Double-liquid metal composite molding lining plate under high negative pressure condition and production method

Through the dual-liquid metal composite molding technology of high-carbon high-chromium cast iron and low-carbon steel, the serious wear problem of mine ball mill lining board is solved, and a composite lining board with wear resistance and toughness is prepared, which improves service life and grinding efficiency , reduces production costs.

CN119020676APending Publication Date: 2024-11-26JIAYUGUAN LIANZHONG MACHINERY EQUIP CO LTD

Patent Information

Application Number
CN202411123178.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The mine ball mill lining plate has severe wear and short life under high negative pressure conditions, making it difficult to meet the needs of long-term operation.

Method used

Using the dual-liquid metal composite molding technology of high carbon and high chromium cast iron and low carbon steel, high-liquid metal composite molding technology is used to extract high negative pressure, deoxidation, casting and heat treatment processes through induction smelting and vacuum pumping to prepare composite lining plates with high wear resistance and toughness. The design Wavy and non-working faces are slotted to reduce costs.

Benefits of technology

It significantly improves the service life of the lining plate, enhances the crushing effect of the abrasive body on the material, reduces production costs, and achieves a good metallurgical combination of the two metals by regulating the casting temperature and speed, improving the surface quality and dimensional accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020676A_ABST
    Figure CN119020676A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wear-resistant lining plates, in particular to a double-liquid metal composite molding lining plate under a high negative pressure condition and a production method. A double-liquid metal composite forming lining plate under the high negative pressure condition comprises high-carbon and high-chromium cast iron, and the high-carbon and high-chromium cast iron comprises, by mass, 2.6%-3.0% of C, 14%-16% of Cr, 0.6%-1.0% of Mn, 3% of Mo, 0.5%-0.8% of Cu, 0.1%-0.2% of La, 0.2%-0.6% of Ce and the balance Fe. The invention discloses a manufacturing method of a double-liquid metal composite molding lining plate under a high negative pressure condition. The technological process comprises the steps of smelting, densification treatment of a composite layer, deoxidation, casting and heat treatment of a casting, and finally the composite lining plate with excellent mechanical properties is obtained. The service life of the double-liquid metal composite forming lining plate under the high negative pressure condition is prolonged by 100%-150% compared with that of an existing manganese steel and chromium molybdenum steel lining plate in similar grinding media.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wear-resistant lining plates, and in particular to a double-liquid metal composite formed lining plate under high negative pressure conditions and a production method thereof. Background Art

[0002] Mining ball mill is a kind of ball mill, which is one of the supporting equipment for ore dressing such as quarrying in mines. It is widely used in the fields of building materials industry, ore dressing industry, electric power industry, chemical industry and metallurgical industry. Large-sized mining wear-resistant parts such as mining ball mill lining, large flat flow plate and large crusher back plate are important parts of heavy crushing equipment in my country. Ball mill lining is used to protect the cylinder from direct impact and friction of grinding body and materials. The working environment of the lining is poor. While bearing high stress impact, it is subjected to continuous friction of materials, grinding balls and some parts. Therefore, the wear of the lining is more serious, and the short life of the lining is a problem that needs to be solved urgently. Summary of the invention

[0003] In view of the existing problems, the present invention provides a double-liquid metal composite formed liner and a production method under high negative pressure conditions to solve the problems of severe wear and short life of the liner mentioned in the background technology.

[0004] In order to solve the existing problems, the present invention provides a double-liquid metal composite formed lining under high negative pressure conditions, including high-carbon high-chromium cast iron, the high-carbon high-chromium cast iron composition and mass percentage are: 2.6-3.0% C, 14-16% Cr, 0.6-1.0% Mn, 3% Mo, 0.5-0.8% Cu, 0.1-0.2% La, 0.2-0.6% Ce, and the balance Fe.

