Nickel-saving high-heat-resistance cast steel and preparation method thereof

Through microalloyation technology and polytetrafluoroethylene/graphene oxide coating, the problems of unstable performance and high cost of heat-resistant cast steel under high temperature conditions are solved, and high performance, high temperature stability and economical nickel-saving high Heat-resistant cast steel material.

CN119020672APending Publication Date: 2024-11-26JIANGYIN HONGCHUANG CASTING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411124163.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing heat-resistant cast steels have unstable performance under high temperature conditions, poor high-temperature mechanical properties, insufficient thermal fatigue resistance, and high cost, which cannot meet the needs of high-temperature exhaust manifolds.

Method used

Using microalloyation technology, by smelting 304 scrap steel, adding iron-chromium alloy, nickel, iron-molybdenum alloy and other alloys, SiCaBa and silicon-manganese alloys as deoxidants, adjusting the C and Cr contents to form ZG40Cr25Ni12Si2V high heat-resistant cast steel, and on the surface Coated with PTFE/graphene oxide coating to improve high temperature oxidation and corrosion resistance.

Benefits of technology

High heat-resistant cast steel that operates stably at a high temperature of 1100℃ is achieved, which reduces nickel content and reduces costs, while improving the comprehensive performance of the material, meeting the application needs of high-temperature exhaust manifolds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004995893420000081
    Figure BDA0004995893420000081
  • Figure BDA0004995893420000082
    Figure BDA0004995893420000082
  • Figure BDA0004995893420000091
    Figure BDA0004995893420000091
Patent Text Reader

Abstract

The invention relates to the technical field of alloys, in particular to nickel-saving high-heat-resistance cast steel and a preparation method thereof. Comprising the following steps that S1, material smelting is conducted, specifically, (1) 304 scrap steel is molten, and iron-chromium alloy, nickel, iron-molybdenum alloy and iron-cobalt alloy are sequentially added for smelting; adding an iron-niobium alloy and an iron-vanadium alloy into the furnace 15-20 minutes before discharging, and continuously smelting; molten steel A is obtained; (2) adding a deoxidizing agent A into the furnace before the molten steel A is tapped for 5-6 minutes; deoxidizing in the furnace, and removing slag for more than or equal to 3 times; molten steel B is obtained; (3) adding an iron-tellurium alloy, an iron-cerium alloy and a deoxidizing agent B into the molten steel B before tapping; deoxidizing in the ladle; discharging to obtain molten steel; s2, precoated sand is made into a shell; dip-coating the surface of the shell layer with paint, and baking; and molten steel is poured in the cast steel, forming is conducted, and the nickel-saving high-heat-resistance cast steel is obtained. The prepared nickel-saving high-heat-resistance cast steel has good high-temperature mechanical properties, thermal fatigue resistance, erosion resistance and growth resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of microalloying, in particular to a nickel-saving high-heat-resistant cast steel and a preparation method thereof. Background Art

[0002] As people's environmental awareness continues to increase, relevant automobile emission regulations are constantly upgraded, and the emission requirements for automobile exhaust are becoming more and more stringent. Due to the promotion and implementation of strict vehicle emission standards across the country, it has become an inevitable trend to promote automobile manufacturers to carry out technological innovation and develop low-energy vehicles. With the introduction of new technologies, the operating temperature of the engine has increased significantly, which has led to an increase in the gas emission temperature, some of which are close to or even exceed 1000℃. Therefore, higher requirements are placed on the application of heat-resistant materials for exhaust manifolds.

[0003] Among them, heat-resistant cast steel has become an indispensable key material in exhaust manifolds due to its excellent high-temperature mechanical properties and heat fatigue resistance. In the existing technology, high-Ni ductile iron is usually used to prepare heat-resistant cast iron alloy materials, and the maximum operating temperature can reach 950°C, but the cost is high, and with the development of technology, the maximum operating temperature of 950°C can no longer fully meet the demand, so it is not suitable for use in actual production applications.

