structure, and the thickness center problem is more serious; rolling in the non-recrystallization zone can lengthen the grain size, increase the grain boundary area, and provide more nucleation points for subsequent phase transformation, thereby achieving the purpose of refining the grain size; increasing the reduction in the finishing rolling stage and lower final rolling temperature are also helpful to increase the grain boundary area and nucleation points; therefore, the intermediate billet temperature is controlled at ≤980℃, the intermediate billet thickness is controlled at 52-60mm, and the final rolling temperature is controlled at 840-870℃;

[0015] If the cooling speed of the steel coil is too slow, the size of the refined grains will grow. If the cooling speed is too fast, the center layer of the product will not be cooled properly due to its large thickness, and then the "red return" problem will occur. To prevent such problems, the cooling speed is controlled at 15-30℃ / s and the coiling temperature is controlled at 540-580℃.

[0016] The composition of the ultra-thick specification open-pit mine wheel spoke steel is as follows, by mass percentage: C: 0.06-0.08%, Si: 0.03-0.10%, Mn: 0.70%-1.00%, P: ≤0.015%, S: ≤0.005%, Alt: 0.020%-0.050%, Nb: 0.010-0.030%, Ti: 0.010%-0.020%, N: ≤70ppm, and the balance is Fe and unavoidable impurities.

[0017] Furthermore, a 2250mm hot rolling mill is used for rolling.

[0018] Furthermore, the thickness of the continuous casting slab is 230 mm.

[0019] Furthermore, the composition of the ultra-thick specification open-pit mine wheel spoke steel is, by mass percentage, C: 0.07%, Si: 0.09%, Mn: 0.91%, P: 0.012%, S: 0.003%, Alt: 0.02%, Nb: 0.023%, Ti: 0.013%, N: 45ppm, and the remainder is Fe and unavoidable impurities.

[0020] Furthermore, the composition of the ultra-thick specification open-pit mine wheel spoke steel is, by mass percentage, C: 0.06%, Si: 0.08%, Mn: 0.89%, P: 0.014%, S: 0.004%, Alt: 0.03%, Nb: 0.021%, Ti: 0.010%, N: 40ppm, and the remainder is Fe and unavoidable impurities.

[0021] Furthermore, the prepared ultra-thick open pit mine wheel spoke steel meets the following requirements: yield strength R el 426-447MPa, tensile strength R m It is 510-530MPa.

[0022] Furthermore, the prepared ultra-thick specification open-pit mine wheel spoke steel meets the following requirements: elongation 34-36%.

[0023] Furthermore, the prepared ultra-thick specification open-pit mine wheel spoke steel meets the following requirements: low temperature impact toughness at -20°C is 200-350J.

[0024] The main elements were chosen for the following reasons:

[0025] C: Carbon is a cheap solid solution strengthening element, but increasing carbon will reduce plastic toughness and formability. This product is mainly used to process automobile wheels, which requires a large degree of spinning deformation, so the material is required to have good cold forming performance while meeting the strength requirements. If its content is too little, it is necessary to add alloy elements to improve the strength of the product, resulting in increased product manufacturing costs. If its content is too much, the material's formability cannot be met. Comprehensive consideration is given to limit its content to 0.06-0.08%.

[0026] Si: Silicon is a deoxidizing element and can also play a role in solid solution strengthening, but Si easily causes red oxides to form on the surface of the steel strip, affecting the surface quality and fatigue performance of the product. Taking comprehensive considerations, its content is limited to 0.03-0.10%.

[0027] Mn: Manganese can be infinitely substituted with iron for solid solution, and is the most cost-effective solid solution strengthening element after C. However, if the Mn content is too high, it is easy to cause slab segregation, which is inherited to the finished product to form a harder center segregated pearlite banded structure. This problem is more serious, especially for thick specifications. The compression ratio is small and the cooling rate at the center of the thickness is low. The pearlite banded structure seriously deteriorates the formability and fatigue properties of the product. Considering all factors, its content is limited to 0.70% to 1.00%.

[0028] P, S: Phosphorus and sulfur are unavoidable harmful elements in steel. The lower their content, the better the product performance. However, controlling too low will increase production costs. Considering comprehensively, their contents are limited to P≤0.015% and S≤0.005% respectively.

[0029] Alt: Aluminum is added for deoxidation. When the aluminum content is insufficient, it cannot exert its effect. When the aluminum content is too high, the ductility deteriorates. Considering all factors, its content is limited to 0.020% to 0.050%.

[0030] Nb: Niobium is the most effective element in refining grain size among alloy elements, and also has precipitation strengthening effect. However, Nb alloy is expensive. If the content is too high, it will increase manufacturing cost on the one hand, and cause mixed crystal problem on the other hand. Adding Nb element is one of the key processes to solve the problem of coarse grains in the center of thick-gauge wheel steel. After comprehensive consideration, its content is limited to 0.010-0.030%.

[0031] Ti: Titanium has the effects of refining grain size and precipitation strengthening. Titanium refines grain size mainly by combining with N element at high temperature to precipitate fine TiN to inhibit the growth of high-temperature austenite grains. The smaller the TiN size, the more fully the high-temperature austenite grain size is refined. The precipitation strengthening effect of titanium is mainly achieved by precipitating fine TiC on the ferrite matrix to hinder dislocation movement. The Ti content has an important influence on the refinement of grain size. If the content is small, Ti is consumed by O and N during the steelmaking process and cannot play a role. If the content is high, the TiN size will increase and the effect of refining grain size will be weakened, and its strengthening effect will be significantly improved. The main purpose of adding Ti element in the method described in this patent is to refine the grain size of the product and solve the problem of coarse grains in the center of the thickness of thick-gauge wheel steel. Taking comprehensive considerations, its content is limited to 0.010-0.020%.