[0005] Furthermore, a method for manufacturing a double-liquid metal composite formed liner under high negative pressure conditions, the process flow includes the following steps:

[0006] S1. Melting: Induction melting furnace melts high chromium cast iron at a melting temperature of 1480-1520°C, and the mass percentages of the components of high chromium cast iron are: 2.6-3.0% C, 14-16% Cr, 0.6-1.0% Mn, 3% Mo, 0.5-0.8% Cu, 0.1-0.2% La, 0.2-0.6% Ce, and the balance Fe; at the same time, induction melting melts carbon steel at a melting temperature of 1600-1620°C, and the mass percentages of the components of carbon steel are: 0.26% C, 0.5% Mn, 0.3% Si, P≤0.10%, S≤0.03%;

[0007] S2. Densification treatment of the composite layer: Before casting, use a vacuum pump to extract high negative pressure in the mold, and the internal pressure P≤0.04MPa;

[0008] S3, deoxidation: 0.15% pure aluminum is added to the high chromium cast iron melt for deoxidation before it is taken out of the furnace. The aluminum powder is taken out of the furnace immediately after deoxidation, and then transferred to the ladle. Rare earth ferrosilicon is placed at the bottom of the ladle, and the flushing method is used for further deoxidation and impurity removal. After the reaction is complete, the slag in the ladle is removed;

[0009] S4, casting: When the temperature of the solution in the ladle in S3 reaches the casting requirement, the two molten metals are poured into the cavity at the same time. During the casting process, pay attention to the casting speed and keep the two molten metals at the same level at all times;

[0010] S5. Heat treatment of castings: the castings are cooled and boxed, the risers are cut off and the surface is polished and trimmed, the castings are heated to 930-980℃, kept warm for 4-5h, oil quenched for 5min and air cooled, put into the furnace again for tempering, heated to 450℃, kept warm for 3h, and air cooled to room temperature to obtain a composite lining with excellent comprehensive mechanical properties.

[0011] Compared with the prior art, the present invention has the following beneficial effects:

[0012] 1. The present invention increases the toughness while ensuring the high wear resistance of the composite lining plate, thereby avoiding fracture when subjected to high impact loads and greatly improving the service life of the lining plate.

[0013] 2. The present invention designs the appearance structure of the liner. The wavy working surface can enhance the grinding effect of the grinding body on the material, improve the grinding efficiency of the ball mill, and increase the output. Without affecting the overall strength of the liner, the amount of metal used is reduced by grooving the non-working surface, thereby reducing the production cost.

[0014] 3. The bimetal forming process under high negative pressure conditions developed by the present invention controls the casting temperature field and the heat transfer conditions of the mold by adjusting the negative pressure conditions, and avoids a large amount of mixing of the two metals by controlling the casting speed and casting temperature, and finally achieves a good metallurgical bond. The problems of shrinkage and shrinkage holes in the castings are effectively reduced by designing reasonable shrinkage feed risers, improving the shrinkage feed capacity of the casting system, and maintaining pressure after casting. The casting process of the present invention not only solves the problems of poor metallurgy such as pores and slag inclusions at the composite interface of the two metals, but also greatly improves the surface quality and dimensional accuracy of the castings by maintaining pressure and regulating the negative pressure inside the mold, and controls the casting speed and casting temperature of the two molten metals to achieve a firm metallurgical bond at the composite interface. The service life of the dual-liquid metal composite liner prepared by the present invention is 100% to 150% higher than that of the existing manganese steel and chrome-molybdenum steel liners in the same grinding media.

[0015] 4. The wear-resistant layer of the bimetallic liner designed and prepared by the present invention is mainly composed of high-chromium cast iron. In order to further improve the service life, rare earth elements are used to micro-alloy the high-chromium cast iron, which successfully refines the matrix structure and improves the morphology and distribution of carbides. A large number of evenly distributed ellipsoidal and blocky primary M7C3 carbides can be regarded as ideal reinforcements, and the wear resistance and toughness of the high-chromium cast iron are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram of the overall structure of the composite molded liner of the present invention; DETAILED DESCRIPTION

[0017] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] A double-liquid metal composite forming lining plate under high negative pressure conditions comprises high-carbon high-chromium cast iron, wherein the high-carbon high-chromium cast iron has the following components and mass percentages: 2.6-3.0% C, 14-16% Cr, 0.6-1.0% Mn, 3% Mo, 0.5-0.8% Cu, 0.1-0.2% La, 0.2-0.6% Ce, and the balance Fe.