[0004] Therefore, it is particularly necessary to solve the above-mentioned defects and prepare a nickel-saving high heat-resistant cast steel. Summary of the invention

[0005] The object of the present invention is to provide a nickel-saving high heat-resistant cast steel and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A method for preparing nickel-saving high-heat-resistant cast steel comprises the following steps:

[0008] S1: Material smelting:

[0009] (1) Melting 304 scrap steel, adding iron-chromium alloy, nickel, iron-molybdenum alloy, and iron-cobalt alloy in sequence for smelting; adding iron-niobium alloy and iron-vanadium alloy into the furnace 15 to 20 minutes before being taken out of the furnace and continuing smelting; obtaining molten steel A;

[0010] (2) adding deoxidizer A into the furnace 5 to 6 minutes before steel tapping; performing deoxidation treatment in the furnace, and performing slag removal for ≥ 3 times; and obtaining molten steel B;

[0011] (3) adding iron-tellurium alloy, iron-cerium alloy and deoxidizer B into the ladle before steel tapping; performing deoxidation treatment in the ladle; and tapping to obtain molten steel;

[0012] S2: Forming a shell with coated sand; coating the surface of the shell with paint and baking it; pouring molten steel inside the shell to form it, thereby obtaining nickel-saving and high-heat-resistant cast steel.

[0013] More optimally, the nickel-saving high heat-resistant cast steel includes the following elements, calculated by mass percentage: 0.3% to 0.5% carbon, 1.0% to 2.5% silicon, manganese ≤2%, phosphorus ≤0.04%, sulfur ≤0.03%, 24.0% to 28.0% chromium, 0.15% to 0.2% molybdenum, 11.0% to 14.0% nickel, 0.14% to 0.20% cobalt, 0.15% to 0.20% vanadium, 0.35% to 0.45% niobium, tellurium ≤0.005%, cerium ≤0.05%, and the rest is iron.

[0014] Among them, due to the problems of unstable performance, poor high-temperature mechanical properties, insufficient heat fatigue resistance, etc. of ordinary heat-resistant cast steel under high temperature conditions, it is easily affected by changes in external conditions. At the same time, it also lacks properties such as oxidation resistance and corrosion resistance. Therefore, in the scheme, the microalloying method is adopted to achieve intergranular strengthening, resistance to high-temperature oxidation, high-temperature corrosion and creep resistance, so that the material can operate stably at a working temperature of up to 1100°C. At the same time, the key problem of chromium depletion is also solved. By adjusting the C and Cr contents and combining microalloying technology, a nickel-saving high-heat-resistant cast steel in this application is developed, referred to as ZG40Cr25Ni12Si2V (A), which is a new type of multi-element alloyed heat-resistant cast steel material, which effectively improves the comprehensive performance of heat-resistant cast steel.

[0015] More optimally, during the material smelting process, the smelting temperature is 1700-1710°C and the furnace outlet temperature is 1680-1700°C.

[0016] More optimally, the process parameters of the coated sand shell making are set as follows: heating temperature is 200-300°C, curing time is 100-300S, and sand shooting pressure is 0.4-0.6MPa;

[0017] During the dipping process: the concentration of the coating is 60°Bé;

[0018] The baking process parameters are set as follows: baking temperature is 210-230° C., and baking time is 60-120 min;

[0019] The process parameters for pouring the molten steel are set as follows: the pouring temperature is 1580-1520°C.

[0020] More optimally, the deoxidizer A includes SiCaBa; the amount of the deoxidizer A added accounts for 0.2-0.3wt% of the molten steel A.

[0021] More optimally, the deoxidizer B includes ReSiCaMn; the amount of the deoxidizer B added accounts for 0.1-0.2wt% of the molten steel B.

[0022] More optimally, the deoxidizer A also includes silicon-manganese alloy; the mass ratio of SiCaBa to silicon-manganese alloy is (2-2.5):1.

[0023] In the scheme, SiCaBa is introduced as a deoxidizer during the material smelting process to improve the quality of molten steel; at the same time, in a further scheme, silicon-manganese alloy is introduced to cooperate with SiCaBa for deoxidation, which has a better effect than a single deoxidizer. Among them, SiCaBa has a strong deoxidation ability and can quickly combine with oxygen in molten steel to form a stable oxide, thereby effectively reducing the oxygen content in molten steel. In addition, it has the effect of refining grains, which helps to improve the mechanical properties and heat resistance of cast steel; while silicon-manganese alloy has a composite deoxidation and alloying effect, and silicon can improve the heat resistance and oxidation resistance of steel; manganese can increase the strength and toughness of steel, while improving the cutting performance of steel, so that it has suitable processing and forming performance. In addition, during the deoxidation process, silicon-manganese alloy can also effectively reduce the content of gas (such as hydrogen, nitrogen) and inclusions (such as sulfides, oxides) in steel, thereby improving the quality of cast steel.