[0032] N: The nitrogen content will affect the TiN size and thus the product grain size. Taking comprehensive considerations, its content is limited to ≤70ppm.

[0033] Compared with the prior art, the beneficial technical effects of the present invention are:

[0034] The ultra-thick spoke steel with a thickness of 18mm or above solves the problem that the existing wheel steel thickness cannot meet the large-scale development needs of open-pit mine transport trucks, and has a broad application prospect. In addition, the product adopts low-cost design and manufacturing, and has significant efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The present invention will be further described below in conjunction with the accompanying drawings.

[0036] Figure 1 The metallographic structure at the 1 / 4 and 1 / 2 positions in the thickness direction of the steel strip in Example 1 of the present invention is polygonal ferrite + a small amount of pearlite. The structure control in the thickness direction is basically the same, the grains are small and uniform, and the grain size rating is 11.0. DETAILED DESCRIPTION

[0037] The following examples are used to specifically illustrate the present invention. These examples are only general descriptions of the present invention and do not limit the present invention.

[0038] In order to further understand the present invention, two groups of steel compositions and preparation method examples for open-pit mine wheel spokes with ultra-thick specifications of 18 mm or more according to the present invention are provided for illustration.

[0039] The chemical composition control of the embodiment is shown in Table 1, the heating-rolling-cooling parameter control of the embodiment is shown in Table 2, and the mechanical properties of the embodiment are shown in Table 3.

[0040] Table 1 Chemical composition of steel in the example (wt%)

[0041]

[0042]

[0043] Table 2 Example steel process system

[0044]

[0045] Table 3 Mechanical properties of example steel

[0046]

[0047] It can be seen from the examples that the yield strength Rel of the steel strip of the present invention is 426-447MPa, the tensile strength Rm is 510-530MPa, the elongation is 34-36%, and the -20℃ low temperature impact toughness is 200-350J, which meets the customer requirements.

[0048] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing steel for mining truck spokes with a thickness of 18 mm or more, characterized in that: include: Steelmaking process: KR desulfurization, converter, LF refining, RH refining and slab continuous casting; the smelting raw materials are processed in turn by KR hot metal desulfurization pretreatment, converter top and bottom blowing, LF refining, RH refining and continuous casting to form high-purity continuous casting billets; RH refining is the key process to control non-metallic inclusions inside the product, and the specific parameters are set as follows: vacuum degree requirement ≤2.6mbar, vacuum holding time ≥10min; during RH vacuum treatment, the circulating pure degassing time is guaranteed to be ≥7min; after the RH vacuum treatment, the calcium wire is fed for calcium treatment, and the soft blowing time is guaranteed to be greater than 8min after wire feeding; Controlled rolling air cooling process: The slab heating temperature is controlled at 1280-1200℃, and the soaking time is controlled at 20-30min; The rough rolling of slab adopts 3+3 rolling, a total of 6 passes, and the reduction of the first pass is controlled at 35-40mm; The intermediate billet temperature is controlled at ≤980℃, the intermediate billet thickness is controlled at 52-60mm, and the final rolling temperature is controlled at 840-870℃; The cooling rate is controlled at 15-30℃ / s, and the coiling temperature is controlled at 540-580℃; The composition of the ultra-thick specification open-pit mine wheel spoke steel is as follows, by mass percentage: C: 0.06-0.08%, Si: 0.03-0.10%, Mn: 0.70%-1.00%, P: ≤0.015%, S: ≤0.005%, Alt: 0.020%-0.050%, Nb: 0.010-0.030%, Ti: 0.010%-0.020%, N: ≤70ppm, and the balance is Fe and unavoidable impurities.

2. The method for preparing steel for mining truck wheel spokes with a thickness of 18 mm or more according to claim 1, characterized in that: It is rolled using a 2250mm hot rolling mill.

3. The method for preparing steel for mining truck wheel spokes with a thickness of 18 mm or more according to claim 1, characterized in that: The thickness of the continuous casting billet is 230 mm.

4. The method for preparing steel for mining truck wheel spokes with a thickness of 18 mm or more according to claim 1, characterized in that: The composition of the ultra-thick specification open-pit mine wheel spoke steel is, by mass percentage, C: 0.07%, Si: 0.09%, Mn: 0.91%, P: 0.012%, S: 0.003%, Alt: 0.02%, Nb: 0.023%, Ti: 0.013%, N: 45ppm, and the remainder is Fe and unavoidable impurities.

5. The method for preparing steel for mining truck wheel spokes with a thickness of 18 mm or more according to claim 1, characterized in that: The composition of the ultra-thick specification open-pit mine wheel spoke steel is, by mass percentage, C: 0.06%, Si: 0.08%, Mn: 0.89%, P: 0.014%, S: 0.004%, Alt: 0.03%, Nb: 0.021%, Ti: 0.010%, N: 40ppm, and the remainder is Fe and unavoidable impurities.

6. The method for preparing steel for mining truck wheel spokes with a thickness of 18 mm or more according to claim 1, characterized in that: The prepared ultra-thick open pit mine wheel spoke steel meets the following requirements: yield strength R el 426-447MPa, tensile strength R m It is 510-530MPa.

7. The method for preparing steel for mining truck wheel spokes with a thickness of 18 mm or more according to claim 1, characterized in that: The prepared ultra-thick specification open-pit mine wheel spoke steel meets the following requirements: elongation 34-36%.

8. The method for preparing steel for mining truck wheel spokes with a thickness of 18 mm or more according to claim 1, characterized in that: The prepared ultra-thick specification open-pit mine wheel spoke steel meets the following requirements: low-temperature impact toughness of -20°C is 200-350J.