[0019] A method for manufacturing a double-liquid metal composite forming liner under high negative pressure conditions, characterized in that the process comprises the following steps:

[0020] S1. Melting: Induction melting furnace melts high chromium cast iron at a melting temperature of 1480-1520°C, and the mass percentages of the components of high chromium cast iron are: 2.6-3.0% C, 14-16% Cr, 0.6-1.0% Mn, 3% Mo, 0.5-0.8% Cu, 0.1-0.2% La, 0.2-0.6% Ce, and the balance Fe; at the same time, induction melting melts carbon steel at a melting temperature of 1600-1620°C, and the mass percentages of the components of carbon steel are: 0.26% C, 0.5% Mn, 0.3% Si, P≤0.10%, S≤0.03%;

[0021] S2. Densification treatment of the composite layer: Before casting, use a vacuum pump to extract high negative pressure in the mold, and the internal pressure P≤0.04MPa;

[0022] S3, deoxidation: 0.15% pure aluminum is added to the high chromium cast iron melt for deoxidation before it is taken out of the furnace. The aluminum powder is taken out of the furnace immediately after deoxidation, and then transferred to the ladle. Rare earth ferrosilicon is placed at the bottom of the ladle, and the flushing method is used for further deoxidation and impurity removal. After the reaction is complete, the slag in the ladle is removed;

[0023] S4, casting: When the temperature of the solution in the ladle in S3 reaches the casting requirement, the two molten metals are poured into the cavity at the same time. During the casting process, pay attention to the casting speed and keep the two molten metals at the same level at all times;

[0024] S5. Heat treatment of castings: the castings are cooled and boxed, the risers are cut off and the surface is polished and trimmed, the castings are heated to 930-980℃, kept warm for 4-5h, oil quenched for 5min and air cooled, put into the furnace again for tempering, heated to 450℃, kept warm for 3h, and air cooled to room temperature to obtain a composite lining with excellent comprehensive mechanical properties.

[0025] It should be noted that: (1) the mold is kept under high negative pressure. A vacuum pump is used to draw high negative pressure from the mold before casting. The heat transfer capacity of the mold is enhanced under the action of negative pressure. The temperature field of the mold is controlled by adjusting the negative pressure. As the negative pressure is continuously drawn from the mold, the molten iron is subjected to strong quenching to produce a large cooling rate. The white cast structure formed after cooling is more compact and the hardness is further improved. Since the vacuum pump is located on the side of the high-chromium cast iron, the temperature of the molten iron decreases when it reaches the interface under the action of strong quenching, and the fluidity becomes worse. The high-temperature molten steel vaporizes the carbon steel layer and contacts the molten iron. The high-chromium cast iron at the front of the interface is reheated by the high-temperature molten steel, and the two metal liquids are mixed in a small range. Since the casting temperature of carbon steel is higher than that of cast iron, the heat flow tempers the composite interface under the action of negative pressure, and the sharp carbides around the interface are dissolved. The hardness of the composite layer decreases, but the toughness increases, avoiding the generation of crack sources due to stress concentration.

[0026] (2) The molten iron and molten steel are cast simultaneously. Compared with the solid-liquid combination method, the present invention simultaneously casts two molten metals and uses two different runners to cast two liquid metals at the same time. During the casting process, the two metal liquid levels are always kept at the same level to prevent the liquid metals from mixing due to pressure imbalance. In addition, since the two metals are both in a liquid state with good fluidity when they meet, this creates favorable conditions for the diffusion of atoms on both sides of the interface. The atoms on both sides of the interface are more likely to diffuse and undergo physical and chemical reactions. The composite layer obtained after solidification has uniform thickness and regular shape, and the metallurgical bonding of the bimetallic liner is more solid.