[0024] In a further embodiment, the surface of the nickel-saving high heat-resistant cast steel is uniformly coated with a polytetrafluoroethylene / graphene oxide coating to obtain a nickel-saving high heat-resistant cast steel B; comprising the following steps:

[0025] S1: (1) adding polytetrafluoroethylene to a tert-butyl lithium / ethylenediamine solution, adding 4-vinylaniline, stirring at 70-80°C for 8-10 hours; washing and drying to obtain polytetrafluoroethylene A; (2) adding polytetrafluoroethylene A to deionized water, adding an epoxy silane coupling agent, stirring at 60-70°C for 30-60 minutes; filtering, and drying at 100-110°C to obtain modified PTFE; (3) adding graphene oxide to anhydrous ethanol for dispersion, then adding modified PTFE, deionized water and hydrochloric acid, ultrasonically dispersing for 1-2 hours, stirring at 50-60°C for 2-5 hours; washing, drying and grinding to obtain modified graphene oxide;

[0026] S2: adding ceramic sol, polytetrafluoroethylene and modified graphene oxide into ethanol in sequence, homogenizing and sieving to obtain a coating;

[0027] S3: uniformly coating the surface of the nickel-saving high heat-resistant cast steel with coating; keeping the surface at 250-300°C for 0.3-0.7 hours; keeping the surface at 350-400°C for 0.5-1 hours to obtain a polytetrafluoroethylene / graphene oxide coating; thereby, obtaining the nickel-saving high heat-resistant cast steel B.

[0028] In a further scheme, in order to further improve the corrosion resistance of the nickel-saving high heat-resistant cast steel, a polytetrafluoroethylene / graphene oxide coating is evenly coated on its surface to obtain nickel-saving high heat-resistant cast steel B.

[0029] A uniform coating is formed with ceramic sol, polytetrafluoroethylene, and modified graphene oxide to form effective protection. The introduced graphene oxide can effectively enhance the heat resistance and heat dissipation of cast steel, but it has compatibility issues, so modified PTET is used for modification in the scheme; among them, PTFE is grafted and modified by introducing 4-vinylaniline, so that polytetrafluoroethylene obtains more active sites and can participate in more chemical reactions, thereby improving its chemical reaction activity, and then it is grafted and modified by amino and epoxy silane coupling agents. The introduction of silane coupling groups not only enhances the compatibility of polytetrafluoroethylene with other materials, but also improves its interfacial bonding strength; finally, graphene oxide is added to produce a "π-π conjugated effect", and the non-covalent bond interaction further enhances the bonding strength between modified polytetrafluoroethylene and graphene oxide, improves the overall anti-corrosion performance of the coating, and makes it have better dispersibility and higher thermal stability.

[0030] More optimally, the raw materials of the tert-butyl lithium / ethylenediamine solution include the following components: 2.5 to 3 parts of tert-butyl lithium, 1 to 1.3 parts of ethylenediamine, and 15 to 20 parts of diethyl ether, by mass.

[0031] The raw materials of the polytetrafluoroethylene A include the following components: 2 to 3 parts by mass of tert-butyl lithium / ethylenediamine solution, 20 to 30 parts of polytetrafluoroethylene, and 15 to 20 parts of 4-ethyleneaniline;

[0032] The raw materials of the modified PTFE include the following components: 15 to 20 parts of polytetrafluoroethylene A, 4 to 6 parts of epoxy silane coupling agent, and 30 to 40 parts of deionized water, calculated by mass.

[0033] The raw materials of the modified graphene oxide include the following components: by mass, 10 to 12 parts of graphene oxide, 20 to 30 parts of anhydrous ethanol, 10 to 12 parts of modified PTFE, 25 to 30 parts of deionized water, and 1.5 to 2 parts of hydrochloric acid;

[0034] The raw materials of the coating include the following components: by weight, 30 to 35 parts of ceramic sol, 5 to 6 parts of polytetrafluoroethylene, 10 to 12 parts of modified graphite oxide, and 40 to 45 parts of ethanol.

[0035] More optimally, a method for preparing nickel-saving high heat-resistant cast steel obtains nickel-saving high heat-resistant cast steel or nickel-saving high heat-resistant cast steel B.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] (1) By limiting the metal elements in the nickel-saving high heat-resistant cast steel, paralleling and micro-alloying methods, deoxidizer A and deoxidizer B are introduced according to different frequency bands to effectively achieve intergranular strengthening, thereby obtaining a nickel-saving high heat-resistant cast steel with resistance to high temperature oxidation, high temperature corrosion and creep;

[0038] (2) In addition, in order to further improve the protectiveness and surface corrosion resistance of nickel-saving high-heat-resistant cast steel, the scheme further introduces polytetrafluoroethylene / graphene oxide coating to improve its comprehensive surface performance and expand its application areas. DETAILED DESCRIPTION

[0039] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] It should be noted that, in the following specific embodiments, parts are parts by mass, and there is no special restriction on the purchase manufacturers of all raw materials involved in the present invention. Exemplary examples include: the particle size of silicon manganese alloy is 2-12 mm, the impurity content is 0.01%, and the brand is Fenglan Metallurgy; the purity of polytetrafluoroethylene (PTFE) is 99%, the item number is TE3859, purchased from Dongwan Gaochuang Plastic Raw Materials Co., Ltd.; the epoxy silane coupling agent is KH-560, and its purity is 98%; the item number of graphene oxide is 180110092632, and the brand is Kramar; ceramic sol 30%, CAS number 14808-60-7, purchased from Zhejiang Jiupeng New Materials Co., Ltd.

[0041] The grade of iron-chromium alloy (Fe-Cr) is FeCr55C6, the grade of iron-molybdenum alloy (Fe-Mo) is FeMo55-A, the grade of iron-cobalt alloy (Fe-Co) is electrolytic cobalt Co99.5, the grade of iron-niobium alloy (Fe-Nb) is FeNi60-A, the grade of iron-vanadium alloy (Fe-V) is FeV60-A, the grade of deoxidizer A is SiCaBa, the grade of iron-tellurium alloy (Fe-Te) is pure tellurium Te99, the grade of iron-cerium alloy (Fe-Ce) is pure cerium Ce99, and the grade of deoxidizer B is ReSiCaMn;

[0042] The coated sand used has been inspected, and the inspection standards are: particle size 70-140, silicon content ≥96%, hot tensile strength 1.4-1.5Mpa, cold tensile strength 2.8-3Mpa, cold bending strength ≥6Mpa, gas evolution ≤13ml / g, loss on ignition 1.1%-2.0%;

[0043] The chemical composition of ZG40Cr25Ni12Si2V(A), by mass fraction, includes: 0.31% carbon, 1.01% silicon, 1.05% manganese, 0.030% phosphorus, 0.015% sulfur, 25.8% chromium, 12.5% ​​nickel, and the rest is iron.

[0044] The chemical composition of QTANi35Si5Cr2, by mass fraction, includes: 2.08% carbon, 5.1% silicon, 0.15% manganese, 0.03% phosphorus, 0.012% sulfur, 1.8% chromium, 35.2% nickel, and the rest is iron.

[0045] The chemical composition of 1.4848, by mass fraction, includes: 0.35% carbon, 1.23% silicon, 1.08% manganese, 0.035% phosphorus, 0.02% sulfur, 25.2% chromium, 20.3% nickel, and the rest is iron.

[0046] The coating for the coated sand shell is an alcohol-based casting coating, the model is ISOMOL300, and the brand is FOSECO.

[0047] Embodiment 1: A method for preparing nickel-saving high heat-resistant cast steel, comprising the following steps:

[0048] Step 1: Material smelting: (1) During the material smelting process, the temperature is set to 1705°C, 304 scrap steel is melted, and then iron-chromium alloy, nickel, iron-molybdenum alloy, and iron-cobalt alloy are added in sequence for smelting for 2.5 hours; iron-niobium alloy and iron-vanadium alloy are added within 17 minutes before the steel is discharged from the furnace and the smelting is continued for 1.5 hours; molten steel A is obtained; (2) 0.25wt% SiCaBa deoxidizer is added to the molten steel A in the furnace 5.5 minutes before the steel is discharged; the steel is deoxidized in the furnace for 4 hours; the slag is removed 5 times; molten steel B is obtained; (3) iron-tellurium alloy, iron-cerium alloy, and 0.15wt% ReSiCaMn deoxidizer are added to the molten steel B in the ladle before the steel is discharged; the steel is deoxidized in the ladle for 3.5 hours; the steel is discharged from the furnace when the temperature reaches 1690°C to obtain molten steel;

[0049] Step 2: Make the shell of the coated sand: solidify at 250°C for 200S, make the shell under 0.5MPa pressure, dip-coat the shell surface at a coating concentration of 60°Bé, and bake at 220°C for 90min; when the temperature reaches 1550°C, pour molten steel inside for 45min to form, and obtain nickel-saving high heat-resistant cast steel, referred to as ZG40Cr25Ni12Si2V(A).

[0050] Comparative Example 1: QTANi35Si5Cr2 was purchased.

[0051] Comparative Example 2: 1.4848 was purchased.