[0027] (3) In order to further improve the impact toughness of the wear-resistant layer of the lining plate, a small amount of rare earth elements was used to micro-alloy the high chromium cast iron layer. During the smelting process of high chromium cast iron, an appropriate amount of rare earth lanthanum-cerium alloy (wt%) was added: La: 10%, Ce: 35%, and the balance Fe. Rare earth elements are good surfactants and can easily form compounds with impurities such as sulfur and oxygen in molten iron. This not only provides a substrate for primary M7C3 carbides, but also aggregates on the surface of carbides or in the front liquid phase to cause component supercooling, ultimately causing the primary carbides to be refined from coarse strips or hexagons to ellipsoids. Since the radii of carbon atoms and chromium atoms are smaller than those of lanthanum atoms, diffusion is hindered, allowing austenite to nucleate and grow in a small range. All alloying elements are consumed before phase change occurs, ensuring that austenite is completely transformed into martensite. Rare earth cerium easily forms compounds with oxygen and sulfur in molten iron, inducing heterogeneous nucleation of carbides, which not only improves the morphology and distribution of carbides, but also effectively increases the volume fraction, greatly improving the wear resistance and toughness of high chromium cast iron.

[0028] (4) The composite lining plate involved in the present invention uses two kinds of metals, and the interface bonding quality has a great influence on the service life of the lining plate. In order to strengthen the metallurgical bonding strength of the interface and control the organizational morphology, the present invention designs a corresponding heat treatment process: heat the casting to 930-980°C, keep it warm for 4-5 hours, oil quench for 5 minutes and then air cool it. After cooling to room temperature, put it into the furnace again for tempering treatment, keep it warm at 450°C for 3 hours and air cool it. In order to prevent quenching cracks from occurring in the casting, take it out of the quenching medium before the quenching stress reaches the maximum, and perform air cooling treatment. During the air cooling process, the heat from the thick part of the lining plate is transferred to the surface, which relieves the quenching cracks caused by uneven stress. After heat treatment, the high chromium cast iron structure is based on martensite, and the primary M7C3 type carbides are dispersed as reinforcing phases in the shape of ellipsoids or blocks, and are dispersed, and the eutectic carbides are wrapped by the primary carbides. Post-casting heat treatment also promotes the diffusion of chromium elements. The chromium atoms diffused to the low-carbon steel side will cause solid solution strengthening, and the strength of the low-carbon steel will increase. The microstructures from high-chromium cast iron to the carbon steel side are cast iron, hypereutectoid steel, eutectoid steel, and hypoeutectoid steel.

[0029] (5) The working surface of the new composite liner designed in the present invention is wavy, which increases the contact area between the liner and the abrasive, enhances the grinding effect of the grinding body on the material, helps to improve the grinding efficiency and increase the output. Square grooves are opened on the non-working surface. On the one hand, it can save metal consumption and reduce costs; on the other hand, the positions of the square grooves are all at the troughs of the corresponding wavy working surface, so that the thickness of the liner tends to be consistent without affecting the strength. Since the thickness uniformity of the casting will vary, the thicker area is prone to heat concentration and the cooling rate is slow. In order to reduce the adverse effects of uneven thickness, on the one hand, the thicker part can be thinned, so grooves are opened where the liner thickness is larger; on the other hand, in order to further reduce casting defects, cold iron is placed in the thicker part of the casting, and risers are added to solve the shrinkage problem.

[0030] Embodiment 1:

[0031] S1. Melting: The induction melting furnace melts high chromium cast iron at a melting temperature of 1482°C, and the mass percentages of the components of the high chromium cast iron are: 2.6% C, 14% Cr, 0.6% Mn, 3% Mo, 0.5% Cu, 0.1% La, 0.2% Ce, and the balance Fe; at the same time, the induction melting furnace melts carbon steel at a melting temperature of 1600°C, and the mass percentages of the components of the carbon steel are: 0.26% C, 0.5% Mn, 0.3% Si, 0.08% P, and 0.02% S;

[0032] S2. Densification treatment of the composite layer: Before casting, a vacuum pump is used to extract high negative pressure from the mold, and the internal pressure P is 0.03MPa;