[0052] Example 2: Based on Example 1, a polytetrafluoroethylene / graphene oxide coating is further used; specifically comprising the following steps:

[0053] Step 1: Material smelting: (1) During the material smelting process, the temperature is set to 1705°C, 304 scrap steel is melted, and then iron-chromium alloy, nickel, iron-molybdenum alloy, and iron-cobalt alloy are added in sequence for smelting for 2.5 hours; iron-niobium alloy and iron-vanadium alloy are added within 17 minutes before the steel is discharged from the furnace and the smelting is continued for 1.5 hours; molten steel A is obtained; (2) 0.25wt% SiCaBa deoxidizer is added to the molten steel A in the furnace 5.5 minutes before the steel is discharged; the steel is deoxidized in the furnace for 4 hours; the slag is removed 5 times; molten steel B is obtained; (3) iron-tellurium alloy, iron-cerium alloy, and 0.15wt% ReSiCaMn deoxidizer are added to the molten steel B in the ladle before the steel is discharged; the steel is deoxidized in the ladle for 3.5 hours; the steel is discharged from the furnace when the temperature reaches 1690°C to obtain molten steel;

[0054] Step 2: Make the shell from the coated sand: solidify at 250°C for 200S, make the shell under 0.5MPa pressure, dip-coat the shell surface with a coating concentration of 60°Bé, and bake at 220°C for 90min; when the temperature reaches 1550°C, pour molten steel inside for 45min to form the shell, and obtain nickel-saving high heat-resistant cast steel;

[0055] Step 3: (1) Add 25 parts of polytetrafluoroethylene to 2.5 parts of tert-butyl lithium / ethylenediamine solution, add 18 parts of 4-ethyleneaniline, stir at 75°C for 9 hours; wash and dry to obtain polytetrafluoroethylene A; (2) Add 18 parts of polytetrafluoroethylene A to 35 parts of deionized water, add 5 parts of epoxy silane coupling agent, stir at 65°C for 45 minutes; filter, and dry at 105°C to obtain modified PTFE; (3) Add 11 parts of graphene oxide to 25 parts of anhydrous ethanol for dispersion, then add 11 parts of modified PTFE, 28 parts of deionized water and 1.5 parts of hydrochloric acid, ultrasonically disperse for 1.5 hours, and stir at 55°C for 4 hours; wash, dry, and grind to obtain modified graphene oxide;

[0056] Step 4: 32 parts of ceramic sol, 5.5 parts of polytetrafluoroethylene, and 11 parts of modified graphene oxide were added to 42 parts of ethanol in sequence, homogenized for 30 minutes, and passed through a 300-mesh sieve to obtain a coating;

[0057] Step 5: uniformly apply the coating on the surface of the nickel-saving and high-heat-resistant cast steel; keep it warm at 275°C for 0.5 hours; keep it warm at 375°C for 0.8 hours to obtain a polytetrafluoroethylene / graphene oxide coating; and obtain the nickel-saving and high-heat-resistant cast steel.

[0058] Example 3: Based on Example 2: Using a composite formula in the deoxidizer; specifically comprising the following steps:

[0059] Step 1: Material smelting: (1) During the material smelting process, the temperature is set to 1705°C, 304 scrap steel is melted, and then iron-chromium alloy, nickel, iron-molybdenum alloy, and iron-cobalt alloy are added in sequence for smelting for 2.5 hours; iron-niobium alloy and iron-vanadium alloy are added within 17 minutes before the steel is discharged from the furnace and the steel is smelted for 1.5 hours; molten steel A is obtained; (2) SiCaBa and silicon-manganese alloy deoxidizers with a mass ratio of 2.2:1 are added to the molten steel A in the furnace 5.5 minutes before the steel is discharged; the steel is deoxidized in the furnace for 4 hours; the slag is removed 5 times; molten steel B is obtained; (3) iron-tellurium alloy, iron-cerium alloy, and 0.15wt% ReSiCaMn deoxidizer are added to the molten steel B in the ladle before the steel is discharged; the steel is deoxidized in the ladle for 3.5 hours; the steel is discharged from the furnace when the temperature reaches 1690°C to obtain molten steel;

[0060] Step 2: Make the shell from the coated sand: solidify at 250°C for 200S, make the shell under 0.5MPa pressure, dip-coat the shell surface with a coating concentration of 60°Bé, and bake at 220°C for 90min; when the temperature reaches 1550°C, pour molten steel inside for 45min to form the shell, and obtain nickel-saving high heat-resistant cast steel;

[0061] Step 3: (1) Add 25 parts of polytetrafluoroethylene to 2.5 parts of tert-butyl lithium / ethylenediamine solution, add 18 parts of 4-ethyleneaniline, stir at 75°C for 9 hours; wash and dry to obtain polytetrafluoroethylene A; (2) Add 18 parts of polytetrafluoroethylene A to 35 parts of deionized water, add 5 parts of epoxy silane coupling agent, stir at 65°C for 45 minutes; filter, and dry at 105°C to obtain modified PTFE; (3) Add 11 parts of graphene oxide to 25 parts of anhydrous ethanol for dispersion, then add 11 parts of modified PTFE, 28 parts of deionized water and 1.5 parts of hydrochloric acid, ultrasonically disperse for 1.5 hours, and stir at 55°C for 4 hours; wash, dry, and grind to obtain modified graphene oxide;

[0062] Step 4: 32 parts of ceramic sol, 5.5 parts of polytetrafluoroethylene, and 11 parts of modified graphene oxide were added to 42 parts of ethanol in sequence, homogenized for 30 minutes, and passed through a 300-mesh sieve to obtain a coating;

[0063] Step 5: uniformly apply the coating on the surface of the nickel-saving and high-heat-resistant cast steel; keep it warm at 275°C for 0.5 hours; keep it warm at 375°C for 0.8 hours to obtain a polytetrafluoroethylene / graphene oxide coating; obtain the nickel-saving and high-heat-resistant cast steel, referred to as ZG40Cr25Ni12Si2V(B).

[0064] Comparative Example 3: A polytetrafluoroethylene / graphene oxide coating was prepared by modifying polytetrafluoroethylene with a single silane coupling agent, and the rest of the process remained unchanged. Specifically:

[0065] Step 1: Material smelting: (1) During the material smelting process, the temperature is set to 1705°C, 304 scrap steel is melted, and then iron-chromium alloy, nickel, iron-molybdenum alloy, and iron-cobalt alloy are added in sequence for smelting for 2.5 hours; iron-niobium alloy and iron-vanadium alloy are added within 17 minutes before the steel is discharged from the furnace and the steel is smelted for 1.5 hours; molten steel A is obtained; (2) SiCaBa and silicon-manganese alloy deoxidizers with a mass ratio of 2.2:1 are added to the molten steel A in the furnace 5.5 minutes before the steel is discharged; the steel is deoxidized in the furnace for 4 hours; the slag is removed 5 times; molten steel B is obtained; (3) iron-tellurium alloy, iron-cerium alloy, and 0.15wt% ReSiCaMn deoxidizer are added to the molten steel B in the ladle before the steel is discharged; the steel is deoxidized in the ladle for 3.5 hours; the steel is discharged from the furnace when the temperature reaches 1690°C to obtain molten steel;

[0066] Step 2: Make the shell from the coated sand: solidify at 250°C for 200S, make the shell under 0.5MPa pressure, dip-coat the shell surface with a coating concentration of 60°Bé, and bake at 220°C for 90min; when the temperature reaches 1550°C, pour molten steel inside for 45min to form the shell, and obtain nickel-saving high heat-resistant cast steel;

[0067] Step 3: (1) adding 25 parts of polytetrafluoroethylene to 2.5 parts of tert-butyl lithium / ethylenediamine solution, stirring at 75°C for 9 hours; washing and drying to obtain polytetrafluoroethylene A; (2) adding 18 parts of polytetrafluoroethylene A to 35 parts of deionized water, adding 5 parts of epoxy silane coupling agent, stirring at 65°C for 45 minutes; filtering, and drying at 105°C to obtain modified PTFE; (3) adding 11 parts of graphene oxide to 25 parts of anhydrous ethanol for dispersion, then adding 11 parts of modified PTFE, 28 parts of deionized water and 1.5 parts of hydrochloric acid, ultrasonically dispersing for 1.5 hours, stirring at 55°C for 4 hours; washing, drying, and grinding to obtain modified graphene oxide;

[0068] Step 4: 32 parts of ceramic sol, 5.5 parts of polytetrafluoroethylene, and 11 parts of modified graphene oxide were added to 42 parts of ethanol in sequence, homogenized for 30 minutes, and passed through a 300-mesh sieve to obtain a coating;

[0069] Step 5: uniformly apply the coating on the surface of the nickel-saving and high-heat-resistant cast steel; keep it warm at 275°C for 0.5 hours; keep it warm at 375°C for 0.8 hours to obtain a polytetrafluoroethylene / graphene oxide coating; and obtain the nickel-saving and high-heat-resistant cast steel.