[0033] S3, deoxidation: 0.15% pure aluminum is added to the high chromium cast iron melt for deoxidation before it is taken out of the furnace. The aluminum powder is taken out of the furnace immediately after deoxidation, and then transferred to the ladle. Rare earth ferrosilicon is placed at the bottom of the ladle, and the flushing method is used for further deoxidation and impurity removal. After the reaction is complete, the slag in the ladle is removed;

[0034] S4, casting: When the temperature of the solution in the ladle in S3 reaches the casting requirement, the two molten metals are poured into the cavity at the same time. During the casting process, pay attention to the casting speed and keep the two molten metals at the same level at all times;

[0035] S5. Heat treatment of castings: the castings are cooled and boxed, the risers are cut off and the surface is polished and trimmed, the castings are heated to 935°C, kept warm for 4 hours, oil quenched for 5 minutes and air cooled, put into the furnace again for tempering, heated to 450°C, kept warm for 3 hours, and air cooled to room temperature to obtain a composite lining with excellent comprehensive mechanical properties.

[0036] Embodiment 2:

[0037] S1. Melting: The induction melting furnace melts high chromium cast iron at a melting temperature of 1500°C, and the mass percentages of the components of the high chromium cast iron are: 2.8% C, 15% Cr, 0.8% Mn, 3% Mo, 0.65% Cu, 0.15% La, 0.4% Ce, and the balance Fe; at the same time, the induction melting furnace melts carbon steel at a melting temperature of 1610°C, and the mass percentages of the components of the carbon steel are: 0.26% C, 0.5% Mn, 0.3% Si, 0.08% P, and 0.02% S;

[0038] S2. Densification treatment of the composite layer: Before casting, a vacuum pump is used to extract high negative pressure from the mold, and the internal pressure P is 0.03MPa;

[0039] S3, deoxidation: 0.15% pure aluminum is added to the high chromium cast iron melt for deoxidation before it is taken out of the furnace. The aluminum powder is taken out of the furnace immediately after deoxidation, and then transferred to the ladle. Rare earth ferrosilicon is placed at the bottom of the ladle, and the flushing method is used for further deoxidation and impurity removal. After the reaction is complete, the slag in the ladle is removed;

[0040] S4, casting: When the temperature of the solution in the ladle in S3 reaches the casting requirement, the two molten metals are poured into the cavity at the same time. During the casting process, pay attention to the casting speed and keep the two molten metals at the same level at all times;

[0041] S5. Heat treatment of castings: the castings are cooled and boxed, the risers are cut off and the surface is polished and trimmed, the castings are heated to 955°C, kept warm for 4.5 hours, oil quenched for 5 minutes and air cooled, put into the furnace again for tempering, heated to 450°C, kept warm for 3 hours, and air cooled to room temperature to obtain a composite lining with excellent comprehensive mechanical properties.

[0042] Embodiment 3:

[0043] S1. Melting: The induction melting furnace melts high chromium cast iron at a melting temperature of 1520°C, and the mass percentages of the components of the high chromium cast iron are: 3.0% C, 16% Cr, 1.0% Mn, 3% Mo, 0.8% Cu, 0.2% La, 0.6% Ce, and the balance Fe; at the same time, the induction melting furnace melts carbon steel at a melting temperature of 1620°C, and the mass percentages of the components of the carbon steel are: 0.26% C, 0.5% Mn, 0.3% Si, 0.08% P, and 0.02% S;

[0044] S2. Densification treatment of the composite layer: Before casting, a vacuum pump is used to extract high negative pressure from the mold, and the internal pressure P is 0.03MPa;

[0045] S3, deoxidation: 0.15% pure aluminum is added to the high chromium cast iron melt for deoxidation before it is taken out of the furnace. The aluminum powder is taken out of the furnace immediately after deoxidation, and then transferred to the ladle. Rare earth ferrosilicon is placed at the bottom of the ladle, and the flushing method is used for further deoxidation and impurity removal. After the reaction is complete, the slag in the ladle is removed;

[0046] S4, casting: When the temperature of the solution in the ladle in S3 reaches the casting requirement, the two molten metals are poured into the cavity at the same time. During the casting process, pay attention to the casting speed and keep the two molten metals at the same level at all times;

[0047] S5. Heat treatment of castings: the castings are cooled and boxed, the risers are cut off and the surface is polished and trimmed, the castings are heated to 980°C, kept warm for 5 hours, oil quenched for 5 minutes and air cooled, put into the furnace again for tempering, heated to 450°C, kept warm for 3 hours, and air cooled to room temperature to obtain a composite lining with excellent comprehensive mechanical properties.