[0070] Test experiment 1: The nickel-saving high heat-resistant cast steel and its preparation method prepared in Example 1, Comparative Example 1 and Comparative Example 2 were subjected to mechanical property tests: (1) High-temperature tensile property test was performed at 24°C using a high and low temperature material testing machine in accordance with GB / T 228.2-2015; (2) Room-temperature tensile property test was performed at 24°C using a high and low temperature material testing machine.

[0071] Table 1

[0072]

[0073] Table 2

[0074]

[0075]

[0076] Conclusion: The above disclosure shows that the present invention realizes intergranular strengthening, high temperature oxidation resistance, high temperature corrosion resistance and creep resistance through microalloying method, and achieves room temperature and high temperature mechanical properties, and service life completely surpasses the performance indicators of high Ni ductile iron and 1.4848, and meets the mechanical performance requirements of the maximum working temperature of 1100℃, and can completely replace QTANi35Si5Cr2 high nickel cast iron (maximum use temperature 950℃) and 1.4848 heat-resistant cast steel material (maximum use temperature 1100℃), and the welding type of cast steel material is completely superior to cast iron material. Therefore, it becomes a new material for manufacturing high temperature exhaust manifolds;

[0077] In addition, the Ni% content of the new heat-resistant cast steel material ZG40Cr25NiSi2V(A) is more than 20% lower than that of QTANi35Si5Cr2 high-Ni ductile iron, and more than 8% lower than that of 1.4848 heat-resistant cast steel material. The Ni% content is greatly reduced, and the amount of newly added alloy is thousand-level. The cost of saved Ni is negligible. This makes the new heat-resistant cast steel material ZG40Cr25NiSi2V(A) completely surpass all other performances while significantly reducing the material cost.

[0078] Test experiment 2: The corrosion resistance of a nickel-saving high-heat-resistant cast steel and its preparation method prepared in Example 1, Example 2, Example 3, and Comparative Example 3 was tested: The corrosion resistance of the samples was tested in a salt spray test box with reference to GB / T 10125-2021.

[0079] Table 3

[0080] name Time to rust (h) Example 1 448 Example 2 478 Example 3 >500 Comparative Example 3 452

[0081] Analysis of results: According to the data analysis in Table 1 above, it can be seen that the present invention uses a method for preparing nickel-saving high heat-resistant cast steel, and at a specific temperature, the nickel-saving high heat-resistant cast steel can still maintain stable high temperature resistance, strong oxidation resistance, and high-temperature mechanical properties; According to the data analysis in Table 2 above, it can be seen that the present invention uses a method for preparing nickel-saving high heat-resistant cast steel, and effectively improves the mechanical properties and hardness of the nickel-saving high heat-resistant cast steel at room temperature; According to the data analysis in Table 3 above, it can be seen that through a method for preparing polytetrafluoroethylene / graphene oxide coating on nickel-saving high heat-resistant cast steel, the corrosion resistance and oxidation resistance of nickel-saving high heat-resistant cast steel are greatly improved, that is, the present invention prepares a nickel-saving high heat-resistant cast steel.

[0082] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing nickel-saving high heat-resistant cast steel, characterized in that: The following steps are involved: S1: Material smelting: (1) Melting 304 scrap steel, adding iron-chromium alloy, nickel, iron-molybdenum alloy, and iron-cobalt alloy in sequence for smelting; adding iron-niobium alloy and iron-vanadium alloy into the furnace 15 to 20 minutes before being taken out of the furnace and continuing smelting; obtaining molten steel A; (2) adding deoxidizer A into the furnace 5 to 6 minutes before steel tapping; performing deoxidation treatment in the furnace, and performing slag removal for ≥ 3 times; and obtaining molten steel B; (3) adding iron-tellurium alloy, iron-cerium alloy and deoxidizer B into the ladle before tapping the molten steel B; performing deoxidation treatment in the ladle; Take out of the furnace and get molten steel; S2: Forming a shell with coated sand; coating the surface of the shell with paint and baking it; pouring molten steel inside the shell to form it, thereby obtaining nickel-saving and high-heat-resistant cast steel.

2. The method for preparing a nickel-saving high heat-resistant cast steel according to claim 1, characterized in that: The nickel-saving high heat-resistant cast steel includes the following elements, calculated by mass percentage: 0.3% to 0.5% carbon, 1.0% to 2.5% silicon, manganese ≤2%, phosphorus ≤0.04%, sulfur ≤0.03%, 24.0% to 28.0% chromium, 0.15% to 0.2% molybdenum, 11.0% to 14.0% nickel, 0.14% to 0.20% cobalt, 0.15% to 0.20% vanadium, 0.35% to 0.45% niobium, tellurium ≤0.005%, cerium ≤0.05%, and the rest is iron.

3. The method for preparing a nickel-saving high heat-resistant cast steel according to claim 1, characterized in that: During the material smelting process, the smelting temperature is 1700-1710°C and the furnace outlet temperature is 1680-1700°C.

4. The method for preparing a nickel-saving high heat-resistant cast steel according to claim 1, characterized in that: The process parameters of the coated sand shell making are set as follows: heating temperature is 200-300°C, curing time is 100-300S, and sand shooting pressure is 0.4-0.6MPa; During the dipping process: the concentration of the coating is 60°Bé; The baking process parameters are set as follows: baking temperature is 210-230° C., and baking time is 60-120 min; The process parameters for pouring the molten steel are set as follows: the pouring temperature is 1580-1520°C.

5. The method for preparing a nickel-saving high heat-resistant cast steel according to claim 1, characterized in that: The deoxidizer A includes SiCaBa; the added amount of the deoxidizer A accounts for 0.2-0.3wt% of the molten steel A.

6. The method for preparing nickel-saving high heat-resistant cast steel according to claim 1, characterized in that: The deoxidizer B includes ReSiCaMn; the added amount of the deoxidizer B accounts for 0.1-0.2wt% of the molten steel B.

7. The method for preparing nickel-saving high heat-resistant cast steel according to claim 5, characterized in that: The deoxidizer A also includes silicon-manganese alloy; the mass ratio of SiCaBa to silicon-manganese alloy is (2-2.5):

1.

8. The method for preparing nickel-saving high heat-resistant cast steel according to claim 1, characterized in that: The surface of the nickel-saving high-heat-resistant cast steel is uniformly coated with a polytetrafluoroethylene / graphene oxide coating to obtain a nickel-saving high-heat-resistant cast steel B; comprising the following steps: S1: (1) adding polytetrafluoroethylene to a tert-butyl lithium / ethylenediamine solution, adding 4-vinylaniline, stirring at 70-80°C for 8-10 hours; washing and drying to obtain polytetrafluoroethylene A; (2) adding polytetrafluoroethylene A to deionized water, adding an epoxy silane coupling agent, stirring at 60-70°C for 30-60 minutes; filtering, and drying at 100-110°C to obtain modified PTFE; (3) adding graphene oxide to anhydrous ethanol for dispersion, then adding modified PTFE, deionized water and hydrochloric acid, ultrasonically dispersing for 1-2 hours, stirring at 50-60°C for 2-5 hours; washing, drying and grinding to obtain modified graphene oxide; S2: adding ceramic sol, polytetrafluoroethylene and modified graphene oxide into ethanol in sequence, homogenizing and sieving to obtain a coating; S3: uniformly coating the surface of the shell mold cavity of the nickel-saving and high-heat-resistant cast steel part; keeping warm at 250-300°C for 0.3-0.7 hours; keeping warm at 350-400°C for 0.5-1 hour to obtain a polytetrafluoroethylene / graphene oxide coating; thereby, obtaining a nickel-saving and high-heat-resistant cast steel B.

9. The method for preparing nickel-saving high heat-resistant cast steel according to claim 8, characterized in that: The raw materials of the tert-butyl lithium / ethylenediamine solution include the following components: 2.5 to 3 parts of tert-butyl lithium, 1 to 1.3 parts of ethylenediamine, and 15 to 20 parts of diethyl ether, by mass. The raw materials of the polytetrafluoroethylene A include the following components: 2 to 3 parts by mass of tert-butyl lithium / ethylenediamine solution, 20 to 30 parts of polytetrafluoroethylene, and 15 to 20 parts of 4-ethyleneaniline; The raw materials of the modified PTFE include the following components: 15 to 20 parts of polytetrafluoroethylene A, 4 to 6 parts of epoxy silane coupling agent, and 30 to 40 parts of deionized water, calculated by mass. The raw materials of the modified graphene oxide include the following components: by mass, 10 to 12 parts of graphene oxide, 20 to 30 parts of anhydrous ethanol, 10 to 12 parts of modified PTFE, 25 to 30 parts of deionized water, and 1.5 to 2 parts of hydrochloric acid; The raw materials of the coating include the following components: by weight, 30 to 35 parts of ceramic sol, 5 to 6 parts of polytetrafluoroethylene, 10 to 12 parts of modified graphite oxide, and 40 to 45 parts of ethanol.