[0048] The present invention uses large-plane double-liquid metal composite forming technology under negative pressure to successfully prepare the mine ball mill liner. After testing, the basic performance of the high-chromium cast iron / low-carbon steel double-liquid metal composite liner is as follows: high-chromium cast iron layer: HRC>55, impact toughness ak>20J / cm2; low-carbon steel layer: impact toughness ak>120J / cm2; interface impact test breaks on the high-chromium cast iron side. The service life of the high-chromium cast iron / low-carbon steel double-liquid metal composite liner is 100% to 150% higher than that of the existing manganese steel and chrome-molybdenum steel liners in the same grinding medium.

[0049] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any ordinary technician in the industry can smoothly implement the present invention as shown in the drawings and described above. However, any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A double liquid metal composite forming liner under high negative pressure conditions, comprising high carbon high chromium cast iron, characterized in that: The composition and mass percentage of high carbon high chromium cast iron are: 2.6-3.0% C, 14-16% Cr, 0.6-1.0% Mn, 3% Mo, 0.5-0.8% Cu, 0.1-0.2% La, 0.2-0.6% Ce, and the balance Fe.

2. A method for manufacturing a double-liquid metal composite forming liner under high negative pressure conditions, characterized in that: The process includes the following steps: S1. Melting: Induction melting furnace melts high chromium cast iron at a melting temperature of 1480-1520°C, and the mass percentages of the components of high chromium cast iron are: 2.6-3.0% C, 14-16% Cr, 0.6-1.0% Mn, 3% Mo, 0.5-0.8% Cu, 0.1-0.2% La, 0.2-0.6% Ce, and the balance Fe; at the same time, induction melting melts carbon steel at a melting temperature of 1600-1620°C, and the mass percentages of the components of carbon steel are: 0.26% C, 0.5% Mn, 0.3% Si, P≤0.10%, S≤0.03%; S2. Densification treatment of the composite layer: Before casting, use a vacuum pump to extract high negative pressure in the mold, and the internal pressure P≤0.04MPa; S3, deoxidation: 0.15% pure aluminum is added to the high chromium cast iron melt for deoxidation before it is taken out of the furnace. The aluminum powder is taken out of the furnace immediately after deoxidation, and then transferred to the ladle. Rare earth ferrosilicon is placed at the bottom of the ladle, and the flushing method is used for further deoxidation and impurity removal. After the reaction is complete, the slag in the ladle is removed; S4, casting: When the temperature of the solution in the ladle in S3 reaches the casting requirement, the two molten metals are poured into the cavity at the same time. During the casting process, pay attention to the casting speed and keep the two molten metals at the same level at all times; S5. Heat treatment of castings: the castings are cooled and boxed, the risers are cut off and the surface is polished and trimmed, the castings are heated to 930-980℃, kept warm for 4-5h, oil quenched for 5min and air cooled, put into the furnace again for tempering, heated to 450℃, kept warm for 3h, and air cooled to room temperature to obtain a composite lining with excellent comprehensive mechanical properties.

Citation Information

Patent Citations

  • Crust-hitting hammer head for aluminum reduction cell and casting technique thereof

    CN101619469A

  • Production method of composite funnel impact guard plate

    CN102242305A

  • Bimetal composite type abrasion-resistant liner plate and manufacturing method

    CN105457722A

  • Double-liquid compound casting method for automobile mold casting

    CN107790678A

  • Centrifugal casting process of producing antiwear composite multicomponent alloy-cast iron roller ring

    CN1241644A

Cited By

  • High negative pressure vacuum precision control double-liquid composite wear-resistant lining plate gradient casting process